Polymer films and communication substrates
By controlling the size and distribution of bright parts and island-shaped areas in the polymer film, the anisotropy problem of liquid crystal polymer film is solved, and more uniform mechanical and electrical characteristics are achieved, which is suitable for the substrate requirements of 5G communication systems.
Patent Information
- Application Number
- CN202180023197.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-27
- Filing Date
- 2021-03-15
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-03-15
AI Technical Summary
In 5G mobile communication system, the liquid crystal polymer film has anisotropy problems caused by its rod-like molecular structure, which leads to cracks and peeling of conductive layers during processing, making it difficult to meet the low dielectric constant and low dielectric loss tangent. Require.
A number of bright parts were observed on the surface of the polymer film. If the bright part with the largest circular equivalent diameter is less than 10 μm, and the circular equivalent diameter of the island-shaped region of the inorganic particle is observed under a scanning electron microscope is 0.001 to 10 μm. Specific material composition and process treatment adjust the anisotropy of the linear expansion coefficient of the polymer film.
The linear expansion coefficient anisotropy of the polymer film is achieved, the uniformity of mechanical and electrical characteristics is improved, cracking and peeling problems are reduced, and it is suitable for 5G communication substrates.
Smart Images

Figure CN115335437B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polymer film and a communication substrate. Background Art
[0002] In the fifth generation (5G) mobile communication system, which is called the next generation communication technology, higher frequencies and wider frequency bands are used than before. Therefore, as a substrate film for a circuit substrate used in a 5G mobile communication system, a substrate film with low dielectric constant and low dielectric loss tangent is required, and development based on various raw materials is being carried out.
[0003] As one of such substrate films, there is a polymer film containing liquid crystal polymer (LCP). In the 4th generation (4G) mobile communication system, the polymer film containing liquid crystal polymer has a lower dielectric constant and a lower dielectric loss tangent than conventional polyimide and glass epoxy films.
[0004] However, liquid crystal polymers have a rod-shaped molecular structure even in the molten state, so they are easy to orient. When liquid crystal polymers are melt-extruded from a T-die for processing, the liquid crystal polymers are subjected to shear stress in the die slit, and the rod-shaped liquid crystal molecules are oriented in the machine axis direction (MD direction), and are further oriented by melt stretching.
[0005] Therefore, the polymer film produced by melt extrusion becomes a uniaxially oriented film with liquid crystal molecules along the MD direction and has strong anisotropy. Due to this anisotropy, it has different mechanical properties, dimensional stability, and electrical properties in the MD direction and the width direction (TD direction: Transverse Direction, transverse direction), so when processed into a circuit board, cracks and peeling of the conductive layer occur.
[0006] As a method for improving the anisotropy of the polymer film as described above, Patent Document 1 discloses a method of obtaining a polymer film by inflation molding using a liquid crystal polymer.
[0007] Previous technical literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 5-43664 Summary of the invention
[0010] Technical issues to be solved by the invention
[0011] The present inventors referred to Patent Document 1 and found that the anisotropy of the linear expansion coefficient sometimes increases, and that there is room for improvement, as a result of producing a polymer film using a liquid crystal polymer.
[0012] Therefore, an object of the present invention is to provide a polymer film having a small anisotropy of linear expansion coefficient. Another object of the present invention is to provide a communication substrate having the polymer film.
[0013] Means for solving technical problems
[0014] As a result of intensive research conducted by the inventors to solve the above-mentioned problems, the inventors have completed the present invention by discovering the following: when observing the surface of a polymer film under an orthogonal Nicol environment through a polarizing microscope, multiple bright portions are observed in the observation area, and if the bright portion with the largest equivalent circular diameter is less than 10 μm, the desired effect is achieved.
[0015] That is, the present inventors have found that the above-mentioned problems can be solved by the following configuration. [1]
[0017] A polymer film comprising a liquid crystal polymer, wherein:
[0018] When the surface of the polymer film is observed under crossed Nicols using a polarizing microscope, a plurality of bright portions are observed in the observed area.
[0019] The bright portion having the largest equivalent circle diameter among the plurality of bright portions has an equivalent circle diameter of 10 μm or less. [2]
[0021] The polymer film according to [1], wherein the ratio of the total area of the bright portions to the area of the observation region in the polarization microscope is 60% or less. [3]
[0023] The polymer film according to [1] or [2], wherein the polymer film comprises a component selected from inorganic particles and a polymer different from the liquid crystal polymer.
[0024] When a cross section perpendicular to the surface of the polymer film was observed with a scanning electron microscope, a plurality of island-shaped regions composed of the above component were observed in the observed region, and the circle-equivalent diameter of the island-shaped regions was 0.001 to 10 μm. [4]
[0026] The polymer film according to [3], wherein a ratio of the total area of the island-shaped regions to the area of the observation region under the scanning microscope is 1 to 60%. [5]
[0028] The polymer film according to [3] or [4], wherein the material constituting the inorganic particles is at least one selected from the group consisting of silicon dioxide, titanium oxide, barium sulfate, talc, zirconium oxide, aluminum oxide, silicon nitride, silicon carbide, calcium carbonate, silicate, glass beads, graphite, tungsten carbide, carbon black, clay, mica, carbon fiber, glass fiber and metal powder,
[0029] The polymer is at least one selected from thermoplastic resins and elastomers. [6]
[0031] The polymer film according to any one of [3] to [5], wherein the distance between the island-shaped regions is 0.0001 to 5 μm. [7]
[0033] The polymer film according to any one of [1] to [6], wherein a ratio of the Young's modulus in a second direction in the plane of the polymer film orthogonal to the first direction to the Young's modulus in the first direction in the plane of the polymer film is 0.5 to 1.9. [8]
[0035] The polymer film as described in any one of [1] to [7], wherein the ratio of the dielectric loss tangent in a second direction in the plane of the polymer film orthogonal to the first direction relative to the dielectric loss tangent in the plane of the polymer film is 0.5 to 1.5. [9]
[0037] The polymer film according to any one of [1] to [8], wherein a ratio of a dielectric constant in a second direction in the plane of the polymer film orthogonal to the first direction to a dielectric constant in the plane of the polymer film is 0.5 to 1.5.
[10]
[0039] The polymer film according to any one of [1] to [9], wherein a ratio of a linear expansion coefficient in a second direction in the plane of the polymer film orthogonal to the first direction to a linear expansion coefficient in the plane of the polymer film is 0.5 to 1.8.
[11]
[0041] The polymer film according to any one of [1] to
[10] , wherein the surface of the polymer film has an arithmetic mean surface roughness Ra of 400 nm or less.
[12]
[0043] The polymer film according to any one of [1] to
[11] , wherein the thickness is 5 to 1100 μm.
[13]
[0045] A communication substrate comprising the polymer film according to any one of [1] to
[12] .
[0046] Effects of the Invention
[0047] According to the present invention, a polymer film having a small anisotropy of linear expansion coefficient can be provided. In addition, according to the present invention, a communication substrate having the polymer film can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is an example of an observed image obtained by observing the polymer film of the present invention under a crossed Nicols environment using a polarizing microscope. DETAILED DESCRIPTION
[0049] Hereinafter, the present invention will be described in detail.
[0050] Although the description of the constituent elements described below may be made based on typical embodiments of the present invention, the present invention is not limited to such embodiments.
[0051] Regarding the marking of groups (atomic groups) in this specification, unless it violates the main purpose of the present invention, the marking not marked with substitution and unsubstituted includes groups without substitution and groups with substitution. For example, "alkyl" includes not only alkyl groups without substitution (unsubstituted alkyl groups) but also alkyl groups with substitution (substituted alkyl groups). In addition, "organic group" in this specification refers to a group containing at least 1 carbon atom.
[0052] In this specification, (meth)acrylic resin means acrylic resin and methacrylic resin.
[0053] In the present specification, when the polymer film is in a long strip shape, the first direction refers to the width direction (short side direction, TD direction) of the polymer film, and the second direction refers to the longitudinal direction (MD direction) of the polymer film.
