Method for producing inkjet printable paper or foil for use as decorative paper or foil

By adding ink active compounds and multi-layer coating technology to the inkjet receiver coating, the problems of cracking, bleeding and dust release during the pressing process of inkjet printing paper or foil are solved, and printing quality and production efficiency are improved.

CN115302966BActive Publication Date: 2024-10-01UNILIN BVBA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211004544.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2017-06-14
Filing Date
2018-06-12
Publication Date
2024-10-01
Estimated Expiration
2038-06-12

AI Technical Summary

Technical Problem

In the existing technology, inkjet printing paper or foil is prone to cracking, bleeding and dust release problems during the pressing process, resulting in unstable printing quality and low production efficiency.

Method used

An inkjet receiver coating containing ink-active compounds stabilizes pigments through an electrical effect, avoids pigment clumping and bleeding, increases color density, and reduces dust release in a two-coat coating step.

Benefits of technology

Significantly improves the print quality of inkjet printing paper or foil, reduces bleeding and dust release, and improves production efficiency and product stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115302966B_ABST
    Figure CN115302966B_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing an inkjet printable paper or foil for use as a decorative paper or foil. A method for producing a paper or a thermoplastic foil or a plastic thermosetting resin foil printable using an inkjet printer, which is used as a decorative paper, a decorative foil in a laminate or a laminated board, respectively, wherein the method comprises at least the following steps: - a step of providing a paper layer (1), a foil, respectively; - a step of coating the paper layer (1), at least one side of the foil, respectively, with an inkjet receiver coating (3) comprising at least a pigment (6) and an adhesive (7); characterized in that the inkjet receiver coating (3) further comprises an ink-active compound. The invention also relates to the paper and foil obtained, and to a method for producing a board, wherein the paper (1) or the foil is provided with a printed pattern and used as a decoration in the board.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an invention patent application with an application date of June 12, 2018, application number 201880052682.7, and invention name “Method for manufacturing inkjet-printable paper or foil for use as decorative paper or foil”. Technical Field

[0002] The present invention relates to a method for manufacturing a board with a decorative surface (or so-called decorative board). The invention also relates to a method for manufacturing a paper or foil printable with inkjet for use as a decorative paper or foil in such a board, and to a paper or foil obtainable in this way. According to a variant, the decorative paper or foil obtained can be used in laminated components other than boards, such as for so-called CPL (compact laminate) or heterogeneous vinyl flooring for whole rooms.

[0003] More specifically, the invention relates to a method for manufacturing a laminated board, wherein the board comprises at least a base material and a top layer with a printed decoration arranged thereon. According to a first possibility, the method can be used to manufacture a board whose top layer is formed by a thermosetting resin and one or more paper layers, wherein the paper layers comprise a decorative paper with a printed pattern. According to a second possibility, the method can be used to manufacture a board whose top layer is formed by a thermoplastic material, such as PVC, comprising at least one thermoplastic decorative foil with a printed pattern. The board of the invention may relate to furniture boards, ceilings, floors or the like, wherein these boards preferably comprise a wood-based substrate, such as an MDF or HDF substrate (medium density fiberboard or high density fiberboard) or a substrate material comprising or essentially consisting of a chipboard. According to an alternative embodiment, which is particularly concerned in combination with the above-mentioned second possibility, the board comprises a filled synthetic composite substrate or a mineral-based substrate. These latter boards are also called LVT boards (luxury vinyl panels). Background Art

[0004] Traditionally, the decoration or pattern of such boards is printed on paper or thermoplastic foil by means of offset printing or rotogravure printing. The paper or foil obtained is used as decorative paper or decorative foil in so-called laminates or LVT boards. In order to manufacture the board of the first possibility mentioned above, a DPL process can be implemented. According to the DPL process (direct pressure laminate), the printed paper or decorative paper is provided with a melamine resin to form a decorative layer. Afterwards, a stack is formed comprising at least one board-shaped substrate, the decorative layer and possibly a protective layer located on top of the decorative layer, wherein the protective layer or covering layer is also based on resin and / or paper. The stack is pressed, and the pressing process causes the decorative paper, substrate and protective layer to be connected or adhered to each other, and also causes the resin present in the stack to be hardened. As a result of the pressing operation, a decorative board with a melamine surface is obtained, which can be highly wear-resistant. A counter layer or balancing layer can be applied at the bottom side of the board-shaped substrate, or alternatively, a decorative layer can also be attached to the bottom side, especially in the case of laminates for furniture. Such a counter layer or balancing layer or any other layer at the bottom side of the laminate limits or prevents possible bending of the decorative board and the same pressing treatment is applied at the side of the stack opposite to the decorative layer, for example by providing a resin-carrying paper layer as the lowest layer of the stack. For example, reference is made to the DPL process of EP 1 290 290, from which it is further known to provide a relief in the melamine surface during the same pressing treatment or pressing operation, i.e. by contacting the melamine surface with a structured pressing element, such as a structured pressing board. In order to manufacture the board of the above-mentioned second possibility, preferably, at least a lamination of a decorative foil and a transparent thermoplastic wear layer is also performed in order to form the top layer of the board. The mutual connection or adhesion of the decorative foil and the transparent wear layer is preferably obtained by a thermal lamination process, for example by using one or more heated pressing rollers. The top layer obtained can then be glued or thermally laminated to the substrate. In order to be able to form a relief in the top layer, a pressing treatment or pressing operation can be used. That is, by contacting the thermoplastic top layer with a structured pressing element, such as a structured pressing roller. Preferably, the pressing element is cooled while the thermoplastic top layer is provided to the roller under heating, so that the thermoplastic top layer can be cooled and frozen while in contact with the pressing element, thereby taking over the structural defects of the pressing element.

[0005] Printing papers or thermoplastic foils at affordable prices with analog printing processes (such as rotogravure or offset printing) inevitably leads to a large number of minimum order quantities for a particular decorative paper or foil and limits the flexibility that can be obtained. A change of decoration or pattern requires the printing device to be stopped for about 24 hours. This stop time is required to replace the printing roller, clean the printing device and adjust the color of the new decoration or pattern to be printed.

[0006] Digital printing techniques, in particular inkjet printing techniques, are becoming increasingly popular as an alternative to analog printing techniques for producing decorations or patterns on paper, on foil or directly on a plate-shaped substrate, possibly with an intermediate preparation layer. Such digital techniques can significantly increase the printing flexibility of the decoration. Reference is also made to EP 1 872 959, WO 2011 / 124503, EP 1 857 511, EP 2 431 190, EP 2 293 946, WO 2014 / 084787, WO 2015 / 140682 and WO 2015 / 118451, which disclose such techniques.

[0007] EP 1 232 041 discloses a method comprising at least the steps of providing a paper layer with a thermosetting resin and providing said resin provided with a paper layer, the paper layer having at least a part of said printed pattern. Preferably, a multi-color printed pattern is applied to achieve a decoration on said paper layer, for example, to represent a wood pattern. Such decoration extends over a large part of the paper layer provided with the resin or even over the entire resin. In EP 2 132 041 a digital printer is applied, more specifically an inkjet printer. However, such printed paper is already very difficult to reliably further process for the manufacture of laminates, such as in a DPL process, because pressing defects may originate from the resin surface, and milling, drilling or sawing through the laminate surface or at its edges often leads to cracks in the top layer. In addition, the inks or dyes of EP '041 may over-wet the paper layer and lead to wrinkling effects or bleeding when further processing the printed paper, resulting in an unstable and / or slow production process. In order to solve this problem, EP '041 proposes to dry the printed paper layer immediately.

[0008] EP1 044 822, EP1 749 676 and EP2 274 485 disclose the use of inkjet receiver coatings to improve the quality of printing on raw decorative paper. Such inkjet receiver coatings include pigments and polymers such as polyvinyl alcohol. Although improved, the color density of the print obtained on such treated paper is still inferior to the color density of the analog print.

[0009] As recognized in WO 2015 / 118451, the use of paper treated with an inkjet receiver coating can cause the printing device to malfunction. Dust can be released by the inkjet receiver coating and have various adverse effects on key components of the inkjet printer. For example, dust can clog one or more nozzles and cause printing failures. WO 2015 / 118451 proposes avoiding excessive bending of the paper in the printing device to minimize the release of dust.

[0010] During private research, the inventors have encountered the problem of dust release from a paper layer during subsequent impregnation, even when the paper layer has been printed on it. The released dust can contaminate the resin bath, rollers, cameras and other components in or in the immediate vicinity of the impregnation path, leading to defects in the final product or the component used.

[0011] WO 2015 / 140682 discloses primer substances which mitigate problems occurring in laminates of digitally printed thermoplastic decorative foils with a transparent thermoplastic wear layer, for example when applied to a print. The digital print can be provided on a decorative foil having an intermediate of an inkjet receiver coating. WO 2014 / 084787 discloses an inkjet receiver coating for a plastic foil, wherein the inkjet receiver coating substantially comprises an aqueous solution of a metal salt such as NaCl or CaCl2. Summary of the invention

[0012] The present invention aims firstly at an alternative method for manufacturing panels with a decorative surface or respectively paper, thermoplastic foil for such panels and seeks, according to several preferred embodiments thereof, to solve one or more of the problems arising in the prior art.

