Nitriding treatment method and tungsten carbide superhard alloy

The domain where tungsten carbide and nitrogen atoms coexist is formed through atomic nitriding treatment, which solves the problem of increasing the hardness of cemented carbide in the existing technology and achieves a significant increase in hardness, especially in the wear resistance within a few μm depth area on the surface.

CN115298348BActive Publication Date: 2024-10-29PLASMA RES & DEV LAB
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202180019393.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-03-17
Publication Date
2024-10-29
Estimated Expiration
2041-03-17

Smart Images

  • Figure CN115298348B_ABST
    Figure CN115298348B_ABST
Patent Text Reader

Abstract

The tungsten carbide-based superhard alloy of the present invention is composed of tungsten carbide and additives, and has a nitrided surface and a domain where nitrogen and tungsten carbide coexist. According to the present invention, the hardness of the superhard alloy subjected to nitriding treatment is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to nitriding treatment. Background Art

[0002] There are materials called superhard alloys. A typical material is a WC-Co superhard alloy in which cobalt is added to tungsten carbide (WC). In order to improve the wear resistance of the superhard alloy, it is considered to perform nitriding treatment on the superhard alloy to increase the hardness (Patent Document 1, etc.).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2002-210525 Summary of the invention

[0006] Problems to be solved by the invention

[0007] In conventional gas nitriding, the required hardness may not be achieved. The present invention aims to improve the hardness of a cemented carbide by atomic nitriding.

[0008] Means for solving problems

[0009] One embodiment of the present invention provides a tungsten carbide-based superhard alloy, which is composed of tungsten carbide and an additive, has a nitrided surface, and has a domain where nitrogen and tungsten carbide coexist.

[0010] In the above-mentioned tungsten carbide superhard alloy, the first layer exists in a domain from the surface to a specified depth, and has a domain where nitrogen and tungsten carbide coexist, and the second layer exists in a region deeper than the above-mentioned first layer, and the number of nitrogen atoms per unit volume existing in the above-mentioned first layer is 3 to 5 times the number of nitrogen atoms per unit volume existing in the above-mentioned second layer in the domain where nitrogen and the above-mentioned additive coexist.

[0011] In another aspect of the present invention, the material is composed of tungsten carbide and an additive, has a nitrided surface, has a domain where nitrogen and tungsten carbide coexist, and has a Vickers hardness of 2000 HV to 3000 HV when measured with a measurement load of 10 g.

[0012] In a preferred embodiment, the Vickers hardness of the tungsten carbide-based superhard alloy measured at a measurement load of 25 g is 1700 HV to 2500 HV.

[0013] Another aspect of the present invention provides a tungsten carbide superhard alloy, characterized in that it is composed of tungsten carbide and additives, has a nitrided surface, has a domain where nitrogen and tungsten carbide coexist, and has a Vickers hardness measured at a measurement load of 10g increased by at least 30% compared to a case where the above-mentioned nitriding is not performed.

[0014] In a preferred embodiment, the tungsten carbide-based superhard alloy is characterized in that the Vickers hardness measured at a measurement load of 25 g is increased by at least 10% compared to a case where the nitriding is not performed.

[0015] In a preferred embodiment, the Co content of the tungsten carbide-based superhard alloy is 0 to 25% by weight.

[0016] In another aspect, the present invention provides a method for producing a nitrided tungsten carbide superhard alloy by treating the tungsten carbide superhard alloy at a temperature of 550°C to 800°C for 12 hours to 120 hours using electron beam excited nitrogen plasma.

[0017] Effects of the Invention

[0018] According to the present invention, the hardness of the cemented carbide subjected to nitriding treatment is improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is a diagram showing the outline of the atomic nitriding treatment apparatus 1 .

[0020] Figure 2A This is a diagram showing the measurement results of the hardness of the sample 1 before the nitriding treatment.

[0021] Figure 2B This is a graph showing the results of measuring the hardness of Sample 1 after nitriding treatment.