[0054] In this specification, each component can use one substance corresponding to each component alone, or can use two or more substances corresponding to each component simultaneously. Here, when two or more substances are used simultaneously for each component, unless otherwise specified, the content of the component refers to the total content of the substances used simultaneously.
[0055] In this specification, "to" is used to mean that the numerical values described before and after it are included as the lower limit and the upper limit.
[0056] [Polymer film]
[0057] The polymer film of the present invention contains a liquid crystal polymer. In the above-mentioned polymer film, when the surface of the above-mentioned polymer film is observed under an orthogonal Nicol environment through a polarizing microscope, multiple bright parts are observed in the observation area, and the circular equivalent diameter of the bright part with the largest circular equivalent diameter among the above-mentioned multiple bright parts (hereinafter also referred to as "the maximum circular equivalent diameter of the bright part") is less than 10 μm.
[0058] The polymer film of the present invention has a small anisotropy of linear expansion coefficient. The reason for this is not clear in detail, but is roughly estimated as follows.
[0059] It is speculated that the bright portion observed by polarizing microscope is a portion where the molecular chains of the liquid crystal polymer are oriented in the same direction and solidified. In other words, it is considered that when the size of the bright portion is small, the portion where the molecular chains of the liquid crystal polymer in the polymer film are oriented in the same direction is reduced. Therefore, it is speculated that the anisotropy of the linear expansion coefficient of the polymer film is reduced.
[0060] 〔Liquid crystal polymer〕
[0061] The polymer film of the present invention comprises a liquid crystal polymer, which is preferably a melt-formable liquid crystal polymer.
[0062] Examples of the liquid crystal polymer include thermotropic liquid crystal polymers. Thermotropic liquid crystal polymers are polymers that exhibit liquid crystallinity in a predetermined temperature range.
[0063] The chemical composition of the thermotropic liquid crystal polymer is not particularly limited as long as it is a melt-moldable liquid crystal polymer, and examples thereof include thermoplastic liquid crystal polyesters and thermoplastic polyester amides in which amide bonds are introduced into thermoplastic liquid crystal polyesters.
[0064] The liquid crystal polymer may use the thermoplastic liquid crystal polymer described in International Publication No. 2015 / 064437 and Japanese Patent Application Publication No. 2019-116586.
[0065] Preferred specific examples of liquid crystal polymers include thermoplastic liquid crystal polyesters or thermoplastic liquid crystal polyester amides having repeating units derived from at least one selected from aromatic hydroxycarboxylic acids, aromatic or aliphatic diols, aromatic or aliphatic dicarboxylic acids, aromatic diamines, aromatic hydroxylamines, and aromatic aminocarboxylic acids.
[0066] As aromatic hydroxycarboxylic acids, p-hydroxybenzoic acid, m-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid and 4-(4-hydroxyphenyl)benzoic acid can be mentioned. These compounds may have substituents such as halogen atoms, lower alkyl groups and phenyl groups. Among them, p-hydroxybenzoic acid or 6-hydroxy-2-naphthoic acid is preferred.
[0067] As the aromatic or aliphatic diol, an aromatic diol is preferred. As the aromatic diol, hydroquinone, 4,4'-dihydroxybiphenyl, 3,3'-dimethyl-1,1'-biphenyl-4,4'-diol and acylates thereof are mentioned, and hydroquinone or 4,4'-dihydroxybiphenyl is preferred.
[0068] As the aromatic or aliphatic dicarboxylic acid, an aromatic dicarboxylic acid is preferred. Examples of the aromatic dicarboxylic acid include terephthalic acid, isophthalic acid, and 2,6-naphthalenedicarboxylic acid, and terephthalic acid is preferred.
[0069] Examples of the aromatic diamine, aromatic hydroxyamine, and aromatic aminocarboxylic acid include p-phenylenediamine, 4-aminophenol, and 4-aminobenzoic acid.
[0070] The liquid crystal polymer preferably has at least one selected from the group consisting of a repeating unit derived from an aromatic hydroxycarboxylic acid, a repeating unit derived from an aromatic diol, and a repeating unit derived from an aromatic dicarboxylic acid.
[0071] Among them, the liquid crystal polymer more preferably has at least a repeating unit derived from an aromatic hydroxycarboxylic acid, further preferably has at least one selected from a repeating unit derived from p-hydroxybenzoic acid and a repeating unit derived from 6-hydroxy-2-naphthoic acid, and particularly preferably has a repeating unit derived from p-hydroxybenzoic acid and a repeating unit derived from 6-hydroxy-2-naphthoic acid.
[0072] Furthermore, as another preferred embodiment, the liquid crystal polymer more preferably has at least one unit selected from the group consisting of repeating units derived from 6-hydroxy-2-naphthoic acid, repeating units derived from aromatic diols, repeating units derived from terephthalic acid, and repeating units derived from 2,6-naphthalene dicarboxylic acid, and further preferably has all repeating units derived from 6-hydroxy-2-naphthoic acid, repeating units derived from aromatic diols, repeating units derived from terephthalic acid, and repeating units derived from 2,6-naphthalene dicarboxylic acid.
[0073] When the liquid crystal polymer contains repeating units derived from an aromatic hydroxycarboxylic acid, the component ratio thereof is preferably 50 to 65 mol % based on all repeating units of the liquid crystal polymer. Furthermore, the liquid crystal polymer preferably has only repeating units derived from an aromatic hydroxycarboxylic acid.
[0074] When the liquid crystal polymer contains repeating units derived from an aromatic diol, the component ratio thereof is preferably 17.5 to 25 mol % based on all the repeating units of the liquid crystal polymer.
[0075] When the liquid crystal polymer contains repeating units derived from an aromatic dicarboxylic acid, the component ratio thereof is preferably 11 to 23 mol % based on all the repeating units of the liquid crystal polymer.
[0076] When the liquid crystal polymer contains a repeating unit derived from any one of an aromatic diamine, an aromatic hydroxyamine, and an aromatic aminocarboxylic acid, the component ratio thereof is preferably 2 to 8 mol % based on all the repeating units of the liquid crystal polymer.
[0077] The method for synthesizing the liquid crystal polymer is not particularly limited, and the liquid crystal polymer can be synthesized by polymerizing the above-mentioned compound by a known method such as melt polymerization, solid phase polymerization, solution polymerization, and slurry polymerization.
[0078] As the liquid crystal polymer, a commercial product may be used. Examples of commercial products of the liquid crystal polymer include "Laperos" manufactured by Polyplastics Co., Ltd., "Vectra" manufactured by Celanese Corporation, "UENO LCP" manufactured by UENOFINE CHEMICALS INDUSTRY. Ltd., "Sumika Super LCP" manufactured by Sumitomo Chemical Co., Ltd., "Zider" manufactured by ENEOS Corporation, and "Siveras" manufactured by Toray Industries, Inc.
[0079] In addition, the liquid crystal polymer may form a chemical bond with a crosslinking agent or a compatible component (reactive compatibilizer) as an arbitrary component in the polymer film. This also applies to components other than the liquid crystal polymer.
[0080] The content of the liquid crystal polymer is preferably 40 to 100% by mass, more preferably 60 to 99% by mass, and particularly preferably 80 to 97% by mass, based on the total mass of the polymer film.
[0081] (The maximum circle equivalent diameter of the bright part)
[0082] In the polymer film of the present invention, the maximum circle-equivalent diameter of the bright portion is 10 μm or less, more preferably 4 μm or less, and particularly preferably 2 μm or less from the viewpoint of achieving more excellent effects of the present invention.
[0083] The lower limit of the maximum circle-equivalent diameter of the bright portion is not particularly limited, but is preferably 0.001 μm or more, more preferably 0.005 μm or more, and particularly preferably 0.01 μm or more.
[0084] Here, the maximum circle equivalent diameter of the bright portion is measured as follows.
[0085] First, a microtome is used to cut 20 different parts of the polymer film along a direction parallel to the main surface of the polymer film (i.e., a direction orthogonal to the thickness direction of the polymer film (in-plane direction)), and thin sheet samples of a specified thickness (e.g., 10 μm) are cut out to obtain 20 samples for observation.