[0013] Thus, according to its first independent aspect, the present invention relates to a method for producing a paper or a thermoplastic foil or a plastic thermosetting resin foil (vitreous foil, dynamically cross-linked polymer foil, vitrimeric foil) printable with an inkjet printer for use as a decorative paper, a decorative foil, respectively, in a laminate, wherein the method comprises at least the following steps:

[0014] - a step of providing a paper layer, a thermoplastic foil or a plastic thermosetting resin foil, respectively;

[0015] - coating the paper layers, respectively, with an inkjet receiver coating comprising at least a pigment and a binder,

[0016] the step of:

[0017] Characterized in that the inkjet receiver coating further comprises an ink active compound.

[0018] The pigment of the inkjet ink is stabilized to obtain a good dispersion in the ink carrier and to avoid the pigment coagulation, in particular to avoid nozzle clogging in the inkjet head. The stabilization in this inkjet ink is obtained by the electrosteric effect between the pigments. Preferably, the ink-active compound is a substance that destroys the stability of the pigment in the ejected droplets, or in other words, an ink destabilizer. The inventors have found that the addition of this ink-active compound to the inkjet receiver coating based on a mixture of pigment and binder greatly improves the print quality, more specifically the color density, that can be obtained for the print on the paper layer or foil. The ink-active compound captures the ink, more specifically the pigment, when it first interacts with it. By interfering with or destroying the potential function on the pigment, the pigment is quickly precipitated out of the ink mixture and the pigment is only minimally driven into the coating together with the ink carrier. This immediate fixation of the pigment leads to excellent color density of the print. The pigment and binder system of the inkjet receiver coating absorbs the ink's carrier fluid, thereby also preventing bleeding (especially when printing on paper), or causing the ink to smear (especially when printing on foil), which in itself can also lead to improved print quality.

[0019] Preferably, in the method of the present invention, it is intended to print paper or foil using water-based inks or UV curing inks. Firstly, the paper and foil obtained by the method of the first aspect are intended to be printed using an inkjet printing device. However, the inventors have also found that the print quality is improved by using the thus treated paper and foil in an analog printing device.

[0020] According to the invention, the ink-active compounds can be selected from one or more of the following possibilities, the most important of which are listed below.

[0021] According to a first possibility, the ink active compound comprises a polyionic polymer, preferably polyDADMAC (polydiallyldimethylammonium chloride). The ionic polymer completely or partially neutralizes the electrostatic function of the pigment in the ink, thus causing the pigment to precipitate rapidly.

[0022] According to a second possibility, the ink active compound comprises a substance that changes (more specifically, reduces) the pH of the inkjet receiver coating. Preferably, the pH of the inkjet receiver coating composition is reduced to pH 3 or below by selecting the amount and type of the substance, and this selection is within the capabilities of the skilled person. Preferably, the substance is selected from the list consisting of the following items: formic acid, tartaric acid, acetic acid, hydrochloric acid, citric acid, phosphoric acid, sulfuric acid, AlCl3 and boric acid. The adjusted (more specifically reduced) pH (preferably, to pH 3 or below) increases the chemical affinity of the inkjet receiver coating with the ink and will interfere with the potential stabilizing function of the pigment, so that the dispersion of the pigment in the ink will quickly become destabilized.

[0023] According to a third possibility, the ink active compound comprises a metal salt, preferably a cationic metal salt. Preferably, the metal salt is selected from the list consisting of: CaCl2, MgCl2, CaBr2, MgBr2, CMA (calcium magnesium acetate), NH4Cl, calcium acetate, ZrCl4 and magnesium acetate. The cations of the dissolved metal salt will tend to neutralize the potential stabilizing function of the pigment. The most preferred cationic metal salts are CaCl2, MgCl2, CMA, calcium acetate and magnesium acetate, as the inventors have obtained the best results with these ink active compounds.

[0024] According to a fourth possibility, the ink active compound comprises a flocculant. Preferably, the flocculant is selected from the list consisting of: sodium aluminate, disulfate salts (such as alum), polyaluminium chloride, polyacrylates, dicyandiamide (e.g. Floquat DI5 from SNF) and polyacrylamide. The flocculant pulls the ink pigment out of the ink dispersion. Thereby preventing the pigment from penetrating deeply into the inkjet receiver coating. Mainly the carrier of the ink (e.g. water in the case of water-based inks) is absorbed more deeply into the inkjet receiver coating.

[0025] Preferably, the paper or foil provides 0.2 to 10 g / m 2 , and preferably between 0.5 and 5 g / m 2 between the dry coating weights of ink active compounds, more specifically, ink destabilizers.

[0026] Preferably, the paper or foil provides 0.2 to 10 g / m 2 , and preferably between 0.5 and 5 g / m 2 Preferably, the pigment has a dry coating weight of between 10 and 1600 m 2 The BET surface area is between 15 and 500 m / g and preferably between 15 and 500 m 2 / g. Preferably, the coating is such that the pigment is 2 The surface area of ​​paper or foil produces 100m 2 Up to 16000m 2 surface, or even better, per m 2 The surface of the paper or foil has a thickness between 150 and 5000 m 2 of the paint surface.

[0027] According to a most preferred embodiment, for the pigment of the inkjet receiver coating, at least or mainly silica particles are used. Preferably, the silica particles are treated with silanes. Typically, the silane treatment of the pigment improves the dust release properties of the obtained inkjet receiver coating (and therefore the treated paper or thermoplastic foil). The silane treatment may involve treatment with a coupling agent (such as aminoorganosilanes, hydroxysilanes, dibasic silanes and / or other silanes). Preferably, the coupling agent is selected so that the risk of yellowing of the obtained inkjet receiver coating during aging is low. Preferably, the coupling agent forms 0.1% to 10% of the total wet weight of the inkjet receiver coating.

[0028] According to a variant, the particles used at least or mainly for the pigments of the inkjet receiver coating are selected from the list consisting of calcium carbonate, silica, alumina, aluminosilicates, ordered mesoporous materials, modified silica, silicone, modified silicone, organic alumina, modified alumina, aluminates, modified aluminates, organic aluminates, modified organic aluminates, zeolites, metal-organic framework complexes and porous polar polymers.

[0029] Preferably, the paper or foil provides 0.2 to 10 g / m 2 , and preferably between 0.5 and 5 g / m 2 According to the most preferred embodiment, for the binder in the inkjet receiver coating, at least or predominantly polyvinyl alcohol is used.

[0030] According to a variation, the inkjet receiver coating contains a polymer selected from the following group as a binder, including: hydroxyethyl cellulose; hydroxypropyl cellulose; hydroxyethyl methyl cellulose; hydroxypropyl methyl cellulose; hydroxybutyl methyl cellulose; methyl cellulose; sodium carboxymethyl cellulose; sodium carboxymethyl hydroxyethyl cellulose; water-soluble ethyl hydroxyethyl cellulose; cellulose sulfate; vinyl alcohol copolymer; polyvinyl acetate; polyvinyl acetal; polyvinyl pyrrolidone; polyacrylamide; acrylamide / acrylic acid copolymer; polystyrene, styrene copolymer; acrylic acid or methacrylic acid polymer; styrene / acrylic acid copolymer; ethylene-acetic acid Ethylene ester copolymers; vinyl-methyl ether / maleic acid copolymers; poly(2-acrylamido-2-methylpropane sulfonic acid); poly(diethylenetriamine-co-adipic acid); polyvinyl pyridine; polyvinyl imidazole; modified polyethylene imine epichlorohydrin; ethoxylated polyethylene imine; polymers containing ether bonds, such as polyethylene oxide (PEO), polypropylene oxide (PPO), polyethylene glycol (PEG) and polyethylene ether (PVE); polyurethane; melamine resins; gelatin; carrageenan; dextran; gum arabic; casein; pectin; albumin; chitin; chitosan; starch; collagen derivatives; collodion and agar. The most preferred variants of the binder are polyvinyl acetate, ethylvinyl acetate, block copolymers based on polyvinyl acetate, block copolymers based on polyvinyl alcohol, acrylates, latexes, polyvinyl derivatives, VCVAC derivatives, polyurethanes based on polyols and isocyanates, polyurethanes based on polyurethanes and polyaldehydes, for example all as aqueous dispersions / emulsions or aqueous or solvent solutions.

[0031] As described above, preferred binders for inkjet receiving layers include polyvinyl alcohol (PVA), but according to variations, vinyl alcohol copolymers or modified polyvinyl alcohols may be used. The modified polyvinyl alcohol may be a cationic polyvinyl alcohol, such as a cationic polyvinyl alcohol grade from Kuraray, such as POVAL C506, POVAL C118 from Nippon Goshei.

[0032] Preferably, the inkjet receiver coating has a pigment to binder ratio broadly viewed between 0 / 1 or 0.01 / 1 and 25 / 1, preferably between 0 / 1 or 0.01 / 1 and 20 / 1. It is not excluded that the inkjet receiver coating is non-uniform and shows layerwise or areawise differences in the composition, in which case the above values ​​are average values ​​for the inkjet receiver coating as a whole.

[0033] The inkjet receiver coating further preferably comprises one or more of the following agents:

[0034] - Cross-linking agent: between 0.05 and 5 g / m 2Between, preferably between 0.2 and 2 g / m 2 Among them, for example, are selected from the list consisting of aldehydes, polyaldehydes, dialdehydes, alcohols, boric acid, borax, polyols, carbamates, polycarbamates, carbonic acid, glyoxal-based agents, zirconium-based agents and polycarbonic acid.