[0022] Figure 3A This is a diagram showing the measurement results of the hardness of Sample 2 before nitriding treatment.

[0023] Figure 3B This is a diagram showing the measurement results of the hardness of Sample 2 after nitriding treatment.

[0024] Figure 4 It is a graph showing the measurement results of EPMA (electron probe microanalyzer).

[0025] Figure 5 It is a graph showing the measurement results of EPMA.

[0026] Figure 6 It is a graph showing the measurement results of EPMA.

[0027] Figure 7 It is a graph showing the measurement results of EPMA.

[0028] Figure 8 It is a graph showing the measurement results of EPMA. DETAILED DESCRIPTION

[0029] First, the gist of the present invention will be described.

[0030] The present invention provides a tungsten carbide-based superhard alloy, which is characterized in that it is composed of tungsten carbide and additives, has a nitrided surface, and has a domain where nitrogen and tungsten carbide coexist.

[0031] In the present invention, it is believed that a domain where nitrogen and tungsten carbide coexist, which has not been achieved in the past, can be formed, thereby improving the hardness of the superhard alloy. Specifically, the invention described in the patent document 1 introduced above states in its paragraph 0004 that "if the superhard alloy is subjected to nitriding or soft nitriding, N atoms and the like diffuse and penetrate from the surface of the alloy, and the impurity components are nitrided to show a hardening effect. As a result, it can be inferred that the bonding force between WC-Co is enhanced", and nitrogen atoms increase the hardness of the alloy by nitriding impurities (Fe, Mo, etc.) in the WC-Co alloy. The inventors believe that in this method, the hardness is not sufficient, and good hardness can be achieved by allowing nitrogen atoms to coexist with tungsten carbide itself (for example, by diffusing nitrogen atoms from the surface so that nitrogen exists in tungsten carbide particles).

[0032] The superhard alloy in the present invention broadly refers to a composite material formed by sintering the carbides of metals of Groups IVa, Va, and VIa of the periodic table with iron-based metals such as Fe, Co, and Ni. In particular, the alloy with the best mechanical properties is an alloy in which iron-based metals (additives) such as Co and Ni are sintered in tungsten carbide (WC), and more specifically, a WC-Co alloy in which Co is sintered in tungsten carbide (WC). Sometimes WC-Co alloys are also referred to as superhard alloys in a narrow sense. These alloys are characterized in that, needless to say, low-temperature hardness, high-temperature hardness, high strength, and stable physical properties are excellent. Superhard alloys are made by a method such as powder metallurgy. Regarding superhard alloys, tungsten carbide (WC), which is its main component, has a melting point of 2900°C, a high temperature, high hardness, and is difficult to smelt or cut, so it is manufactured by powder metallurgy.

[0033] The tungsten carbide (WC) superhard alloy of the present invention typically includes WC-Co alloy, WC-TiC-Co alloy, WC-TaC-Co alloy, WC-TiC-TaC-Co alloy, WC-Ni alloy, WC-Ni-Cr alloy, WC-Ni alloy, WC-Ni-Cr alloy, etc., which refers to all metals with tungsten carbide as the main body (hereinafter, tungsten carbide superhard alloy is sometimes referred to as "alloy"). For example, the content of the additive of the tungsten carbide superhard alloy is 0 to 25% by weight. In addition, in the tungsten carbide (WC) superhard alloy of the present invention, in addition to tungsten carbide and additives, substances (Fe, Mo, etc.) as impurities can also be contained.