[0086] Next, 20 observation images corresponding to the observation area are obtained by observing from the normal direction of the main surface of the observation sample under the orthogonal Nicol environment using a polarizing microscope. Here, the orthogonal Nicol environment refers to a state in which the angles formed by the polarization axes of the two polarizers holding the observation sample are orthogonal to each other. In addition, the magnification during observation is selected to be an appropriate magnification within the range of 10 to 1000 times.
[0087] Next, for each of the 20 observation images, the outer periphery of the bright portion is traced, and the diameter of a circle having the same area as the traced area (equivalent circle diameter) is measured by an image analysis device. Furthermore, the maximum value of the equivalent circle diameter of the bright portion obtained from the 20 observation images is defined as the maximum equivalent circle diameter of the bright portion.
[0088] Figure 1 This is an example of an observed image obtained by observing the polymer film of the present invention under a crossed Nicol environment using a polarizing microscope. Figure 1 As shown, in the observed image, a relatively bright bright portion and a relatively dark dark portion are observed.
[0089] As methods for setting the maximum circle equivalent diameter of the bright portion to within the above range, for example, there can be cited a method of adding inorganic particles of a specified size described later and at least one component of the polymer together with the liquid crystal polymer when manufacturing a polymer film, a method of adjusting the temperature, discharge amount and / or screw speed when melt-kneading particles formed using a liquid crystal polymer through an extruder, a method of adjusting the residence time of particles formed using a liquid crystal polymer until they are discharged from a die through an extruder, and a method combining these.
[0090] (Area ratio of bright part)
[0091] The ratio of the total area of the bright parts in the polarizing light microscope to the area of the observation area (hereinafter also referred to as the "area ratio of the bright parts") is preferably 60% or less, more preferably 55% or less, further preferably 50% or less, particularly preferably 40% or less, and most preferably 30% or less.
[0092] The lower limit of the area ratio of the bright portion is not particularly limited, but is preferably 1% or more, more preferably 2% or more, and particularly preferably 5% or more.
[0093] Here, the area ratio of the bright portion is calculated from an observed image obtained by the above-mentioned method for measuring the maximum circle equivalent diameter of the bright portion.
[0094] Specifically, for each of the 20 observation images obtained as described above, the total area of the circle equivalent diameter of the bright portion is calculated, and the ratio (%) of the total area of the circle equivalent diameter of the bright portion to the total area of the observation image (i.e., the observation area) is calculated. Furthermore, the arithmetic mean value of the 20 observation images is calculated and defined as the area ratio of the bright portion.
[0095] As a method for setting the area ratio of the bright portion within the above range, there can be mentioned the same method as the method for adjusting the maximum circle equivalent diameter of the bright portion.
[0096] [Component A (inorganic particles, polymer)]
[0097] The polymer film preferably contains a component selected from inorganic particles and a polymer different from the liquid crystal polymer (hereinafter also referred to as "component A"). This makes it easy to adjust the maximum circle-equivalent diameter of the bright portion within the above range.
[0098] Among them, from the viewpoint of being able to easily adjust the circle-equivalent diameter (described later) of the island-shaped regions, component A preferably contains a polymer.
[0099] From the viewpoint of more excellent effects of the present invention, the material constituting the inorganic particles is preferably at least one selected from the group consisting of silica, titanium oxide, barium sulfate, talc, zirconium oxide, aluminum oxide, silicon nitride, silicon carbide, calcium carbonate, silicate, glass beads, graphite, tungsten carbide, carbon black, clay, mica, carbon fiber, glass fiber, and metal powder, and is particularly preferably at least one selected from the group consisting of silica, titanium oxide, barium sulfate, talc, calcium carbonate, silicate, and clay.
[0100] From the viewpoint of easily adjusting the circle-equivalent diameter (described later) of the island-shaped regions to a desired range, the average primary particle size of the inorganic particles is preferably 5 to 10,000 nm, more preferably 10 to 1,000 nm, and particularly preferably 50 to 200 nm.
[0101] The particle size of the primary particles of inorganic particles is measured as follows: using a transmission electron microscope to shoot inorganic particles at a photographic magnification of 10,000 times, and printing on a photo paper in a particle photo obtained by a total magnification of 50,000 times, the outline of the particle (primary particle) is traced by a digital converter, and the diameter (circle area equivalent diameter) of a circle with the same area as the traced area is calculated. Here, primary particles refer to independent particles that are not aggregated. The shooting using a transmission electron microscope is set to the shooting performed by a direct method using a transmission electron microscope at an accelerating voltage of 300kV. The observation and measurement of a transmission electron microscope can be carried out, for example, using a transmission electron microscope H-9000 type manufactured by Hitachi and image analysis software KS-400 manufactured by Carl Zeiss.
[0102] Here, regarding the average primary particle size of various particles described in this specification, when commercially available products are used, the catalog value is adopted.
[0103] When there is no catalog value, the arithmetic mean of the values obtained for 500 particles randomly selected using the particle photographs taken as described above is used.
[0104] The polymer is preferably at least one selected from thermoplastic resins and elastomers.
[0105] Examples of thermoplastic resins include polyurethane resins, polyester resins, (meth) acrylic resins, polystyrene resins, fluororesins, polyimide resins, fluorinated polyimide resins, polyamide resins, polyamide-imide resins, polyetherimide resins, cellulose acylate resins, polyurethane resins, polyetheretherketone resins, polycarbonate resins, polyolefin resins (e.g., polyethylene resins, polypropylene resins, resins composed of cyclic olefin copolymers, alicyclic polyolefin resins), polyarylate resins, polyethersulfone resins, polysulfone resins, fluorene ring-modified polycarbonate resins, alicyclic modified polycarbonate resins, and fluorene ring-modified polyester resins. Among them, polyolefin resins are preferred from the viewpoint that they are general materials and that the circle equivalent diameter (described later) of the island region can be easily adjusted.
[0106] In this specification, an elastomer refers to a polymer compound that exhibits elastic deformation, that is, a polymer compound having the property of instantly deforming in response to an external force applied thereto and returning to its original shape in a short time when the external force is removed.
[0107] The elastomer is not particularly limited, and examples thereof include elastomers containing repeating units derived from styrene (polystyrene elastomers), polyester elastomers, polyolefin elastomers, polyurethane elastomers, polyamide elastomers, polyacrylic elastomers, silicone elastomers, polyimide elastomers, etc. Among them, polystyrene elastomers are preferred from the viewpoint that they are general-purpose materials and the circle equivalent diameter (described later) of the island region can be easily adjusted.
[0108] The elastomer is preferably a hydride, and is particularly preferably a hydride of a polystyrene elastomer. If the elastomer is a hydride, thermal stability and storage stability are improved. In addition, a hydride refers to a polymer having a structure in which the elastomer is hydrogenated.
[0109] As polystyrene elastomers, styrene-butadiene-styrene block copolymers (SBS), styrene-isoprene-styrene block copolymers (SIS), polystyrene-poly (ethylene-propylene) diblock copolymers (SEP), polystyrene-poly (ethylene-propylene)-polystyrene triblock copolymers (SEPS), polystyrene-poly (ethylene-butylene)-polystyrene triblock copolymers (SEBS) and polystyrene-poly (ethylene / ethylene-propylene)-polystyrene triblock copolymers (SEEPS) can be mentioned. Among them, SEBS is preferred from the viewpoint of more excellent effects of the present invention.
[0110] As the polymer, from the viewpoint of achieving more excellent effects of the present invention, a polyolefin resin is preferred, a linear or branched polyolefin resin is preferred, a polyethylene resin or a polypropylene resin is more preferred, and a polyethylene resin is particularly preferred.
[0111] From the viewpoint of further improving the effects of the present invention, the content of Component A is preferably 1 to 60% by mass, more preferably 2 to 20% by mass, and particularly preferably 5 to 15% by mass based on the total mass of the polymer film.