[0035] - Particle surface modifier or coupling agent: between 0.05 and 5 g / m 2 Between, preferably between 0.2 and 2 g / m 2 between, for example, selected from the following non-limiting list, including: aminosilane, ureidosilane, aldehyde silane, tetraethyl orthosilicate, silazane, organic modified silane, organic modified silazane, chlorosilane, organic modified chlorosilane, disilane, organic disilane, silsesquioxane, polysilsesquioxane, silane oligomer, organic modified silane oligomer, disilane oligomer, organic modified disilane oligomer, oligomeric silsesquioxane, and oligomeric silsesquioxane.

[0036] -Additives: between 0.005 and 2 g / m 2 Wetting agent between 0.05

[0037] Up to 1g / m 2 and / or between 0.005 and 2 g / m 2 Defoamer between 0.05 and 1 g / m 2 and / or between 0.005 and 2 g / m 2 The fungicide is preferably between 0.05 and 1 g / m 2 between.

[0038] Preferably, the paper layer or thermoplastic foil onto which the inkjet receiver coating is applied has a basis weight of 50 to 100 grams per square meter, for example, between 60 and 80 grams per square meter.

[0039] Preferably, in the case of a paper layer, the edges of the paper layer onto which the inkjet receiver coating is to be applied have been smoothed (German: ), preferably during its production. Smoothing reduces the amount of adhesive that penetrates into the paper core, so that the pigment contained therein can be better bound by the existing adhesive material and can reduce absorption variation. Preferably, the paper obtained using the method of the present invention (i.e., including the inkjet receiver coating) has a Gurley value between 30 and 120 seconds, and preferably, between 30 and 80 seconds. This paper layer leads to excellent print quality because the deposited ink tends to seep into the paper less, and it is easier to obtain and maintain consistency of position or so-called alignment between print patterns applied with different inkjet heads. In fact, a relatively high Gurley value causes the paper to be more stable in size because it is not so easy to absorb water. When impregnating with a thermosetting resin treatment of such a high Gurley value paper, it may be considered to reduce the speed of the impregnation route, use a pressurized impregnation technique, and reduce the viscosity of the impregnation resin.

[0040] According to a most preferred embodiment, the inkjet receiver coating is applied in at least two partial steps, wherein respectively a first layer is applied with a first composition and subsequently, a second layer is applied with a second composition, both compositions comprising at least the binder.

[0041] The inventors have demonstrated that applying the inkjet receiver coating in two partial steps results in better incorporation or binding of the pigment. The risk of dust release from the paper is reduced compared to the situation where the same amount of pigment is applied in only one coating step. According to the inventors, this surprising effect is attributed to the first layer forming a barrier for preventing the adhesive of the second layer from penetrating the paper layer. The adhesive of the second layer is more effective in binding the pigment, which would otherwise be loosely or poorly bound to the paper surface. Better embedded pigments lead to a significant reduction in dust released from the paper when the paper is further processed (e.g. printed, impregnated with resin).

[0042] Applying the inkjet receiver coating in two steps can further result in a more uniform coating of the entire inkjet receiver coating. Where the first composition can be partially absorbed in the paper layer in a non-uniform manner and thus can result in an uneven first layer with a small effective portion, the second composition can at least to some extent even out possible unevenness.

[0043] Coating the inkjet receiver coating in at least two steps allows for the creation of a gradient of certain components of the coating through its thickness, since the first composition and the second composition may have different components or may both have components present in different concentrations, as will be further explained. Coating the inkjet receiver coating in at least two steps further allows for the creation of coating layers of varying thickness.

[0044] When starting from a paper layer with a low average air resistance (e.g., a Gurley value of 30 seconds or less, such as 25 seconds or less), the method of the present invention and especially those embodiments in which the inkjet receiver coating is applied in two partial steps are particularly concerned. In this case, the adhesive contained in the first layer tends to be absorbed in large quantities in the mass of the paper, leaving a large amount of unbound pigment content on the surface. Preferably, the paper layer is a standard printing base paper or another untreated paper layer with an average air resistance represented by a Gurley value of 30 seconds or less. Of course, it is not excluded that in the method of the present invention, according to an alternative embodiment, it starts with a paper treated with a thermosetting resin before applying the inkjet receiver coating. Preferably, in the latter case, the paper layer provided with the resin has an average air resistance of a Gurley value of 100 seconds or less. In this case as well, applying the inkjet receiver coating in two partial steps has significant advantages, for example, with respect to dust release, minimization of bleeding of the ejected ink, and uniform coating of the inkjet receiver coating.

[0045] Typically, the method of the present invention allows the application of an inkjet receiver coating with a higher pigment content, and therefore has a higher capacity or higher speed to absorb the carrier liquid (e.g., water in the case of aqueous coloring ink) of the applied ink, while maintaining or even reducing the dust released from the printable surface of the treatment. The higher capacity or speed to absorb the carrier liquid can lead to higher print clarity. Since the carrier liquid is absorbed into the inkjet receiver coating substantially vertically, i.e., there is no large amount of lateral bleeding, the pigment remains in the position where the ink is applied, i.e., the pigment is not driven laterally with the ink carrier liquid. As described above, since the coating of the second layer of the inkjet receiver coating flattens the first layer partially or completely, any bleeding that is still effective can manifest itself in a more uniform manner. The availability of the ink-active compound in the inkjet receiver coating helps to immediately capture the ink pigment at the surface of the paper or foil being treated.

[0046] Preferably, in the case where the inkjet receiver coating is applied in two partial steps, the first layer and the second layer differ in that they exhibit one or more of the following properties:

[0047] 1.- The first layer and the second layer contain a pigment and a binder, although the ratio of pigment to binder is different;

[0048] 2.- Different properties for the dry weight of the material applied for the first and second layers;

[0049] 3.- The first layer and the second layer contain a pigment and a binder, wherein

[0050] The average particle size of the pigment included in the first layer is larger than the average particle size of the pigment included in the second layer;

[0051] 4.- The first layer and the second layer contain ink-active compounds of a nature, albeit of different compositions;

[0052] 5.- The first layer comprises at least a pigment and a binder, and the second layer has no pigment or at least comprises less pigment than the first layer or comprises less than 10% of the pigment content of the first layer.

[0053] With regard to the first of these properties, preferably the first composition has a pigment to binder ratio that is greater than the pigment to binder ratio of the second composition, in such a way that the binder of the second layer primarily binds the pigment of the first layer and evens out any inhomogeneities in the first layer.

[0054] Preferably, the ratio of pigment to binder in the second composition is less than 2:1, and preferably between 0:1 and 2:1. When the ratio in the second composition is lower than 1.5:1, extremely low dust release has been demonstrated. As described above, in some embodiments, it is not excluded that the second composition does not have a pigment.

[0055] Whether or not combined with the preferred second composition mentioned, the ratio of pigment to binder in the first composition may be chosen to be between 1:1 and 25:1 or between 2:1 and 10:1, and preferably 3.5:1 or more, and even better 5.5:1 or more, although preferably less than 10:1.

[0056] Good bonding of the first and second compositions is achieved when the ratio of pigment to binder in the second composition is between 0: 1 and 2: 1 and the ratio of pigment to binder in the first composition is between 3.5: 1 and 10: 1, inclusive. However, it is clear that within the scope of the present invention, the ratio of pigment to binder of the first and second compositions may be equal or substantially equal.

[0057] As regards the second of said properties, it is of course not excluded that the same dry weight will be applied for both layers. In this case, however, preferably, the ratio of pigment to binder applied in the first composition and the second composition is different. Preferably, for each of said two layers, a dry weight of material between 0.5 and 5 grams per square meter is applied to the paper layer, and even better between 0.8 and 4.5 grams per square meter. In the case where the dry weight of material applied by said first and second layers is different, preferably the first layer comprises the highest dry weight of material, for example at least 20% more than the second layer. The composition of each layer preferably comprises between 12% and 20% by weight of solid matter, so that the wet applied material applied to the paper layer is preferably between 4 and 23 grams per square meter in terms of the wet weight of the layer.

[0058] Regarding the third described property, larger pigment particles are preferably included in the first composition. The use of large particles in the first layer provides excellent absorption of the ink carrier, while the use of small particles in the second layer provides a flattening effect at the surface of the paper layer and well reduces dust release. Preferably, in this case, the pigment particles in the first composition have an average particle size between 1 and 20 microns. Preferably, the pigment particles in the second composition have an average particle size between 100 nanometers and 1 micron. Of course, it is generally not excluded that the first composition and the second composition will contain pigment particles with similar or identical average particle sizes.

[0059] With regard to the fourth mentioned property, preferably, the second layer comprises a higher amount of the ink active compound than the first layer. The availability of the ink active compound at the upper layer of the coating results in an effective interaction with the pigment in the jetted ink droplets. The ink active compound preferably comprises a flocculant or other ink destabilizer, such as a cationic metal salt.

[0060] The adhesive used in the present invention (or the adhesive contained in the first composition and / or the second composition) can also be formed by a mixture of the possibilities listed above for the adhesive. According to a specific embodiment, a mixture of polyvinyl alcohol and ethylene vinyl acetate (EVA) and / or polyvinyl acetate (PVAc) is used as an adhesive, wherein preferably, the main component of the adhesive is polyvinyl alcohol, and for example at least 5% by weight of EVA and / or PVAc is used. The inventor has recorded that the paper or foil treated in this way has increased flexibility compared to the paper or foil in which the adhesive is essentially polyvinyl alcohol. The increased flexibility and reduced dust release are advantageous in the further processing of the paper and foil treated in this way (for example, in a printing device).