[0034] In the present invention, tungsten carbide-based superhard alloy is composed of tungsten carbide and additives. The additive is not particularly limited, but usually functions as a bonding agent for bonding tungsten carbide. As such additives, Co, TiC, TaC, Ni, Cr, etc. can be cited, but if the practicality when used in tools, etc. is considered, Co is preferably used. The content of such additives is not particularly limited, but when the tungsten carbide superalloy is set to 100 weight %, it is usually more than 0 weight % and less than 25 weight %. The preferred content varies depending on the purpose of using the tungsten carbide superhard alloy (cutting tools, wear-resistant / impact-resistant tools, civil engineering / mining tools, geotechnical tools, non-magnetic materials). For example, in cutting tools, it is set to more than 3 weight % and less than 15 weight %, in wear-resistant / impact-resistant tools, it is set to more than 3 weight % and less than 25 weight %, in civil engineering / mining tools, it is set to more than 5 weight % and less than 20 weight %, in geotechnical tools, it is set to more than 1 weight % and less than 5 weight %, and in non-magnetic materials, it is set to more than 5 weight % and less than 20 weight %.

[0035] In addition, the surface of the tungsten carbide superhard alloy of the present invention is nitrided, and has a domain where nitrogen and tungsten carbide coexist. Here, the surface being nitrided refers to a state in which nitrogen is distributed or exists from the surface (the outermost surface) of the tungsten carbide superhard alloy to the depth of a specified area. In order to make such a distribution or existence of nitrogen, a method for diffusing nitrogen from the surface of the tungsten carbide superhard alloy to the inside by using the atomic nitriding method described later can be used.

[0036] It should be noted that the surface refers to the surface of the alloy, and when the alloy is nitrided with a substance other than the alloy (in an argon and nitrogen gas atmosphere), it is the interface separating the mixed gas phase from the alloy. If nitrogen atoms adhere to the interface at a predetermined temperature, they enter the interior of the alloy (metal crystal).

[0037] The tungsten carbide-based superhard alloy of the present invention has a domain where nitrogen and tungsten carbide coexist. The domain (phase) where nitrogen and tungsten carbide coexist means an area where nitrogen and tungsten carbide coexist. Moreover, whether it is a coexistence domain can be judged by appropriate analysis. For example, it is possible to judge whether there is an area where both tungsten and nitrogen atoms are detected by an image of EPMA (Electron Probe Micro Analyzer). More specifically, EPMA is used to perform element mapping (such as color mapping) of tungsten and nitrogen atoms on the cross section (including the cross section of the surface) of the tungsten carbide-based superhard alloy, and the two mapping images are compared. If any element is also detected in the same area, it is judged that the area is a domain where nitrogen and tungsten carbide coexist.

[0038] In the present invention, the first layer exists in a domain where nitrogen and tungsten carbide coexist from the surface to a predetermined depth, and the second layer exists in a region deeper than the first layer, and the number of nitrogen atoms per unit volume in the first layer (nitride layer) is preferably 3 to 5 times the number of nitrogen atoms per unit volume in the domain (phase) where nitrogen and the additive coexist in the second layer (diffusion layer). Here, the predetermined depth is a depth of 2 μm to 10 μm from the surface, preferably a depth of 2 μm to 4 μm from the surface.

[0039] The relationship between the distance (depth) from the surface and the distribution of each element can be evaluated using EPMA (electron probe microanalyzer) as described above. In the present invention, as analysis conditions, an electron beam diameter of 1 μm, an acceleration voltage of 10 kV to 20 kV, a current of 2×10^-7 A, a magnification of 3000 times (40 μm×30 μm), and a resolution of 256×192 pixels are used.

[0040] The detailed analysis results are described later.

[0041] As described above, in the tungsten carbide (WC) superhard alloy of the present invention, nitrogen atoms enter tungsten carbide to form a domain where nitrogen and tungsten carbide coexist, thereby improving hardness. Specifically, the Vickers hardness of the tungsten carbide (WC) superhard alloy of the present invention measured with a measurement load of 10g is 2000HV to 3000HV, and the Vickers hardness measured with a measurement load of 25g is 1700HV to 2500HV.

[0042] In addition, compared with the case of non-nitriding, the Vickers hardness of the tungsten carbide (WC) superhard alloy of the present invention measured with a measurement load of 10g is increased by at least 30%, and the Vickers hardness measured with a measurement load of 25g is increased by at least 10%. Here, the Vickers hardness in the "non-nitriding case" can be measured by measuring the Vickers hardness of the surface before the nitriding treatment is performed, or a method of using the non-nitrided surface of the tungsten carbide (WC) superhard alloy of the present invention to measure the Vickers hardness of the surface can be adopted.