[0112] When the polymer film includes component A, when a cross section perpendicular to the surface of the polymer film is observed by a scanning electron microscope, a plurality of island-like regions composed of component A are observed in the observed region. In this case, the polymer film means a film having a sea-island structure in which component A is dispersed in a liquid crystal polymer, and the sea-island structure has a plurality of island-like regions composed of component A and a continuous region composed of a liquid crystal polymer.
[0113] (Circle equivalent diameter of island area)
[0114] From the perspective of easily adjusting the maximum circle equivalent diameter of the bright portion within the above range and / or being able to reduce the arithmetic mean surface roughness Ra of the surface of the polymer film, the circle equivalent diameter of the island region is preferably 0.001 to 10 μm, more preferably 0.005 to 5 μm, and particularly preferably 0.01 to 1 μm.
[0115] Here, the circle-equivalent diameter of the island-shaped region is measured as follows.
[0116] First, the polymer film is cut in such a manner that fracture cross sections parallel to a first direction in the plane of the polymer film and perpendicular to the surface of the polymer film are obtained at 10 different locations of the polymer film. Furthermore, the polymer film is cut in such a manner that fracture cross sections parallel to a second direction in the plane of the polymer film (a direction perpendicular to the first direction) and perpendicular to the surface of the polymer film are obtained at 10 different locations of the polymer film.
[0117] Next, a scanning electron microscope was used to observe the fractured cross sections of 20 locations in total (i.e., the total of 10 locations of the fractured cross sections parallel to the first direction and perpendicular to the surface of the polymer film and 10 locations of the fractured cross sections parallel to the second direction and perpendicular to the surface of the polymer film), and 20 observation images corresponding to the observation area were obtained. In addition, an appropriate magnification within the range of 100 to 100,000 times was selected during the observation, and the images were taken in a manner that the entire range in the thickness direction of the polymer film could be observed.
[0118] Next, for any 200 island-shaped areas in the 20 observation images, the periphery of the island-shaped area is traced, and the diameter of a circle having the same area as the traced area (equivalent circle diameter) is measured by an image analysis device. Furthermore, the arithmetic mean of the equivalent circle diameters of the 200 island-shaped areas is defined as the equivalent circle diameter of the island-shaped area.
[0119] Examples of methods for setting the circle-equivalent diameter of the island-shaped region to the above range include a method of using inorganic particles having a predetermined average primary particle diameter when component A is inorganic particles, a method of using a predetermined type of polymer when component A is a polymer, a method of adjusting the shear rate during granulation as described later, and a combination of these methods.
[0120] (Area ratio of island region)
[0121] The ratio of the total area of the island-shaped region to the area of the observation region in the scanning microscope (hereinafter, also referred to as "the area ratio of the island-shaped region") is preferably 1 to 60%, more preferably 1 to 50%, further preferably 2 to 20%, and particularly preferably 5 to 15%. If it is above the lower limit, the effect of the present invention is more excellent. And, if it is below the upper limit, the surface of the polymer film can be flat.
[0122] Here, the area ratio of the island-shaped regions is calculated based on the observed image obtained by the above-mentioned method of measuring the circle-equivalent diameter of the island-shaped regions.
[0123] Specifically, an arbitrary region (hereinafter also referred to as a "selected region") is selected from each of the 20 observed images obtained as described above. For example, a square region of 10 μm in length×10 μm in width can be cited as the selected region.
[0124] Next, the outer periphery of the island-shaped area existing in the selected area is traced, and the total area occupied by the island-shaped area is measured by an image analysis device, and the ratio (%) of the total area of the island-shaped area to the area of the selected area is calculated. Furthermore, the arithmetic mean value of the 20 observed images is obtained and defined as the area ratio of the island-shaped area.
[0125] As a method for setting the area ratio of the island-shaped regions within the above range, there is a method of adjusting the content of the component A relative to the content of the liquid crystal polymer when producing a polymer film.
[0126] (Distance between islands)
[0127] From the viewpoint of achieving more excellent effects of the present invention, the distance between the island-shaped regions is preferably 0.0001 to 5 μm, more preferably 0.001 to 1 μm, and particularly preferably 0.01 to 0.1 μm.
[0128] Here, the distance between the island-shaped regions is calculated based on the observed image obtained by the above-mentioned method of measuring the circle-equivalent diameter of the island-shaped regions.
[0129] Specifically, an arbitrary region (hereinafter also referred to as a "selected region") is selected from each of the 20 observed images obtained as described above. For example, a square region of 10 μm in length×10 μm in width can be cited as the selected region.
[0130] Next, the outer periphery of the island-shaped region existing in the selected area is traced, and the shortest distance between different island-shaped regions is measured by an image analysis device. Furthermore, the arithmetic mean value in 20 observed images is calculated and defined as the distance between the island-shaped regions.
[0131] Examples of a method for setting the distance between the island-shaped regions within the above range include the same method as the method for adjusting the circle-equivalent diameter of the island-shaped regions, the same method as the method for adjusting the area ratio of the island-shaped regions, and a combination of these methods.
[0132] [Other ingredients]
[0133] The polymer film of the present invention may contain components other than those mentioned above. Examples of such other components include a crosslinking component, a compatible component, a plasticizer, a stabilizer, a lubricant, and a colorant.
[0134] (Cross-linking component)
[0135] Examples of crosslinking components include compounds having reactive groups such as epoxy-containing ethylene copolymers (e.g., ethylene-glycidyl methacrylate copolymers, ethylene-vinyl acetate-glycidyl methacrylate copolymers, ethylene-methyl acrylate-glycidyl methacrylate copolymers, poly(ethylene-glycidyl methacrylate)-graft-poly(acrylonitrile-styrene)), bisphenol-type epoxy compounds, and carbodiimide compounds.
[0136] The content of the crosslinking component is preferably 0 to 50% by mass based on the total mass of the polymer film.
[0137] (compatible ingredients)
[0138] Examples of the compatible component include oxazoline-based compatibilizers (e.g., bisoxazoline-styrene-maleic anhydride copolymers, bisoxazoline-maleic anhydride-modified polyethylene, bisoxazoline-maleic anhydride-modified polypropylene), elastic-based compatibilizers (e.g., styrene-ethylene-butadiene copolymers, styrene-ethylene-butadiene-styrene copolymers, hydrogenated styrene-isopropylene-styrene copolymers, aromatic resins, petroleum resins), reactive compatibilizers (e.g., ethylene-glycidyl methacrylate copolymers, ethylene-maleic anhydride-ethyl acrylate copolymers, ethylene-glycidyl methacrylate-acrylonitrile-styrene, acid-modified polyethylene paraffins, COOH-modified polyethylene graft polymers, COOH-modified polypropylene graft polymers), and copolymer-based compatibilizers (e.g., polyethylene-polyamide graft copolymers, polypropylene-polyamide graft copolymers, methyl methacrylate-butadiene-styrene resins, acrylonitrile-butadiene rubbers, EVA-PVC-graft copolymers, vinyl acetate-ethylene copolymer resins, ethylene-α-olefin copolymers, propylene-α-olefin copolymers, and hydrogenated styrene-isopropylene-block copolymers).
[0139] In addition, as compatible components, ionomer resins such as ethylene-methacrylic acid copolymer ionomer, ethylene-acrylic acid copolymer ionomer, propylene-methacrylic acid copolymer ionomer, propylene-acrylic acid copolymer ionomer, butylene-acrylic acid copolymer ionomer, ethylene-vinyl sulfonic acid copolymer ionomer, styrene-methacrylic acid copolymer ionomer, sulfonated polystyrene ionomer, fluorine-based ionomer, telechelic polybutadiene acrylic acid ionomer, sulfonated ethylene-propylene-diene copolymer ionomer, hydrogenated polypentene ionomer, polypentene ionomer, poly(vinyl pyridinium salt) ionomer, poly(vinyl trimethylammonium salt) ionomer, poly(vinyl benzyl phosphonium salt) ionomer, styrene-butadiene acrylic acid copolymer ionomer, polyurethane ionomer, sulfonated styrene-2-acrylamide-2-methylpropane sulfate ionomer, acid-amine ionomer, aliphatic ionene or aromatic ionene can be used.