[0061] Preferably, the binder in the first composition and the second composition is the same, or at least the major component of the binder is the same. As mentioned before, the major component is preferably polyvinyl alcohol.

[0062] As the pigment commonly used in the present invention, or as the pigment in the first composition and / or the second composition, in fact any inorganic pigment can be used and most preferably a porous inorganic pigment. A mixture of two or more pigments can also be used. The pigment used is preferably an inorganic pigment that can be selected from neutral, anionic and cationic pigment types. Useful pigments include, for example, silicon dioxide, silicone, talc, clay, hydrotalcite, kaolin, diatomaceous earth, calcium carbonate, magnesium carbonate, basic magnesium carbonate, aluminosilicate, aluminum hydroxide, aluminum oxide (aluminum oxide), titanium oxide, zinc oxide, barium sulfate, calcium sulfate, zinc sulfide, satin white, aluminum oxide hydrates such as boehmite, zirconium oxide or mixed oxides. The inorganic pigment is preferably selected from the following group, comprising hydrated aluminum oxide, aluminum oxide, aluminum hydroxide, aluminum silicate and silicon dioxide. Particularly preferred inorganic pigments are silicon dioxide particles, colloidal silicon dioxide, aluminum oxide particles and pseudo-boehmite, because they form better porous structures. When used in this article, the particles can be primary particles directly used as is, or they can form secondary particles. The preferred type of alumina hydrate is crystalline boehmite, or γ-AlO(OH). Useful boehmite types include DISPERAL HP14, DISPERAL 40, DISPAL 23N4-20, DISPAL 14N-25 and DISPERAL AL ​​25 from Sasol; and MARTOXIN VPP 2000-2 and GL-3 from Martinswerk GmbH. Useful cationic alumina (alumina) types include α-Al2O3 types (such as NORTON E700 available from Saint-Gobain Ceramics & Plastics, Inc), and γ-Al2O3 types (such as ALUMINUM OXID C from Degussa). Other useful inorganic pigments include aluminum hydroxide (such as Bayerite), or α-Al(OH)3 (such as PLURAL BT) available from Sasol and Gibbsite, or γ-Al(OH)3 (such as MARTINAL grade and MARTIFIN grade from Martinswerk GmbH, MICRAL grade from JM Huber; HIGILITE grade from ShowaDenka KK). As described above, the preferred type of inorganic pigment is silica which can be used in its anionic form or after cationic modification. Silica can be selected from different types, such as crystalline silica, amorphous silica, precipitated silica, fumed silica, silica gel, spherical and non-spherical silica. Silica may contain a small amount of metal oxides selected from the Al, Zr, Ti groups. Generally, depending on their production method, silica particles are divided into two types: wet particles and dry (fumed or gas phase) particles.In the wet process, two types of reactions can be used to make these precipitated silica materials. The first is a method of treating sodium silicate with an inorganic acid to obtain precipitated silica. In the second method, pure silica materials are prepared by polycondensation of alkoxy or halosilanes. The gas phase process includes two types; one includes high temperature gas phase hydrolysis of silicon halides to obtain anhydrous silica (flame hydrolysis), and the other includes thermal reduction evaporation of quartz sand and coke in an electric furnace, followed by oxidation in air to also obtain anhydrous silica (arc process). "Fumed silica" is meant to represent the anhydrous silica particles obtained in the gas phase process.

[0063] For the silica particles preferably used in the inkjet receiving layer of the present invention, precipitated silica particles are particularly preferably used. The difference between precipitated silica and fumed silica is the density of the surface silicon hydrocarbon group and the pores that exist or do not exist therein, and the two different types of silica have different properties. The inventors are surprised to note that, compared to fumed silica, the use of precipitated silica as the pigment in the inkjet receiver coating causes a higher color density of prints to be presented on the coating, and achieves better adhesion with the transparent layer to be laminated on the top of the prints afterwards. The inventors believe that the higher smoothness of the inkjet receiver coating with fumed silica causes a reduction in color density and lamination strength.

[0064] Alternatively, organic pigments can be used in the inkjet receiver coating, preferably selected from the list consisting of polystyrene, polymethyl methacrylate, silicone, melamine formaldehyde polycondensate, urea formaldehyde polycondensate, polyester and polyamide. Mixtures of inorganic and organic pigments can be used. In addition, hybrid pigments such as organosilicon materials can be used. However, the most preferred pigments are inorganic pigments.

[0065] Preferably, the pigment contained in the inkjet receiver coating has an average particle size of 100 nm to 20 μm, with 1-12 μm being ideal and 2 to 7 μm being even better. Pigments with small particle sizes can be easily bonded to paper or foil, while pigments with large particle sizes show great water absorption, resulting in good print quality. The optimal average particle size is in the range of 1 to 12 μm, preferably 2 to 7 μm.

[0066] Preferably, the pigment contained in the inkjet receiving layer has a particle size of 20 to 1600 m 2 The average surface area is preferably between 250 and 1600 m 2 / g in order to obtain good absorption of the ink carrier.

[0067] Preferably, the pigments contained in the inkjet receiver coating have an average pore volume of 0.2 to 3 ml / g, preferably between 1 and 3 ml / g.

[0068] With an average particle size between 2 and 7 μm, 300 to 800 μm 2 Pigments having an average surface area of ​​100 ml / g and an average pore volume between 1 and 2 ml / g provide an ideal combination of absorbency, print quality and adhesion (ie, lack of dust release from the treated paper).

[0069] Preferably, usually, the inkjet receiver coating, or in either of the first composition or the second composition, or in both the first composition and the second composition, further comprises a crosslinking agent, preferably selected from the list consisting of the following items: aldehydes, aziridines, isocyanates, epoxides and borates. This crosslinking agent further binds the pigment in the inkjet receiver coating and further limits the dust released from the printing paper or thermoplastic foil so treated. The availability of the crosslinking agent in either composition further significantly increases the pot life of the related composition. Preferably, the first composition and / or the second composition include a crosslinking agent in an amount of 0.1% to 25% of the total wet weight of the first composition and / or the second composition.

[0070] Typically, the inkjet receiver coating or the first composition and / or the second composition may further comprise additives other than the crosslinking agent, the total amount accounting for 0.1% to 2% of the total wet weight of the first composition and the second composition, respectively. Such additives may be one or more of a fungicide, a defoamer, a leveling agent, a wetting agent (such as an alkylphenol ethoxylate), a thickener (such as hydroxyethyl cellulose or xanthan gum).

[0071] The leveling agent used can be made of APEO (alkylphenol polyoxyethylene ether).

[0072] The preservative used may be made of BIT or MIT (phenylisothiazolinone or methylisothiazolinone).

[0073] The defoamer used can be made of silicone polyether copolymer.

[0074] Preferably, the paper obtained with the process of the invention is provided with a thermosetting resin, such as a melamine resin, preferably after providing it with a print pattern by means of inkjet printing. Thus, preferably, the paper layer is provided with an inkjet receiver coating only on one side thereof, i.e. on the side arranged to be printed. The other opposite side is preferably not treated, so that this opposite side shows the original porosity of the paper layer starting therefrom. The resin can then be provided into the paper core essentially from the bottom side. In order to allow a sufficient impregnation of the paper with the inkjet receiver coating, the speed of the impregnation path can be reduced, the resin can be made less viscous, the impregnation can be pressurized and / or the resin can be heated, for example to between 45 and 100° C.

[0075] In general, it is noted that, although the paper and foil obtained with the process of the invention can be printed with an inkjet printer, it is not excluded that the paper or foil may be finally printed using other technologies, such as rotogravure or offset printing. In this case as well, reduced dust emission and potentially better print quality are of interest. This is especially true when using aqueous inks.

[0076] Preferably, the inkjet receiver coating is a liquid substance deposited on the paper layer and is preferably force dried, for example in a hot air oven or with the aid of infrared or near infrared light or with the aid of microwave drying. In the case where the inkjet receiver coating is applied in at least two partial steps, preferably, at least this drying operation occurs between the partial steps of the first aspect of the invention. Preferably, the liquid substance is an aqueous suspension of at least the binder (and possibly the pigment). Preferably, the first composition has a dry matter content of 8% to 25% by weight of the liquid substance. Preferably, the second composition has a dry matter content of 4% to 20% by weight of the liquid substance. Preferably, the dry matter content expressed as a percentage by weight is higher in the first composition than in the second composition.

[0077] The deposition of the liquid substance of the inkjet receiver coating can be obtained in any way, by means of printing, for example inkjet printing, but preferably by means of coating techniques, such as roller coating (for example by means of one or more embossing rollers), spraying, metering rollers, beading coating, spreading, slot die coating. By the latter technique, a coating covering at least 80% of the surface of the paper layer or foil is preferably obtained. Preferably, the excess liquid substance is first applied to the paper layer, and the excess material is then removed again (for example, squeezed out) until the required weight is obtained. Inline measurement systems are satisfactory to guide and control the weight of the inkjet receiver coating. This technique leads to the risk of uncoated areas of the paper, which can lead to local defects in the printed pattern. The preferred device for applying the liquid substance is a coating device comprising counter-metering rollers. Such rollers can produce a smooth coating surface.