[0043] In addition, the tungsten carbide (WC) superhard alloy of the present invention is manufactured by treating the tungsten carbide superhard alloy at a temperature of 550° C. to 800° C. for 12 to 120 hours using electron beam excited nitrogen plasma. By adopting this manufacturing method, it is easy to obtain a tungsten carbide (WC) superhard alloy having a domain where nitrogen and tungsten carbide coexist.

[0044] Here, it is preferred that, in the case of continuous operation, the nitriding temperature is 650°C ± 20°C, and the nitriding time is 96 hours or more, and in the case of intermittent operation, the nitriding temperature is 670°C to 730°C, and the nitriding time is 24 hours or more. It should be noted that studies have found that if the nitriding treatment is continuously operated at a treatment temperature of 670°C or above, brittle Co is easily formed on the surface of WC-Co. 3 W layer, there is a tendency for the surface roughness to increase easily. In addition, there seems to be a tendency that the surface hardness and wear resistance have increased to a certain extent, but a significant increase has not yet been confirmed. However, under this condition, it is also possible to form a domain where nitrogen and tungsten carbide coexist by optimizing the nitriding conditions. If intermittent operation is performed (i.e., temperature management with an appropriate holding time is set during the nitriding treatment), there is a tendency to suppress Co 3 The formation of the W layer tends to be less likely to cause an increase in surface roughness, and it is confirmed that it is easier to achieve an increase in surface hardness and an improvement in wear resistance. Intermittent transport can use a high nitriding treatment temperature range, so it is also preferred in that the treatment time can be shortened.

[0045] Hereinafter, the present invention will be described in detail with reference to the accompanying drawings. However, the following is only one of the preferred embodiments of the present invention, and the present invention is not limited to the following embodiments.

[0046] Figure 1 This is an outline of the atomic nitriding treatment apparatus 1 used in the present invention.

[0047] A WC-Co superhard alloy (i.e., a tungsten carbide alloy with cobalt (Co) as an additive) is set in a chamber, the chamber is vacuum-exhausted, and argon gas is introduced into the plasma source on the left side of the figure to generate argon plasma. An electron beam is drawn out from the argon plasma to excite nitrogen gas and generate a high concentration of nitrogen atoms (electron beam excited nitrogen plasma). In this way, by exposing a sample of a WC-Co superhard alloy to electron beam excited nitrogen plasma, nitrogen atoms are diffused from the surface of the sample to the inside. Here, a heater is provided in the container in which the sample is provided, and the sample is maintained at a constant temperature during the nitriding treatment. Specifically, the temperature of the sample is maintained at 550°C to 800°C, preferably at 650°C to 700°C. The processing time is 12 hours to 120 hours, preferably 96 hours.

[0048] Regarding the temperature, if it is higher than 800°C, there is a tendency to increase the damage to the sample surface. On the other hand, if it is lower than 550°C, the temperature is low and there is a tendency that diffusion is difficult to carry out. Regarding the treatment time, as described later, it is believed that if it is too short, the diffusion of nitrogen atoms is difficult to carry out. Even if the treatment time is increased, the effect of hardness improvement also tends to reach a limit. As a result, there can be multiple combinations of the preferred temperature and treatment time for obtaining the manufacturing conditions of the tungsten carbide superhard alloy of the present invention, so it is possible to optimize the above conditions and set them according to the materials of the tungsten carbide and additives used.

[0049] It should be noted that, in the material commonly referred to as WC-Co superhard alloy, there are differences in the content of cobalt, for example, it is usually 0 wt% to 25 wt%. One of the advantages of the nitriding method (manufacturing method) of the present invention is that, even when the cobalt content varies greatly from 0 wt% to 25 wt%, it is not dependent on the content, and it is easy to obtain a tungsten carbide superhard alloy with good hardness. In the following examples, as representative examples, an alloy (sample 1) in which WC is 87 wt% and cobalt is 13 wt% and an alloy (sample 2) in which WC is 92 wt% and cobalt is 8 wt%.