[0140] The content of the compatible component is preferably 0 to 50% by mass based on the total mass of the polymer film.
[0141] However, in the case where the compatible component corresponds to component A, the compatible component is classified as component A.
[0142] (Plasticizers, stabilizers, lubricants, organic particles)
[0143] Examples of the plasticizer include alkyl phthalyl alkyl glycolates, phosphoric acid esters, carboxylic acid esters, and polyols. The content of the plasticizer is preferably 0 to 20% by mass based on the total mass of the polymer film.
[0144] Examples of the stabilizer include phosphite stabilizers (e.g., tris(4-methoxy-3,5-diphenyl)phosphite, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite), phenol stabilizers (e.g., 2,6-di-tert-butyl-4-methylphenol, 2,2-methylenebis(4-ethyl-6-tert-butylphenol), 2,5-di-tert-butylhydroquinone, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], 4,4-thiobis-(6-tert-butyl-3-methylphenol), 1,1-bis(4-hydroxyphenyl)cyclohexane, octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propiolate), epoxy compounds, and thioether compounds. The content of the stabilizer is preferably 0 to 10% by mass.
[0145] Examples of the lubricant include fatty acid esters and metal soaps (eg, inorganic stearic acid salts). The content of the lubricant is preferably 0 to 5% by mass relative to the total mass of the polymer film.
[0146] Examples of the organic fine particles include organic fine particles of cross-linked acrylic acid and cross-linked styrene, etc. The content of the organic fine particles is preferably 0 to 50% by mass relative to the total mass of the polymer film.
[0147] 〔Physical properties of polymer films, etc.〕
[0148] The ratio of the Young's modulus in the second direction orthogonal to the first direction in the plane of the polymer film to the Young's modulus in the first direction in the plane of the polymer film is preferably 0.5 to 1.9, more preferably 0.5 to 1.5, further preferably 0.7 to 1.3, and particularly preferably 0.8 to 1.2.
[0149] The method for measuring the Young's modulus is described in the Examples section below.
[0150] The ratio of the dielectric loss tangent in the second direction orthogonal to the first direction in the plane of the polymer film to the dielectric loss tangent in the first direction in the plane of the polymer film is preferably 0.5 to 1.5, more preferably 0.7 to 1.3, and particularly preferably 0.8 to 1.2.
[0151] The method for measuring the dielectric loss tangent is described in the Examples section below.
[0152] The ratio of the dielectric constant in the second direction orthogonal to the first direction in the plane of the polymer film to the dielectric constant in the first direction in the plane of the polymer film is preferably 0.5 to 1.5, more preferably 0.8 to 1.2, and particularly preferably 0.9 to 1.1.
[0153] The method for measuring the dielectric constant is described in the Examples section below.
[0154] The arithmetic mean surface roughness Ra of the surface of the polymer film is preferably 400 nm or less, more preferably 300 nm or less, and particularly preferably 200 nm or less.
[0155] The lower limit of the arithmetic mean surface roughness Ra of the surface of the polymer film is not particularly limited, but is usually 10 nm or more.
[0156] The method for measuring the arithmetic mean roughness Ra is described in the Examples section below.
[0157] The thickness of the polymer film is preferably 5 to 1100 μm, more preferably 5 to 1000 μm, further preferably 5 to 250 μm, and particularly preferably 5 to 150 μm.
[0158] The method for measuring the thickness of the polymer film is described in the Examples section below.
[0159] [Method for producing polymer film]
[0160] The method for producing the polymer film of the present invention is not particularly limited, and for example, preferably includes a granulation step of obtaining granules by kneading the above-mentioned components and a film-forming step of obtaining a polymer film using the above-mentioned granules. Hereinafter, the polymer film of the present invention is sometimes referred to as a "film". Each step is described below.
[0161] 〔Granulation process〕
[0162] (Granulation)
[0163] (1) Raw material form
[0164] The liquid crystal polymer used for thin film formation can also be used as is in the form of particles, flakes or powders, but for the purpose of stabilizing the film formation and uniformly dispersing additives (referring to components other than the liquid crystal polymer. The same applies hereinafter). It is preferred to use an extruder to mix and granulate one or more raw materials (referring to the liquid crystal polymer and at least one of the additives. The same applies hereinafter.) for use.
[0165] (2) Drying or ventilation instead of drying
[0166] When granulating, it is preferred to dry the liquid crystal polymer and additives in advance. As a drying method, it is possible to circulate heated air with a low dew point and dehumidify by vacuum drying. In particular, in the case of easily oxidizable resins, vacuum drying or drying using an inert gas is preferred.
[0167] Furthermore, drying can also be replaced by using a vent type extruder. The vent type extruder has a single shaft and a double shaft type, and either type can be used, and the double shaft type is more effective and preferred. Granulation is performed in the extruder through the vent and at a pressure of less than 1 atmosphere, more preferably 0 to 0.8 atmospheres, and even more preferably 0 to 0.6 atmospheres. This decompression can be achieved by exhausting air from the vent or hopper provided in the kneading section of the extruder using a vacuum pump.
[0168] (3) Raw material supply method
[0169] The raw material supply method may be a method of supplying raw materials by mixing them in advance before kneading and granulation, a method of supplying raw materials separately so as to have a certain ratio in the extruder, or a method combining the two.
[0170] (4) Type of extruder
[0171] Granulation can be made by using a mixer to melt and evenly disperse the liquid crystal polymer and / or additives, and then cooling and solidifying them and then cutting them. As for the extruder, as long as sufficient melt-kneading effect can be obtained, a known single-screw extruder, a non-intermeshing counter-rotating twin-screw extruder, an intermeshing counter-rotating twin-screw extruder, an intermeshing co-rotating twin-screw extruder, etc. can be used.
[0172] (5) Atmosphere during extrusion
[0173] During melt extrusion, it is preferred to prevent thermal and oxidative degradation as much as possible within a range that does not affect uniform dispersion, and it is also effective to reduce the pressure using a vacuum pump or to flow an inert gas to reduce the oxygen concentration. These methods may be implemented alone or in combination.
[0174] (6) Speed
[0175] The rotation speed of the extruder is preferably 10 to 1000 rpm, more preferably 20 to 700 rpm, and particularly preferably 30 to 500 rpm. Since the residence time can be shortened if the rotation speed is set to be above the lower limit, the molecular weight reduction caused by thermal degradation or the coloring of the resin caused by thermal degradation can be suppressed from becoming significant. In addition, since the molecular chain cutting caused by shearing can be suppressed if the rotation speed is set to be below the upper limit, the molecular weight reduction and the increase in the production of cross-linked gel can be suppressed. Regarding the rotation speed, it is preferred to select appropriate conditions from the two aspects of uniform dispersibility and thermal degradation caused by prolonged residence time.
[0176] (7) Temperature
[0177] The mixing temperature is preferably set to below the thermal decomposition temperature of the resin and the additive, and is preferably set to a low temperature as much as possible within the range where the load of the extruder and the decrease in uniform mixing properties are not a problem. Wherein, if the temperature is set too low, the melt viscosity rises, on the contrary, the shear stress during mixing rises and sometimes causes molecular chain severance, so it is necessary to select an appropriate range. In addition, in order to take into account the improvement of dispersibility and thermal degradation, melt mixing is performed at a higher temperature in the first half of the extruder, and the condition of reducing the resin temperature in the second half stage is also effective.
[0178] (8) Pressure
[0179] The mixing resin pressure during granulation is preferably carried out at 0.05 to 30 MPa. In the case of a resin that is easily colored and gelled by shearing, it is preferred to apply an internal pressure of about 1 to 10 MPa in the extruder so that the resin raw material is filled into the twin-shaft extruder. As a result, since mixing can be more effectively carried out under low shear, uniform dispersion is promoted while suppressing thermal decomposition. This pressure adjustment can be carried out by adjusting Q / N (the discharge amount per screw rotation) and setting a pressure regulating valve at the outlet of the twin-shaft mixing extruder.