[0078] The deposition of liquid substances for inkjet receiver coating can be performed immediately before the printing operation in the immersion approach or alternatively on the printing device. This last case solves any possible problem of the limited shelf life of the inkjet receiver coating. Preferably, the deposition of liquid substances is carried out when the paper or foil is still in a "continuous" shape (i.e., taken out from the roller without cutting). This technology allows the inkjet receiver coating to be coated more evenly. In the case where the coating is completed completely or partially on the printing device, the printing device is preferably a roller-to-roller or roller-to-sheet printer, including a coating device upstream of the print head, such as a roller coater and / or an additional print head suitable for printing liquid substances for the corresponding sub-layers of the inkjet receiver coating. This additional print head (e.g., an additional row of print heads) may have nozzles with a larger diameter than the nozzles used for the actual printing pattern. A resolution of 1 to 100 or even 1 to 25 dots per inch may be sufficient for these nozzles. A larger diameter allows the spraying of more viscous substances. According to a specific embodiment, the first layer is coated on the paper or foil using a roller, and the second layer is coated using this additional print head. This embodiment is of particular interest when the ratio of pigment to binder in the second composition is low, ie below 2: 1. In this case, the liquid substance for the second layer will be easier to apply with the additional print head.

[0079] The liquid substance for the inkjet receiver coating preferably shows a viscosity of 10 to 75 seconds at 20°C Din cup 4. This property allows the liquid substance to be applied directly to the surface of a paper layer or foil. In experiments, a solid content of about 12% and a viscosity of about 24 seconds produced a sufficiently uniform coating on a previously untreated paper layer, for example when applied by a roll coater.

[0080] Clearly, instead of a paper layer, a thermoplastic foil, such as a polyvinyl chloride (PVC) foil, a polypropylene (PP) foil, a polyethylene (PE) foil, a polyethylene terephthalate (PET) foil or a thermoplastic polyurethane (TPU) foil is treated with the inkjet receiver coating according to the first aspect.

[0081] Preferred binders for such foils are polyurethane-based, acrylate-based or polyvinyl acetate-based. Furthermore, in the case where the inkjet receiver coating is applied in at least two partial steps, the binder content in the first composition can be slightly reduced compared to the processing of the paper layer, since less absorption into the layer core is expected. In this case, preferably, the ratio of pigment to binder in the first composition is between 1:1 and 6:1.

[0082] It is noted that the use of an inkjet receiver coating having a pH of 3 or below forms a specific independent inventive aspect of the present invention per se, whether or not this pH has been obtained according to the second possibility of ink-active compounds described above, and independently of any other possible composition of the inkjet receiver coating. This specific inventive aspect can be defined as a method for producing a paper or thermoplastic foil or plastic thermosetting resin foil printable with an inkjet printer for use as a decorative paper, decorative foil, respectively, in a laminate, wherein the method comprises at least the following steps:

[0083] - a step of providing a paper layer, a thermoplastic foil or a plastic thermosetting resin foil, respectively;

[0084] - coating the paper layer and at least one side of the foil with a composition to form an inkjet interface

[0085] The step of collecting the coating;

[0086] Characterized in that the composition has a pH of 3 or below. As explained above, the low pH of the composition and the resulting coating has a high tendency to destroy the potential stability of the pigment in the inkjet ink, resulting in a high print quality. It is clear that the composition can be obtained according to the above-mentioned second possibility, and this specific independent aspect can have preferred embodiments corresponding to the preferred embodiments listed above for the above-mentioned first independent aspect of the invention, and may but does not necessarily contain one or more of the ink-active compounds, binders or pigments listed above. Preferably, the composition includes at least a binder, such as PVA, and a substance that reduces the pH to 3 or below.

[0087] It is clear that the present invention also relates to a paper layer and a thermoplastic foil obtained using the method of the first aspect of the present invention. In accordance with a second independent aspect, the present invention also relates to a paper or a thermoplastic foil or a plastic thermosetting resin foil for inkjet printing, wherein the paper or foil is provided at least on one side with an inkjet receiver coating comprising at least a pigment and a binder, characterized in that the inkjet receiver coating further comprises an ink-active compound and in that the inkjet receiver coating preferably has a ratio of pigment to binder of between 0 / 1 or 0.01 / 1 and 25 / 1, preferably between 0 / 1 or 0.01 / 1 and 20 / 1. Preferably, the paper or foil comprises from 0.2 to 10 g / m2 of the ink-active compound in a dry coating weight. 2 , and even better between 0.5 and 5 g / m 2 The ink active compound preferably comprises at least a flocculant.

[0088] Further, the paper or foil preferably comprises a pigment in a dry coating weight of from 0.2 to 10 g / m 2More preferably, the paper comprises an adhesive preferably in an amount of from 0.2 to 10 g / m 2 , and preferably between 0.5 and 5 g / m 2 between.

[0089] Further, the paper or foil may further exhibit one or more of the following properties:

[0090] - the paper or foil is substantially composed at its surface of the adhesive and / or the ink active

[0091] Formation of sexual compounds;

[0092] - the paper or foil is provided with a quantity of pigment having a particle surface area of ​​between 100 and 16000 m 2 Surface area of ​​pigment / m 2 between the surfaces of paper or foil, and

[0093] Preferably between 150 and 5000m 2 / m 2 between;

[0094] - the paper or foil comprises from 0.05 to 5 g / m 2 , preferably between 0.2 and 2 g / m 2 between

[0095] of the dry coating weight of a cross-linking agent;

[0096] - the paper or foil comprises from 0.05 to 5 g / m 2 , preferably between 0.2 and 2 g / m 2 between

[0097] of dry coating weight of surface modifier;

[0098] - the paper or foil comprises from 0.005 to 2 g / m 2 , preferably between 0.05 and 1 g / m 2 dry coating weight of wetting agent between ;

[0099] - the paper or foil comprises from 0.005 to 2 g / m 2 , preferably between 0.05 and 1 g / m 2 between 100 and 200 g of dry coating weight of defoamer;

[0100] - the paper or foil comprises from 0.005 to 2 g / m 2 , preferably between 0.05 and 1 g / m 2 between dry coating weights of fungicide.

[0101] According to its third independent aspect, the present invention further relates to a method for manufacturing a laminate, wherein the board comprises at least a base material and a top layer with a printed decoration arranged thereon, wherein the top layer is essentially formed by a thermosetting resin and one or more paper layers, wherein the paper layers comprise decorative paper based on a paper for inkjet printing according to the second independent aspect and / or obtained by means of a method according to the first independent aspect and / or a preferred embodiment of these aspects. According to its fourth independent aspect, the present invention also relates to a method for manufacturing a laminate or a laminate, wherein the laminate or laminate comprises at least a carrier (such as a non-woven textile sheet) or a base material, and a top layer with a printed decoration arranged thereon, wherein the top layer is essentially formed by a thermoplastic material including one or more thermoplastic foils, wherein the thermoplastic foils comprise decorative foils based on a thermoplastic foil for inkjet printing obtained by means of a method according to the first independent aspect and / or a preferred embodiment of this first aspect, as long as they involve the processing of thermoplastic foils.

[0102] Preferably, in the third aspect, the paper for inkjet printing printed by means of an inkjet printer is impregnated with a certain amount of the thermosetting resin and attached to the base material by means of a hot pressing process. Preferably, in the fourth aspect, the thermoplastic foil for inkjet printing is printed by means of an inkjet printer and attached to the base material by means of a hot pressing process. Preferably, the inkjet printer operates based on water-based inks, wherein, more specifically, a single-pass inkjet printer and / or an inkjet printer operating in a single-pass mode is preferred.

[0103] It is clear that the paper layer with the inkjet receiving layer of the present invention can be used in a method for manufacturing a board with a decorative surface, wherein the board comprises at least a substrate and a top layer comprising a thermosetting resin, wherein the top layer comprises a paper layer with a printed pattern, characterized in that for the portion providing the printed pattern, a pigment comprising an ink deposited on the paper layer by means of a digital inkjet printer is used, and that the total volume of the pigment comprising the ink deposited on the paper layer has a dry weight of 9 grams per square meter or less, preferably 3 to 4 grams per square meter or less, wherein for the pigment comprising the ink, a water-based ink or so-called aqueous ink is used. The limitation of the dry weight of the applied ink results in an ink layer that reduces the risk of pressing defects and cracking in the top layer. In fact, the possible interference between the ink layer and the thermosetting resin during the pressing operation is limited. Because the ink load is limited to a maximum of 9 grams per square meter, the wrinkling or swelling of the paper caused by the ink can be made to an acceptable level, which ensures the stability of further processing. Preferably, for the pigment comprising the ink, an organic pigment is used. It is well known that organic pigments are more stable when exposed to sunlight or other ultraviolet sources. Preferably, said pigment of said pigment comprising ink has an average particle size of less than 250 nanometers. Preferably, said dry weight of the deposited pigmented ink is 5 grams per square meter or less, for example, 4 or 3 grams per square meter or less. Preferably, the printed pattern consists entirely or at least substantially of such pigmented ink, wherein the printed pattern covers a large part of the surface of the paper layer, and preferably 80% or more. Preferably, said total volume of the deposited pigment comprising ink is less than 15 ml, or even better, less than 10 ml or still less, for example 5 ml or less.

[0104] Preferably, the paper layer of the present invention is opaque and / or contains titanium oxide as a whitening agent.

[0105] Preferably, the printed pattern applied to the paper layer of the present invention covers a majority of the surface of the paper layer, and preferably 80% or more.