[0050] Using the above-mentioned apparatus, a WC-Co superhard alloy sample was subjected to nitriding treatment. Figure 2A , 2B 3A and 3B show the results of hardness measurement.

[0051] Figure 2A and Figure 2B The measurement results at five different positions in one sample (sample 1) before treatment and the results at five different positions in the sample after nitridation treatment are shown. For sample 1, the atomic nitridation treatment temperature was set to 650° C. and the nitridation treatment time was set to 96 hours.

[0052] Likewise, Figure 3A and Figure 3B The measurement results at five different positions in the sample 2 before treatment and the results at five different positions in the sample after nitridation treatment are shown. Regarding the sample 2, the atomic nitridation treatment temperature was 7000° C. and the nitridation treatment time was 30 hours.

[0053] For each sample, the Vickers hardness (unit: HV) was measured using a tester (model HM-125) manufactured by Mitutoyo Corporation.

[0054] Here, when measuring the hardness of a sample, the setting of the measuring load is important. This is because, assuming that the hardness has depth dependence, depending on the measuring load, which part of the sample in the thickness direction the hardness is measured changes. Specifically, a measuring load of 10g is equivalent to measuring the physical properties from the surface to a depth of about 5μm. A measuring load of 25g is equivalent to measuring the physical properties from the surface to a depth of 9μm. In Figure 2 (before nitriding treatment), there is no big difference between the shallow part from the surface (from the surface to a depth of about 5μm) and the deep part from the surface (from the surface to a depth of 9μm), but according to Figure 2B and Figure 3B It is found that in the sample subjected to nitriding treatment, the portion shallower than the surface becomes harder.

[0055] For sample 1, Figure 2B As shown in the figure, the Vickers hardness measured with a measurement load of 10g is 1623HV to 2500HV, and if the average of the three values ​​in the middle excluding the maximum and minimum values ​​is taken, it is 2110HV. There are also three measured values ​​exceeding 2000HV. Compared with the case where nitriding treatment is not performed, the Vickers hardness measured with a measurement load of 10g is increased by about 39% (+597HV) by taking the average of the three values ​​in the middle excluding the maximum and minimum values.

[0056] On the other hand, the Vickers hardness measured with a measurement load of 25g is 1496HV to 1781HV, and the average of the three values ​​in the middle excluding the maximum and minimum values ​​is 1694HV. There are also three measured values ​​exceeding 1700HV. Compared with the case where the above-mentioned nitriding treatment is not performed, the Vickers hardness measured with a measurement load of 25g is increased by about 15% (+219HV).

[0057] Similarly, for sample 2, Figure 3B As shown in the figure, the Vickers hardness measured with a measuring load of 10g is 2770HV to 3929HV, and if the three values ​​in the middle excluding the maximum and minimum values ​​are averaged, it is 3007HV. Compared with the case where nitriding treatment is not implemented, the Vickers hardness measured with a measuring load of 10g is increased by about 48% by the average of the three values ​​in the middle excluding the maximum and minimum values. On the other hand, the Vickers hardness measured with a measuring load of 25g is 2421HV to 2564HV, and if the three values ​​in the middle excluding the maximum and minimum values ​​are averaged, it is 2530HV. Compared with the case where nitriding treatment is not implemented, the Vickers hardness measured with a measuring load of 10g is increased by about 27% by the average of the three values ​​in the middle excluding the maximum and minimum values.

[0058] Thus, it was confirmed that the hardness was improved after nitriding treatment at any measurement load in both Samples 1 and 2. In addition, at least in the depth region of about 5 μm to 9 μm, the ratio of hardness improvement in the shallower region (closer to the surface) was greater.