[0180] (9) Shear and screw types
[0181] In order to evenly disperse the various raw materials, it is preferred to apply shearing, but excessive shearing may cause molecular chain severance or gel formation. Therefore, it is preferred to appropriately select the number or gap of the rotor segments and kneading disks disposed on the screw. Generally, since the gap between the rotor segments is large, there is a tendency to have lower shearing than the kneading disk type.
[0182] The shear rate in the extruder (shear rate during granulation) is preferably 60 to 1000 sec. -1 , more preferably 100 to 800 seconds -1 , especially preferably 200 to 500 seconds -1 If the shear rate is above the lower limit, poor melting of the raw materials and poor dispersion of the additives can be suppressed. If the shear rate is below the upper limit, the severance of the molecular chain can be suppressed, and the decrease in molecular weight and the increase in the generation of cross-linked gel can be suppressed. In addition, if the shear rate during granulation is within the above range, it becomes easy to adjust the circle equivalent diameter of the above island region to the above range.
[0183] (10) Residence time
[0184] The residence time in the mixer can be calculated from the volume of the resin retention portion in the mixer and the discharge capacity of the polymer. The extrusion residence time during granulation is preferably 10 seconds to 30 minutes, more preferably 15 seconds to 10 minutes, and particularly preferably 30 seconds to 3 minutes. As long as sufficient melting conditions can be ensured, resin degradation and discoloration of the resin can be suppressed, so a shorter residence time is preferred.
[0185] (11) Pelletization method
[0186] The granulation method is generally a method of solidifying a noodle-shaped extruded material in water and then cutting it. However, granulation can also be performed by an underwater cutting method in which the material is melted by an extruder and then cut while being extruded directly in water through a die or by a hot cutting method in which the material is cut in a hot state.
[0187] (12) Particle size
[0188] The particle size is preferably 1 to 300 mm 2 , length is 1 to 30 mm, and cross-sectional area is preferably 2 to 100 mm 2 , length is 1.5~10mm.
[0189] (13) Other granulation methods 1 (solution method)
[0190] As a common pelletizing method, the above-mentioned melt kneading method using an extruder is generally used. However, a method of uniformly preparing a dispersed solution using a common solvent for the liquid crystal polymer and the additive and then removing the solvent may also be used.
[0191] Examples of such a solvent include methanol, ethanol, acetone, methyl ethyl ketone, diethyl ether, ethyl acetate, butyl acetate, and dichloromethane.
[0192] From the viewpoint of efficiency and dispersibility, the concentration after dissolution is preferably 1 to 50% by mass, more preferably 3 to 35% by mass, and particularly preferably 5 to 30% by mass.
[0193] The solidification may be achieved by drying the solvent after dissolution (drying method), or by placing the solid in a poor solvent after dissolution to precipitate the solid (precipitation method).
[0194] (dry)
[0195] (1) Purpose of drying
[0196] Before melt film formation, it is preferred to reduce the moisture and volatile components in the particles, and it is effective to dry the particles. When the particles contain moisture and volatile components, sometimes not only bubbles are mixed into the film-forming film or the appearance is deteriorated due to the decrease in haze, but also the physical properties are deteriorated due to the severance of the molecular chain of the liquid crystal polymer or the roll contamination is caused by the generation of monomers or oligomers. In addition, depending on the type of liquid crystal polymer used, the generation of oxidative crosslinking bodies during melt film formation can be suppressed by removing dissolved oxygen through drying.
[0197] (2) Drying method and heating method
[0198] Regarding the drying method, a dehumidified hot air dryer is generally used from the viewpoint of drying efficiency and economy, but there is no particular limitation as long as the target moisture content can be obtained. Furthermore, there is no problem in selecting a more appropriate method according to the characteristics of the physical properties of the liquid crystal polymer.
[0199] Examples of the heating method include pressurized steam, heater heating, far infrared ray irradiation, microwave heating, and heat medium circulation heating.
[0200] In order to use energy more efficiently and to perform uniform drying by reducing temperature unevenness, it is preferable to make the drying equipment a heat-insulating structure.
[0201] In order to improve the drying efficiency, stirring may be performed, but sometimes particle powder may be generated, so it is sufficient to distinguish and use them appropriately. In addition, the drying method is not limited to one, and multiple drying methods can be combined to effectively perform the drying.
[0202] (3) Device form
[0203] There are two types of drying methods: continuous and batch. Among the drying methods using vacuum, the batch method is preferred. On the other hand, the continuous method has the advantage of excellent uniformity in a stable state, and it is necessary to distinguish and use it according to the application.
[0204] (4) Atmosphere and air volume
[0205] The dry atmosphere can be made by blowing or reducing the pressure of low dew point air or low dew point inert gas. The dew point of the air is preferably 0 to -60°C, more preferably -10 to -55°C, and particularly preferably -20 to -50°C. From the viewpoint of reducing the volatile components in the particles, it is preferably a low dew point atmosphere, but it is disadvantageous from the viewpoint of economic efficiency, and an appropriate range can be selected. In the case where the raw material is lost by oxygen, it is also effective to use an inert gas to reduce the oxygen partial pressure.
[0206] The required air volume per ton of liquid crystal polymer is preferably 20 to 2000 m 3 / hour, more preferably 50 to 1000 m 3 / hour, particularly preferably 100 to 500 m 3 / hour. If the drying air volume is above the lower limit, the drying efficiency is improved. When the drying air volume is below the upper limit, it is economically preferred.
[0207] (5) Temperature and time
[0208] As for the drying temperature, when the raw material is in a non-crystalline state, it is preferably {glass transition temperature (Tg) (℃) -1℃} to {Tg (℃) -100℃} (that is, a temperature 1℃ to 100℃ lower than Tg), more preferably {Tg (℃) -5℃} to {Tg (℃) -60℃}, and particularly preferably {Tg (℃) -10} to {Tg (℃) -40℃}.
[0209] If the drying temperature is below the upper limit, agglomeration due to softening of the resin can be suppressed, so that the conveyability is excellent. On the other hand, if the drying temperature is above the lower limit, the drying efficiency can be improved and the moisture content can be set to a desired value.
[0210] In addition, in the case of a crystalline resin, if {melting point (Tm) (°C) -30°C} or less, the resin can be dried in an unmelted state. If the temperature is set too high, it may cause coloration and changes in molecular weight (usually decrease, but increase depending on the situation). In addition, if the temperature is too low, it is necessary to select appropriate conditions because the drying efficiency is low. As an indicator, {Tm (°C) -150°C} to {Tm (°C) -50}°C is preferred.
[0211] The drying time is preferably more than 15 minutes, more preferably more than 1 hour, and especially preferably more than 2 hours. In addition, even if the drying exceeds 50 hours, the effect of further reducing the water content is also small, because the thermal degradation of the resin is considered, and therefore the drying time does not need to be set too long.
[0212] (6) Moisture content
[0213] The moisture content of the particles is preferably 1.0% by mass or less, more preferably 0.1% by mass or less, and particularly preferably 0.01% by mass or less.
[0214] (7) Transportation method
[0215] In order to prevent moisture from being reabsorbed into the dried pellets, it is preferred to use dry air or nitrogen to transport the pellets. In addition, for extrusion stabilization, it is also effective to supply high-temperature pellets at a certain temperature to the extruder. In order to maintain the heated state, heated dry air is usually used.
[0216] 〔Film forming process〕
[0217] (Manufacturing equipment)
[0218] Hereinafter, an example of each device constituting the production apparatus will be described.