[0106] Preferably, the paper layer is provided with a thermosetting resin in an amount equal to 40% to 250% of the dry weight of the resin compared to the weight of the paper, before or after printing and before or after application of the inkjet receiver coating. Experiments have shown that this range of applied resin provides for sufficient impregnation of the paper, largely avoiding cracking and making the paper highly dimensionally stable.

[0107] Preferably, the paper layer is provided with a certain amount of thermosetting resin that at least saturates the paper core with resin before or after printing and before or after applying the inkjet receiver coating. This saturation can be achieved when the amount of resin is set to correspond to at least 1.5 or at least 2 times the weight of the paper. It should be clear that the resin provided on the paper layer does not necessarily have to be present only in the paper core, but can form a surface layer on both flat sides of the paper. The inkjet receiver coating can then be present on the surface of the paper with the intermediate of this surface layer of thermosetting resin. According to a specific embodiment, the paper layer is first impregnated or saturated, and thereafter, the resin is partially removed at least on its side to be printed, and the inkjet receiver coating can be provided.

[0108] Preferably, the obtained paper layer provided with resin (ie after being provided with the thermosetting resin) has a relative humidity lower than 15% and better still, 10% by weight or less.

[0109] Typically, paper and inkjet receiver coatings, whether provided with resin or not, have a relative humidity of less than 15% when printed, and better still, 10% or less by weight.

[0110] Preferably, the step of providing the paper layer with a thermosetting resin involves applying a mixture of water and resin to the paper layer. Application of the mixture may involve dipping the paper layer in a bath of the mixture and / or spraying, spraying or otherwise applying the mixture to the paper. Preferably, the resin is provided in a metered manner, for example by using one or more squeeze rollers and / or doctor blades to set the amount of resin added to the paper layer.

[0111] Preferably, the thermosetting resin is a melamine-based resin, more specifically, a melamine-formaldehyde resin having a formaldehyde to melamine ratio of 1.4 to 2. Such melamine-based resins are resins that undergo polycondensation when exposed to heat during a pressing operation. The polycondensation reaction produces water as a by-product. The present invention is particularly concerned with these types of thermosetting resins, i.e., those that produce water as a by-product. The water produced, as well as any residual water in the thermosetting resin before pressing, must leave the hardened resin layer to the greatest extent possible before being captured and causing a loss of transparency in the hardened layer. Existing ink layers can hinder the diffusion of vapor bubbles to the surface, however, the present invention provides measures for limiting such hindrance. An inkjet receiver coating is beneficial in this regard because it can provide an additional buffer for capturing such escaping vapor. When a porous and / or hydrophilic inkjet receiver coating is used (which is the case when, for example, silica and / or polyvinyl alcohol is used), some of the water vapor generated when the thermosetting resin of the paper layer is cured during pressing can be absorbed by the coating, making the process less prone to press defects such as being locked in water vapor bubbles. Other examples of such thermosetting resins that result in similar polycondensation reactions include urea-formaldehyde based resins and phenol-formaldehyde based resins.

[0112] Preferably, the paper layer is impregnated with the resin only after application of the inkjet receiver coating and after printing. In this way the inkjet receiver coating is completely unaffected by the water contained in the water-resin mixture applied for impregnation purposes.

[0113] As is evident from the above, the method of the third aspect of the invention preferably comprises a step of hot pressing the printed and provided with resin paper layers, at least to cure the resin of the obtained resin-provided decorative paper. Preferably, the method of the invention forms part of a DPL process as described above, wherein the printed and provided with resin paper layers of the invention are stacked to be pressed into a decorative layer. It is of course not excluded that the method of the invention will form part of a CPL (compact laminate) or HPL (high pressure laminate) process, wherein the decorative layer is hot pressed at least together with a plurality of core paper layers impregnated with resin, such as so-called kraft paper, to form a substrate beneath the decorative layer, and wherein in the case of HPL the obtained pressed and cured laminate or laminate is bonded to another substrate, such as to a particle board or an MDF or HDF board.

[0114] Preferably when the decorative layer is loose or already connected or adhered to the substrate, preferably a further resin layer is applied over the printed pattern after printing (eg by superposition), ie a carrier layer or a liquid coating provided with resin.

[0115] The paper layer or foil of the present invention may be a colored, tinted and / or dyed base paper or foil. The use of a colored and / or dyed base layer can further limit the dry weight of ink deposited to obtain a specific pattern or color. In the case of paper, preferably, the dye or pigment is added to the pulp before the paper is formed. According to a variant, the inkjet receiver coating on the paper layer or foil to be printed is colored or colored with a colored pigment. However, according to general disclosures, the pigment contained in the inkjet receiver coating is preferably colorless or white.

[0116] Preferably, for printing the paper layer or foil of the invention, a digital inkjet printer is used that allows the ejection of ink droplets having a volume of less than 50 picoliters. The inventors have found that operating with droplets having a volume of 15 picoliters or less (e.g. 10 picoliters) brings considerable advantages in limiting the dry weight of the deposited ink. Preferably, a digital inkjet printer is used that allows operating with several volumes of ink droplets in the same print, or operating in so-called halftones or grayscale. The possibility of halftone or grayscale printing can further limit the dry weight of the deposited ink while maintaining excellent print clarity. Preferably, a digital inkjet printer is used that allows a clarity of at least 200 dpi, or even better at least 300 dpi (dots per inch). Preferably, the digital inkjet printer is a single-pass type, in which the paper layer or foil provides the printed pattern with a single continuous relative movement of the paper layer relative to the printer or print head. It is not excluded to use other digital inkjet printers to practice the invention, such as so-called multi-pass printers or plotter-type printers. In the case of single-pass printers as well as multi-pass printers, the print head preferably extends over the entire width of the paper to be printed. This is not the case for plotter arrangements in which the print head needs to perform a scanning movement in the width direction of the paper layer. However, such printers are not excluded from application in the method of the present invention. It is noted that multi-pass printers have the advantage that any failed nozzles can be hidden by the printing of subsequent passes. In printers of this type, the nozzles can be slightly moved between passes so that a specific position of a paper point is printed by several nozzles. By means of a multi-pass device or even by a plotter, automatic maintenance or cleaning can be performed between subsequent passes when necessary. The problem of failed nozzles is particularly relevant when using inks containing water-based pigments or so-called aqueous pigments. In fact, since the water has dried, the nozzles may be clogged with ink pigments. For example, the risk of nozzle failure is reduced by using UV curable inks. In addition, when using an inkjet receiver coating, generally, the risk of nozzle failure may increase. However, the double-layer coating of the inkjet receiver coating according to the first aspect of the present invention enhances the time of autonomous production due to reduced dust release.

[0117] It is clear that according to the most preferred embodiment of the invention, the paper layer is still flexible when printing and it is attached or placed on the plate-shaped substrate only after printing. According to a variant, the paper layer is already attached or loosely placed on the plate-shaped substrate when printing. The possible attachment to the substrate can be achieved by means of urea-based, phenol-based, melamine-based, polyurethane-based glues and similar adhesives. This attachment can be achieved by means of a pressing process, whether or not it is hot.

[0118] Preferably, the method of the third aspect of the invention further comprises the step of applying a counter layer or balancing layer at the surface of the substrate opposite to the printed paper layer. In the case of a paper-based decorative layer, the counter layer or balancing layer preferably comprises a paper layer and a thermosetting resin, preferably the same resin as the top layer.

[0119] Preferably, mutual adhesion of the plate-shaped substrate, possible counter layer and possible transparent or translucent layer is obtained in the same pressing process.According to a most preferred embodiment of the third aspect, these steps are performed in a DPL process.

[0120] According to the most important embodiment of the invention, a standard printing paper (like paper for rotary photocopying) having a weight between 60 and 90 grams per square meter is provided with an inkjet receiver coating according to the first aspect of the invention and printed with a wood pattern using a digital inkjet printer with an aqueous pigmented ink. Subsequently, the printed paper layer is provided with a melamine resin by means of a standard impregnation route; i.e. by means of a roller, a dip, a spray and / or a sputtering device. The paper layer provided with the resin is then dried until its residual moisture reaches less than 10%, preferably about 7%. The stack formed by the counter layer provided with the resin, the board-shaped substrate, the printed paper layer provided with the resin and the paper layer provided with the resin forms a so-called cover layer. The stack is then pressed for less than 30 seconds at a temperature of about 180-210° C. and a pressure greater than 20 bar, for example 38 bar. During the pressing, the surface of the stack contacts a structured pressing element, such as a structured pressing board, and a relief portion is formed in the top layer of the obtained laminate. Possibly, the relief portion obtained can be formed in alignment with the printed pattern of the paper layer provided with the resin.

[0121] It is further clear that the paper or thermoplastic foil obtained in the first aspect of the present invention is suitable for use as decorative paper, decorative foil, respectively, in a process for producing floor, furniture panels, ceiling and / or wall panels.

[0122] It is clear that during the process of the invention, the above-mentioned printed pattern, board-shaped substrate, paper layer and thermoplastic layer may have to be separated to obtain their respective final dimensions. The board obtained by means of a DPL pressing process or a similar process is preferably sawn or otherwise separated. Other treatments of the obtained board are of course not excluded.

[0123] The base paper of the decorative paper produced by the process of the invention preferably has a base paper weight (ie without inkjet receiver coating) of more than 20 g / m2, wherein in the case of floor boards weights of between 55 and 95 g / m2 are achieved.