[0059] The rate of improvement in hardness depends on the depth, and it is presumed that the degree of distribution of nitrogen atoms has depth dependence. Therefore, the distribution of elements in the sample was measured at each depth using an electron probe microanalyzer (EPMA) (manufactured by JEOL, model JXA8530F).

[0060] Figures 4 to 8 The measurement results are shown in FIG. 1 and FIG. 2 , which are diagrams showing the measurement results of the sample after the treatment from the cross section (thickness direction).

[0061] Figure 4 , Figure 5 , Figure 6 The distributions of tungsten atoms (tungsten atoms in tungsten carbide), cobalt atoms, and nitrogen atoms are shown respectively. Figure 8 It is shown Figures 4 to 6 A graph showing the relationship between the color of the image data and the density of atoms. Figures 4 to 6 In the figure, the vertical axis represents the distance (depth) from the sample surface. Brightness represents the density of atoms at that position (density decreases gradually in the order of red → vermilion → yellow → yellow-green → green → light blue → blue → black; refer to Figure 8 ). Figure 7 It is along Figure 6 The distribution of nitrogen atoms in the cross section of line A is measured.

[0062] like Figure 4 As shown in FIG. 1 , tungsten (i.e., tungsten carbide) is distributed approximately uniformly in the thickness direction. Figure 5 As shown, there is a distribution deviation of cobalt atoms in the thickness direction, but no regularity is confirmed in the depth dependence.

[0063] like Figure 6 As shown in FIG. 1 , it can be confirmed that the distribution of nitrogen atoms is diffused to a depth of at least 30 μm from the surface. Figure 7 As shown, there is a peak near the surface (near a depth of 2 μm in the figure), and the density varies at a depth of about 4 μm, but is roughly constant. The density of nitrogen atoms at the peak is about 4 times that at a depth of 4 μm.

[0064] It should be noted that in Figure 7 Although the peak of the nitrogen atom density appears to be located at a position from the surface to the inside, if we consider that the resolution of the electron beam is about 1 μm, as in Figure 6The middle surface is shown as the brightest, which shows that the peak of the density of nitrogen atoms is considered to be in the area less than 4μm (shallow) from the surface. Since tungsten carbide is nitrided by nitrogen atoms distributed in this area, this area becomes a domain where nitrogen and tungsten carbide coexist, which can be said to be a nitrided layer. Special attention should be paid to Figure 6 The depth of about 1μm from the surface. The blue color here becomes lighter in a straight line horizontally compared to the surrounding area, indicating that the density of nitrogen has increased. Figure 4 Obviously, there is tungsten (tungsten carbide) in this area. Figure 5 The depth of about 1 μm from the surface and Figure 4 When comparing the depth of about 1 μm from the surface, an area where tungsten and nitrogen coexist is observed. Therefore, it is believed that this area becomes a domain where nitrogen and tungsten carbide coexist, and the presence of this domain increases the hardness.

[0065] In addition, comparison Figure 5 and Figure 6 It can be seen that the distribution of the high-density nitrogen atoms from the surface to at least about 30 μm in depth is roughly consistent with the distribution of cobalt atoms. This is believed to be because the nitrogen atoms that have diffused into the interior beyond the above-mentioned nitride layer pass through the cobalt domain and diffuse rapidly into the deep area. On the other hand, it is believed that the diffusion rate in the tungsten (tungsten carbide) domain is slow, so the intrusion of nitrogen atoms stays at a depth of about 4 μm. Figure 6 , nitrogen atoms diffuse almost uniformly over the entire surface of the alloy from the surface to a depth of about 4 μm. This is contrary to the uneven density distribution of cobalt in this depth region. In addition, compared with Figure 3, the depth region where the hardness is improved (i.e., the nitride layer from the surface to a depth of about 4 μm) corresponds to the distribution of the nitrogen atoms. That is, the more nitrogen diffuses in the region, the higher the strength. This is consistent with the following result in Figure 3: the region up to 5 μm from the surface, which is a shallower region, has a higher rate of increase in hardness after nitriding than the region up to 9 μm from the surface. That is, it is believed that the nitrogen atoms present in the domain of tungsten (tungsten carbide) in the nitride layer contribute to the improvement of hardness, while on the other hand, the nitrogen atoms located in the domain of cobalt atoms do not contribute much to the improvement of hardness.