[0219] (Extruder, screw, barrel)
[0220] (1) Extruder structure
[0221] Liquid crystal polymer raw materials (particles) are supplied to the cylinder via the supply port of the extruder. In the cylinder, from the supply port side, it is composed of a supply section for quantitatively transferring the supplied liquid crystal polymer, a compression section for melt-kneading and compressing the liquid crystal polymer, and a measuring section for measuring the melt-kneaded and compressed liquid crystal polymer. The outer periphery of the cylinder is provided with a heating and cooling device divided into multiple parts, so that each area in the cylinder can be controlled at a desired temperature. Usually, a belt heater or a sheathed aluminum casting heater is used to heat the cylinder, but a heat medium circulation heating method can also be used. In addition, cooling is usually air cooling by a blower, but there is also a method of flowing water or oil through a pipe wrapped around the outer periphery of the cylinder.
[0222] Furthermore, in order to prevent the pellets from being heated and fused and to prevent heat conduction for protecting the screw drive device, it is preferable to cool the supply port.
[0223] The inner wall surface of the cylinder needs to be made of a material that is excellent in heat resistance, wear resistance, and corrosion resistance, and that can ensure friction with the resin. Nitrided steel with the inner surface nitrided is usually used, but chrome-molybdenum steel, nickel-chrome-molybdenum steel, and stainless steel can also be nitrided and used.
[0224] In particular, in applications requiring wear resistance and corrosion resistance, it is effective to use a bimetallic cylinder obtained by lining the inner wall surface of the cylinder with a corrosion-resistant and wear-resistant raw material alloy such as nickel, cobalt, chromium and tungsten by centrifugal casting, and to form a ceramic sprayed film.
[0225] Furthermore, the cylinder generally has a smooth inner surface, but the inner wall of the cylinder may have axial grooves (square grooves, semicircular grooves, spiral grooves, etc.) for the purpose of increasing the extrusion volume. However, since the grooves in the cylinder may cause the polymer to be retained in the extruder, care should be taken when using it in applications with strict foreign matter levels.
[0226] (2) Type of extruder
[0227] The commonly used extruder generally has a single shaft (single screw) and a double shaft, and the single shaft extruder is widely used. The double shaft (multi-shaft) screw is generally divided into a meshing type and a non-meshing type, and the rotation direction is also divided into the same direction and the opposite direction. Since the meshing type has a greater mixing effect than the non-meshing type, there are many examples of its use. In addition, the mixing effect of the counter-rotating screw is higher than that of the same-direction rotating type, but since the same-direction rotating type has a self-cleaning effect, it is effective for stopping and being trapped in the extruder. In addition, it also has parallel and oblique intersections in the axial direction, and also has a conical shape used when strong shear is given. In a double shaft extruder, since the raw materials (granules, powders, flakes) in an undried state and the corners of the film produced in the middle of the film formation can be used as they are by properly configuring the vent, it is widely used, but in the case of a single shaft extruder, the volatile components can also be removed by properly configuring the vent. It is important to select an extruder used for film formation based on the required extrusion performance (extrusion stability, kneading properties, retention prevention, thermal history) and the characteristics of the extruder.
[0228] Extruders are usually used singly, and twin-spindle (multi-spindle) extruders are usually used, but are also usually used in combination by utilizing their respective characteristics. For example, in the film formation of PET (polyester) resin, a combination of a twin-spindle extruder that can use undried raw materials and a single-spindle extruder with good measuring properties is widely used.
[0229] (3) Screw type and structure
[0230] Among them, an example of a screw for a uniaxial extruder is shown. As the shape of the screw commonly used, a full-length screw with one helical thread of equal pitch is often used, but a double-thread screw that can stabilize the extrudability by using two threads to separate the solid and liquid phases of the resin in the melting process is also often used. In addition, in order to improve the mixing performance in the extruder, mixing elements such as Maddock, Dulmadge and barrier are usually combined. In addition, in order to improve the mixing effect, a screw with a multi-square cross-section and a screw with a distribution hole that gives the screw a distribution function in order to reduce the temperature unevenness in the extruder are also used.
[0231] As the raw material used in the screw, it is necessary to use a raw material that is excellent in heat resistance, wear resistance, and corrosion resistance and can ensure friction with the resin, just like the cylinder. Common examples include nitrided steel, chrome-molybdenum steel, nickel-chrome-molybdenum steel, and stainless steel. The screw can usually be made by grinding the above steel and performing nitriding treatment and / or HCr plating treatment, but sometimes special surface processing such as TiN, CrN, or Ti coating based on PVD (Physical Vapor Deposition) or CVD (Chemical Vapor Deposition) is also performed on the screw surface.
[0232] Diameter, groove depth
[0233] The preferred screw diameter varies depending on the target extrusion amount per unit time, but the screw diameter is preferably 10 to 300 mm, more preferably 20 to 250 mm, and particularly preferably 30 to 150 mm. The groove depth of the screw feed portion is preferably 0.05 to 0.20 times the screw diameter, more preferably 0.07 to 0.18 times, and particularly preferably 0.08 to 0.17 times. The pitch is generally set to the same value as the screw diameter, but a shorter pitch is used to improve the uniformity of melting, or conversely, a longer pitch is used to increase the extrusion amount. In addition, the width of the thread groove is preferably 0.05 to 0.25 of the thread pitch, and from the perspective of reducing friction between the screw and the barrel and the retention portion, a width of about 0.1 is generally used. The clearance between the flight and the barrel is also 0.001 to 0.005 times the screw diameter, but is preferably 0.0015 to 0.004 times from the viewpoint of reducing friction between the barrels and stagnation.
[0234] Compression rate
[0235] Furthermore, the screw compression ratio of the extruder is preferably 1.6 to 4.5. The screw compression ratio is expressed by the volume ratio of the supply section and the measuring section, that is, (the volume per unit length of the supply section) ÷ (the volume per unit length of the measuring section), and is calculated using the outer diameter of the screw shaft of the supply section, the outer diameter of the screw shaft of the measuring section, the groove diameter of the supply section, and the groove diameter of the measuring section. If the screw compression ratio is 1.6 or more, sufficient melt kneading properties can be obtained, the generation of undissolved parts can be suppressed, undissolved foreign matter becomes less likely to remain in the thermoplastic film after manufacture, and the mixing of bubbles can be suppressed by the degassing effect. On the contrary, if the screw compression ratio is 4.5 or less, excessive application of shear stress can be suppressed. Specifically, the decrease in the mechanical strength of the film caused by molecular chain severance, the overheating coloring development caused by shear heat generation, and the decrease in the level of foreign matter caused by gel generation can be suppressed. Therefore, the appropriate screw compression ratio is preferably 1.6 to 4.5, more preferably 1.7 to 4.2, and particularly preferably 1.8 to 4.0.
[0236] ·L / D
[0237] L / D refers to the ratio of the cylinder length to the cylinder inner diameter. If L / D is 20 or more, melting and kneading are insufficient, and the generation of undissolved foreign matter in the thermoplastic film after manufacture can be suppressed, as in the case where the compression ratio is appropriate. In addition, if L / D is 70 or less, the residence time of the liquid crystal polymer in the extruder becomes shorter, so the degradation of the resin can be suppressed. In addition, if the residence time can be shortened, the decrease in the mechanical strength of the thermoplastic film caused by the decrease in molecular weight caused by the severance of the molecular chain can be suppressed. Therefore, L / D is preferably in the range of 20 to 70, more preferably 22 to 65, and particularly preferably 24 to 50.
[0238] Screw ratio
[0239] The length of the extruder supply section is preferably set to 20 to 60% of the effective length of the screw (the total length of the supply section, the compression section and the measuring section), and more preferably 30 to 50%. The length of the extruder compression section is preferably set to 5 to 50% of the effective length of the screw, preferably 5 to 40% in the case of crystalline resins, and preferably 10 to 50% in the case of amorphous resins. The measuring section is preferably set to 20 to 60% of the effective length of the screw, and more preferably 30 to 50%. The measuring section is usually divided into multiple parts, and a mixing element is arranged between them to improve the mixing performance.