[0124] The base foil of the decorative foil or the base paper of the decorative paper produced by means of the method according to the invention preferably has a thickness of 0.05 mm or more, wherein a preferred thickness is between 0.05 and 0.5 mm. BRIEF DESCRIPTION OF THE DRAWINGS

[0125] In order to better illustrate the features according to the invention, one embodiment of an example of non-limiting features is described below with reference to the accompanying drawings, in which:

[0126] Figure 1 schematically illustrates one embodiment of a paper layer provided with an inkjet receiver coating according to a preferred embodiment of the method of the first aspect of the present invention;

[0127] Figure 2 and Figure 3 Provided in large proportion Figure 1 The view on the area F3 is shown in FIG. Figure 2 In the case of , only the first layer of the two-layer inkjet receiver coating has been applied to the paper layer;

[0128] Figure 4 Some steps of a method according to the third aspect of the present invention are shown;

[0129] Figure 5 shows in perspective Figure 4 The plate obtained by the method;

[0130] Figure 6 Shown according to Figure 5 A view of line VI-VI shown above;

[0131] Figure 7 A piece of apparatus for use in the other parts of the first aspect of the invention is shown;

[0132] Figure 8 schematically shows a top view of a printer operating in a single pass mode;

[0133] Fig. 9 Included is a graph of color density obtained with treated papers of the present invention compared to papers not pertaining to the present invention. DETAILED DESCRIPTION

[0134] Figure 1A processed paper layer 1 which can be printed with an inkjet printer is schematically shown. The printable paper layer 1 comprises a paper 2 provided with an inkjet receiver coating 3, the inkjet receiver coating 3 comprising a first layer 4 having a first composition and a second layer 5 having a second composition. In this case, the paper 2 is a base printing paper having a weight of about 70 grams per square meter and having an average air resistance expressed as a Gurley value of less than 30 seconds.

[0135] It is generally noted that, in order to better illustrate the invention, the dimensions of the sheets 2 and of the layers 4 - 5 shown in the figures are not drawn to scale.

[0136] Figure 2 and Figure 3 The inkjet receiver coating 3 is shown to include a pigment 6 and a binder 7. Both the composition of the first layer 4 and the composition of the second layer 5 include a binder. The inkjet receiver coating 3 (more specifically at least the second layer 5 thereof) further comprises an ink active compound, more specifically a flocculant, as in accordance with the first aspect of the invention. However, it is clear that the figures are also illustrative for many aspects of the invention in the case where an ink active compound other than a flocculant (more specifically an ink destabilizer, such as, for example, a cationic metal salt) has been applied.

[0137] Figure 2 A semi-finished product 8 is shown in which only the first layer 4 is applied to the paper 2. The binder 7 is partially and inhomogeneously absorbed into the paper 2. Loosely and / or poorly bound pigments 6 are present at the surface 9. Such pigments 6 cause dust release during further processing of the semi-finished product 8. The surface 9 of the obtained first layer 4 also suffers from unevenness.

[0138] Figure 3 A paper layer 1 is shown in which a second layer 5 is also applied on top of the first layer 4 . Figure 3 It is shown that the second layer 5 flattens the surface 9, resulting in a more uniform surface 10 of the second layer and the paper layer 1. In this case, the composition of the second layer 5 has a lower pigment to binder ratio than the composition of the first layer 4 and additionally comprises an ink-active compound. It is clear that it is not excluded that the first layer 4 may also comprise an ink-active compound that is the same as or different from the ink-active compound of the second layer 5, and that the ink-active compound may be in different concentrations.

[0139] It should be noted that Figure 3 is an embodiment of a paper layer wherein, at the surface of the treated paper layer, less than 10 weight percent of the total pigment 6 is unbound or free, and wherein the surface 10 of the second layer is substantially (and in this case entirely) formed by the binder 7.

[0140] Figure 4 Shown for manufacturing Figure 5 and Figure 6 Method for producing a laminate 11 of the type shown in FIG. The method forms an illustration of a third independent aspect of the invention as described in the introduction to the present patent application. The decorative board 11 obtained comprises at least a substrate 12 and a top layer 13. The top layer 13 comprises a paper layer 1 manufactured according to the first aspect and provided with a printed pattern or digital printed ink layer 14, such as in this case representing a wood pattern. The method of this exemplary embodiment comprises at least a step S1 of providing the paper layer 1 with an inkjet receiving layer and a printed pattern with a thermosetting resin 15. Therein, the paper layer 1 is taken from a roller 16 and conveyed to a first impregnation station 17, wherein the paper layer is immersed in a bath 18 of the resin 15 (more specifically, a mixture of water and resin 15). The paper layer 1 is then allowed to rest while being conveyed upwards in this case. The resting allows the resin 15 to penetrate the paper core. The paper layer 1 then enters a second impregnation station 19, wherein in this case the paper layer 1 is again immersed in a bath 18 of the resin 15 (more specifically, a mixture of water and resin 15). A set of extrusion rollers 20 allows applying an amount of resin 15 to the paper layer 1 .

[0141] In this embodiment, a plurality of doctor blades 21 may be employed for partially removing the resin at the surface of the paper layer 1 provided with the resin.

[0142] In a second step S2, the paper layer 1 provided with resin is dried to a residual moisture level below 10%. In this embodiment a drying oven 22 is used, but alternatively other heating means may be used, such as microwave or infrared drying means.

[0143] Figure 4 Also shown is the cutting of the continuous paper layer 2 into sheets 23 and stacking.

[0144] Figure 4 It is further shown that in the subsequent step S3, the obtained sheet 23 or paper layer 1 is made into a stack for pressing in a short multilayer press 24 between an upper pressing plate and a lower pressing plate 25-26. The stack comprises, from bottom to top, an opposing layer 27, a plate-shaped substrate 12, the above-mentioned paper layer 1 and a protective layer 28, wherein both the opposing layer 27 and the protective layer 28 comprise paper 2 and resin 15. The stack is then pressed, and the pressing process results in the mutual connection between the component layers 1-12-27-28 of the stack, including the substrate 12, and the hardening or curing of the existing resin 15. More specifically, a polycondensation reaction of the melamine formaldehyde resin 15 occurs here, with water as a by-product.

[0145] The upper pressed board 25 is a structured pressed board which provides a relief in the melamine surface of the board 1 by bringing the structured surface 29 of the upper pressed board 25 into contact with the melamine of the protective layer 28 during the same pressing process of step S3 .

[0146] Figure 5 and Figure 6 The resulting decorative board or laminate board 11, which can have a rectangular or oblong shape of laminate flooring, is shown, having a pair of long sides 30 and a pair of short sides 31, and having an HDF or MDF substrate 12. In this case, the board 11 has coupling means 32 at least at the long sides 30, which allow the corresponding edge 30 to be locked together with an edge of a similar board both in a direction R1 perpendicular to the plane of the coupling board (such as in a direction R2 perpendicular to the coupling side) and in the plane of the coupling board. Figure 6 As shown, such coupling means or coupling portion may substantially have the shape of a tongue 33 and a groove 34 provided with additional cooperating locking means 35 allowing said locking in direction R2 .

[0147] Figure 7 According to a preferred embodiment, at least one of the first layer 4 and the second layer 5 of the inkjet receiver coating 3 can be obtained by applying a liquid substance 36 to the paper 2 in one of the two partial steps. In this case, the application of the first layer is shown. The device 37 includes an applied counter-metering roller 38. The device 37 can initially apply an excess of liquid substance 36, which is squeezed out to the required weight by means of a roller 38 that can also be used to smooth the coating surface. Preferably, the semi-finished product 8 obtained is then dried, for example by means of a hot dryer, to preferably reach a residual moisture level of less than 10% (or about 7%). The obtained treated paper is then further treated by applying the second layer 5 of the inkjet receiver coating 3. This treatment is not shown here, but it can be carried out in a fairly similar manner. It is clear that other coating techniques (such as coating by one or more embossing rollers that can also run counter-clockwise) can be used as an alternative to the device 37.

[0148] Figure 8It is shown that a paper layer 1 having an inkjet receiver coating according to the first aspect of the invention can be printed by means of an inkjet printer 39, which in this embodiment comprises a plurality of rows 40 of print heads extending beyond the area of ​​the paper layer 1 to be printed. In this embodiment, the printer 39 relates to a single-pass printer, wherein the provision of a print pattern involves a relative movement of the inkjet printer 39 (more specifically the rows 40) and the paper layer 1 in a printing direction D during printing. In this case, during the ejection of ink onto the paper layer 1 (more precisely onto the inkjet receiver coating 3 applied to the paper), the rows 40 and the print heads are stationary and the paper layer 1 moves. The paper layer 1 is printed during a single continuous movement of the paper layer 1 relative to the printer 39 or the rows 40 of print heads. In this embodiment, the print pattern 14 obtained comprises a wood decorative pattern with wood veins 41 extending generally in the printing direction D. Preferably, a drying station 42 is arranged downstream of the printer 39. After drying the ink, the printed paper layer is preferably rolled up and rolled off. Figure 4 The method shown is used as roller 16.

[0149] The present invention, which does not have any limiting features, is further illustrated by the following, with reference to Fig. 9 Further exemplary embodiments are listed.

[0150] Example C:

[0151] 6 kg of commercially available amorphous silica (Syloid ED5) were dispersed in 41 kg of water and heated to a temperature of 80°C. 2.7 kg of silane (Dynasilan) as a particle surface modifier or coupling agent was added to the mixture and stirred for 30 minutes. Then 2.3 kg of 40% glyoxal (BASF) as a crosslinking agent was mixed and stirred for another 30 minutes. Then 0.5 kg of boric acid, also used as a crosslinking agent, was added and stirred for 10 minutes.