[0066] It is speculated that the reason for achieving such a distribution state in which nitrogen atoms are diffused roughly uniformly over the entire surface of the alloy from the surface to a depth of about 4 μm is that the treatment time is extended to 96 hours. In the past, it was common knowledge that the treatment time in the usual nitriding treatment was about several hours. Regarding superhard alloys, there has been no quantitative evaluation of the depth dependence of the distribution of hardness and nitrogen atoms.

[0067] According to the present invention, by significantly extending the processing time, a domain where nitrogen and tungsten carbide coexist, which has not been achieved in the past, can be formed, and the production of a superhard alloy with a good hardness of more than 2000 HV Vickers hardness in a depth region of several μm from the surface is successfully achieved. It should be noted that in the formation of the domain where nitrogen and tungsten carbide coexist, not only the processing time, but also the processing temperature and the nitriding method used also contribute. Therefore, by appropriately combining the nitriding method, the nitriding temperature, and the processing time, the formation of the domain where nitrogen and tungsten carbide coexist can be appropriately performed.

[0068] Here, several μm means, for example, a level roughly the same as the thickness of a hard film applied in surface treatment of cutting tools, etc. That is, in terms of the wear resistance of various tools, molds, etc., it is sufficient as long as the hardness is improved in a thickness region of several μm, and the hardness in a deeper region than that is almost not a problem. That is, the nitriding method of the present invention is particularly effective in improving the wear resistance by increasing the surface hardness of such a superhard alloy.

[0069] Explanation of symbols

[0070] 1...Atomic nitriding treatment device

Claims

1. A tungsten carbide superhard alloy, which is obtained by treating a tungsten carbide superhard alloy composed of tungsten carbide and an additive at a temperature of 550° C. to 800° C. for 12 hours to 120 hours using electron beam excited nitrogen plasma, characterized in that: When evaluated by electron probe microanalyzer (EPMA), there is a domain where nitrogen and tungsten carbide coexist within a depth of at least 1 μm from the surface. The first layer exists at 2μm to 10μm from the surface, the second layer exists in a region deeper than the first layer, and the number of nitrogen atoms per unit volume in the first layer is 3 to 5 times the number of nitrogen atoms per unit volume in the second layer in a domain where nitrogen and the additive coexist.

2. The tungsten carbide superhard alloy according to claim 1, characterized in that: The Vickers hardness measured with a measurement load of 10 g is 2000 HV to 3000 HV.

3. The tungsten carbide based superhard alloy according to claim 1, characterized in that: The Vickers hardness measured at a measurement load of 25 g is 1700 HV to 2500 HV.

4. The tungsten carbide based superhard alloy according to claim 1, characterized in that: The Vickers hardness measured at a test load of 10 g is increased by at least 30% compared to the case where nitriding is not performed.

5. The tungsten carbide based superhard alloy according to claim 1, characterized in that: The Vickers hardness measured at a test load of 25 g is increased by at least 10% compared to the case where nitriding is not performed.

6. The tungsten carbide based superhard alloy according to any one of claims 1 to 5, characterized in that: The Co content of the tungsten carbide-based superhard alloy is 0 wt% to 25 wt%.

7. A method for producing a tungsten carbide superhard alloy, wherein: The tungsten carbide-based superhard alloy is treated at a temperature of 550° C. to 800° C. for 12 to 120 hours using electron beam excited nitrogen plasma to produce a nitrided tungsten carbide-based superhard alloy.

Citation Information

Patent Citations

  • Carbide tool

    JP2002210525A

  • Hard film coated member and its manufacturing method

    JP2007217771A