[0152] Separately, 2.5 kg of polyvinyl alcohol (Mowiol 20 / 98 Kuraray) were dissolved in 26.4 kg of water at 90° C. and kept stirring until complete dissolution (2 hours).

[0153] Next, the silica dispersion was added to the Mowiol solution and stirred thoroughly. To this mixture was added 0.04 kg of leveling agent, 0.04 kg of defoamer and 0.03 kg of fungicide and stirred for a further 5 minutes before the coating was bottled and cooled. The coating composition obtained did not contain any ink-active compounds or ink destabilizers. Specifically, the availability of boric acid was not in an amount capable of reducing the pH of the ink-receiving composition to pH 3 or below.

[0154] The pigment to binder ratio was 2.4 / 1 and the solids content was 13.5% by weight.

[0155] The coating was brought to the correct viscosity (30 seconds for 4 cups at 23°C) by adding water for application with an inverse patterned roller. Solids content was brought to 10% by weight.

[0156] 20g / m 2 The coating is applied with the aid of counter-rotating embossing rollers and dried.

[0157] Embodiment D:

[0158] 6 kg of commercially available amorphous silica (Syloid ED5) are dispersed in 41 kg of water and heated to a temperature of 80° C. 2.7 kg of silane (Dynasilan) as a particle surface modifier or coupling agent are added to the mixture and stirred for 30 minutes. 2.3 kg of 40% glyoxal (BASF) as a crosslinking agent are then mixed and stirred for a further 30 minutes. 0.5 kg of boric acid, also used as a crosslinking agent, is then added and stirred for 10 minutes. 5 kg of a 40% aqueous solution of polyDADMAC (polyquat 40U05 from Katpol) are then added and stirred for a further 10 minutes. PolyDADMAC is a polyionic polymer used as an ink destabilizer according to the invention.

[0159] Separately, 2.5 kg of Mowiol 20 / 98 (Kuraray) were dissolved in 26.4 kg of water at 90°C and kept stirring until complete dissolution (2 hours).

[0160] Next the silica dispersion was added to the Mowiol solution and stirred thoroughly. To this mixture was added 0.04 kg of levelling agent, 0.04 kg of defoamer and 0.03 kg of fungicide and stirred for a further 5 minutes before the paint was bottled and cooled.

[0161] The pigment to binder ratio was 2.4 / 1 and the solids content was 18.5% by weight.

[0162] The coating was brought to the correct viscosity (30 seconds for 4 cups at 23°C) by adding water for application with an inverted embossing roller. Solids content was brought to 15% by weight.

[0163] 20g / m 2 The coating is applied with the aid of counter-rotating embossing rollers and dried.

[0164] Embodiment E:

[0165] Two coating compositions were produced.

[0166] First coating composition:

[0167] 13.4 kg of commercially available amorphous silica (Syloid ED5) are dispersed in 41 kg of water and heated to a temperature of 80°C. 6 kg of silane (Dynasilan) are added to the mixture and stirred for 30 minutes. Then 5.2 kg of 40% glyoxal (BASF) are mixed and stirred for a further 30 minutes. Then 0.5 kg of boric acid is added and stirred for 10 minutes. After that, 5 kg of polyquat 40U05 (from Katpol) are added and stirred for a further 10 minutes.

[0168] Separately, 2.5 kg of Mowiol 20 / 98 (Kuraray) were dissolved in 26.4 kg of water at 90°C and kept stirring until complete dissolution (2 hours).

[0169] Next the silica dispersion was added to the Mowiol solution and stirred thoroughly. To this mixture was added 0.04 kg of levelling agent, 0.04 kg of defoamer and 0.03 kg of fungicide and stirred for a further 5 minutes before the paint was bottled and cooled.

[0170] The pigment to binder ratio was 5.5 / 1 and the solids content was 26% by weight.

[0171] Second coating composition:

[0172] 46 kg of the first coating composition were mixed with 54 kg of an 8% mixture of Mowiol 20 / 98 in water.

[0173] The second coating composition had a pigment to binder ratio of 0.95 / 1 and a solids content of 17% by weight.

[0174] Both coating compositions were brought to the correct viscosity (30 seconds for -4 cup at 23°C) by adding water for application by means of opposing embossing rollers. The solids content of the first coating composition was 20% by weight and the second coating composition had a solids content of 11% by weight.

[0175] The inkjet receiver coating was applied in two partial steps on a blank paper (Technocel MPK 3723), wherein respectively, 12 g / m 2 The first coating composition of 12 g / m 2 was applied as a first layer and then dried, and then, likewise by means of an opposing embossing roller, a 12 g / m 2 coating composition was applied as a first layer and then dried, and then, 2 A second coating composition of the present invention is applied thereon with a second layer and then dried.

[0176] Print proofing:

[0177] The pre-metered coating method was used to apply the ink to the treated papers of Example C to Example E, as well as to an untreated base paper (Technocel MPK 3723) designated as Paper A and a commercial inkjet quality paper designated as Paper B. The high absorption of the paper ruled out wire rod coating (Mayer bar coating). For this purpose, a K print proofer from RK Print Coating Instruments was used with a 100 lines / inch printing plate and a water-based red digital printing ink.

[0178] The print is then analyzed by a Byk Spectro guide to measure the L, a, and b values. The CD (color density) value is then calculated by multiplying a with b and dividing it by L. All papers A to E are then sorted based on the CD value, which is Fig. 9 The horizontal axis contains different test papers, where A is an untreated base paper, B is a commercial inkjet quality paper, and C to E correspond to the treated papers of Example C to Example E. The vertical axis gives the CD value obtained with the respective paper. A higher CD value means better optical density and means better image quality. This simplified color density (CD) value allows a quick evaluation and ranking of the coating.

[0179] from Fig. 9 It can be seen that the use of an ink destabilizer in the inkjet receiver coating has a significant effect on the color density achieved. Particularly high color densities are achieved in a preferred embodiment in which the inkjet receiver coating with different coating compositions is applied in two steps.

[0180] The invention is not in any way limited to the embodiments described above, but such a method, paper layer, thermoplastic foil and plastic thermosetting resin foil may be realized according to several variants without departing from the scope of the invention.

Claims

1. An inkjet receiver coating (3) for use in the production of paper printable with an inkjet printer, wherein the paper is used as decorative paper in a laminate, wherein the paper (1) is coated on at least one side with the inkjet receiver coating (3), the inkjet receiver coating comprising at least a pigment (6) and a binder (7), characterized in that The inkjet receiver coating (3) comprises an ink-active compound, wherein before coating the inkjet receiver coating (3), the paper (1) has a Gurley value of less than 30 seconds; after coating the inkjet receiver coating (3), the paper (1) has a Gurley value between 30 and 120 seconds; and after printing, the paper (1) is impregnated with a thermosetting resin.

2. The inkjet receiver coating (3) according to claim 1, characterized in that The ink active compound comprises a polyionic polymer.

3. The inkjet receiver coating (3) according to claim 1 or 2, characterized in that The ink active compound comprises a substance that changes the pH of the inkjet receiver coating (3).

4. The inkjet receiver coating (3) according to claim 3, characterized in that The substance is selected from the list consisting of formic acid, tartaric acid, acetic acid, hydrochloric acid, citric acid, phosphoric acid, sulfuric acid, AlCl3 and boric acid.

5. The inkjet receiver coating (3) according to claim 1 or 2, characterized in that The ink active compound comprises a metal salt.

6. The inkjet receiver coating (3) according to claim 5, characterized in that The metal salt is selected from the list consisting of CaCl2, MgCl2, CaBr, MgBr2, calcium magnesium acetate, calcium acetate, ZrCl4 and magnesium acetate.

7. The inkjet receiver coating (3) according to claim 1 or 2, characterized in that The ink active compound comprises a flocculant.

8. The inkjet receiver coating (3) according to claim 7, characterized in that The flocculant is selected from the list consisting of sodium aluminate, bisulfate, polyaluminium chloride, polyacrylate, dicyandiamide and polyacrylamide.

9. The inkjet receiver coating (3) according to claim 1 or 2, characterized in that The inkjet receiver coating (3) has a pigment to binder ratio between 0.01 / 1 and 25 / 1.

10. The inkjet receiver coating (3) according to claim 1 or 2, characterized in that The pigment (6) has a 2 Surface area of ​​pigment / m 2 The surface area of ​​the particles between the surfaces of the paper.

11. The inkjet receiver coating (3) according to claim 1 or 2, characterized in that The pigment (6) has an average particle size of 100 nm to 20 μm.

12. The inkjet receiver coating (3) according to claim 11, characterized in that The pigment (6) has a particle size between 1 μm and 12 μm.

13. The inkjet receiver coating (3) according to claim 1 or 2, characterized in that The pigment (6) is a porous inorganic pigment.

14. The inkjet receiver coating (3) according to claim 1 or 2, characterized in that The pigment (6) comprises precipitated silica, amorphous silica and / or fumed silica.

15. The inkjet receiver coating (3) according to claim 1 or 2, characterized in that The inkjet receiver coating (3) is applied in at least two-part steps, wherein separately, a first layer (4) is applied with a first composition and subsequently, a second layer (5) is applied with a second composition, both compositions comprising at least the binder (7).