[0240] Q / N
[0241] The extruder output (Q / N) is preferably the theoretical maximum output (Q / N). MAX 50 to 99% of the discharge volume, more preferably 60 to 95%, and particularly preferably 70 to 90%. 3 / min], N represents the screw speed [rpm], (Q / N) represents the discharge volume per screw rotation. If the discharge volume (Q / N) is the theoretical maximum discharge volume (Q / N) MAX When the back pressure is less than 99%, the kneading property is improved due to sufficient back pressure, and not only the melting homogenization is improved, but also the stability of the extrusion pressure is improved.
[0242] The screw size is preferably selected as the optimal screw size in consideration of the crystallinity, melt viscoelastic properties and thermal stability of the resin, extrusion stability and uniformity of melt plasticization.
[0243] (4) Extrusion conditions
[0244] Raw material drying
[0245] In the melt-plasticizing step of the pellets by the extruder, it is also preferred to reduce the water content and volatile components as in the granulation step, and it is effective to dry the pellets.
[0246] ·Raw material supply method
[0247] When there are multiple raw materials (particles) fed from the supply port of the extruder, they can be pre-mixed (pre-mixing method), or they can be fed separately so that they become a certain ratio in the extruder, or a method combining the two can be used. In addition, in order to stabilize the extrusion, the temperature and volume specific gravity of the raw materials fed from the supply port are usually reduced. In addition, from the viewpoint of plasticization efficiency, as long as it is within the range of not agglomerating to the supply port by adhesion, the raw material temperature is preferably high temperature, and in the case of amorphous state, it is preferably in the range of {glass transition temperature (Tg) (℃) -150℃} to {Tg (℃) -1℃}, and in the case of crystalline resin, it is preferably in the range of {melting point (Tm) (℃) -150℃} to {Tm (℃) -1℃}, and the raw material is heated and kept warm. In addition, from the viewpoint of plasticization efficiency, the volume specific gravity of the raw material is preferably 0.3 times or more of that in the molten state, and particularly preferably 0.4 times or more. When the bulk specific gravity of the raw material is less than 0.3 times the specific gravity in the molten state, a processing such as simulating granulation by compressing the raw material is performed.
[0248] Atmosphere during extrusion
[0249] The atmosphere during melt extrusion is the same as the granulation process. It is necessary to prevent heat and oxidative degradation as much as possible within the range that does not hinder uniform dispersion. It is also effective to reduce the oxygen concentration in the extruder by injecting inert gas (nitrogen, etc.) and using a vacuum hopper and to provide a vent on the extruder to perform decompression based on a vacuum pump. These decompression and injection of inert gas can be implemented independently or in combination.
[0250] Speed
[0251] The rotation speed of the extruder is preferably 5 to 300 rpm, preferably 10 to 200 rpm, and particularly preferably 15 to 100 rpm. If the rotation speed is above the lower limit, the residence time becomes shorter, the decrease in molecular weight caused by thermal degradation can be suppressed, and discoloration can be suppressed. If the rotation speed is below the upper limit, the severance of molecular chains caused by shearing can be suppressed, and the decrease in molecular weight and the increase in cross-linked gel can be suppressed. From the two aspects of uniform dispersibility and thermal degradation caused by the extension of the residence time, the rotation speed is preferably selected as an appropriate condition.
[0252] ·temperature
[0253] The barrel temperature (supply section temperature T1°C, compression section temperature T2°C, measurement section temperature T3°C) is usually determined by the following method. When the pellets are melted and plasticized at the target temperature T°C through the extruder, the measurement section temperature T3 is set to T±20°C in consideration of the shear calorific value. At this time, T2 is set in consideration of the extrusion stability and the thermal decomposition of the resin within the range of T3±20°C. T1 is usually set to {T2(°C)-5°C}~{T2(°C)-150°C}, and the optimal value is selected from the perspective of ensuring the friction between the resin and the barrel, which is the driving force (feeding force) for conveying the resin, and preheating in the feed section. In the case of a normal extruder, the temperature can be set by subdividing each region T1~T3, and by setting the temperature change between each region to be smooth, it can be made more stable. At this time, T is preferably set below the thermal degradation temperature of the resin. When the thermal degradation temperature is exceeded by the shear heat generated by the extruder, the shear heat is usually actively cooled to remove the shear heat. Furthermore, in order to achieve both improvement in dispersibility and thermal degradation, it is also effective to perform melt mixing at a relatively high temperature in the first half of the extruder and to lower the resin temperature in the second half.
[0254] Temperature regulation of the screw
[0255] In order to stabilize extrusion, the temperature of the screw is also controlled. As a temperature control method, water or a medium is usually passed through the inside of the screw, and a heater is built into the inside of the screw to heat it. The temperature control range is usually carried out in the supply part of the screw, and sometimes in the compression part and the measurement part, and different temperatures are controlled in each area.
[0256] ·pressure
[0257] The resin pressure in the extruder is usually 1 to 50 MPa, preferably 2 to 30 MPa, and particularly preferably 3 to 20 MPa from the viewpoint of extrusion stability and melt uniformity. If the pressure in the extruder is 1 MPa or more, the melt filling rate in the extruder is insufficient, so the generation of foreign matter caused by the instability of the extrusion pressure and the generation of the stagnation portion can be suppressed. In addition, if the pressure in the extruder is 50 MPa or less, the shear stress received in the extruder can be suppressed from being too much, so the thermal decomposition caused by the increase in the resin temperature can be suppressed.
[0258] ·Residence time
[0259] The residence time in the extruder (residence time during film formation) can be calculated from the volume of the extruder part and the discharge capacity of the polymer, similarly to the granulation process. The residence time is preferably 10 seconds to 30 minutes, more preferably 15 seconds to 15 minutes, and particularly preferably 30 seconds to 10 minutes. If the residence time is more than 10 seconds, melt plasticization and dispersion of the additive become sufficient. If the residence time is less than 30 minutes, it is preferred from the viewpoint of being able to suppress the degradation of the resin and the discoloration of the resin.
[0260] (Filtration (filter changing device))
[0261] Type, purpose, structure
[0262] In order to prevent the gear pump from being damaged by foreign matter contained in the raw material and to extend the life of the filter with a fine pore size arranged downstream of the extruder, a filtering device is usually arranged at the outlet of the extruder. It is preferred to use a mesh filter material and a reinforcing plate with a high opening rate to perform so-called splitter plate filtration.
[0263] Mesh size, filtration area
[0264] The mesh size is preferably 40 to 800 meshes, more preferably 60 to 700 meshes, and particularly preferably 100 to 600 meshes. If the mesh size is 40 meshes or more, it is possible to fully suppress foreign matter from passing through the mesh. Furthermore, if it is 800 meshes or less, it is possible to suppress the increase in the rate of increase in the filtration pressure, and to reduce the mesh exchange frequency. Furthermore, from the viewpoint of filtering accuracy and maintaining strength, the filter screen usually uses a plurality of meshes of different sizes overlapped. Furthermore, since the filter opening area can be expanded and the strength of the mesh can be maintained, it is also possible to use a diverter plate to strengthen the filter screen. From the viewpoint of filtering efficiency and strength, the opening rate of the diverter plate used is usually 30 to 80%.
[0265] In addition, the filter screen changing device generally uses a device with the same diameter as the barrel of the extruder, but in order to increase the filtration area, it is usually also used to use a tapered pipe, a filter screen with a larger diameter, or a branch flow path with multiple manifolds. The filtration area is preferably 0.05 to 5 g / cm per second. 2 The index is selected, and more preferably 0.1 to 3 g / cm 2 , especially preferably 0.2 to 2 g / cm 2 .
[0266] The filter is clogged by the capture of foreign matter, and the filtration pressure increases. In this case, the extruder needs to be stopped and the filter replaced, but a type that allows the filter to be replaced while continuing extrusion can also be used. In addition, as a countermeasure for the increase in filtration pressure caused by the capture of foreign matter, a countermeasure that has the function of reducing the filtration pressure by reversing the flow path of the polymer to clean and remove the foreign matter captured by the filter can also be used.
[0267] (Precision Filtration)
[0268] Type, purpose, structure
[0269] In order to filter foreign matter with higher accuracy, it is preferred to set a precision filter device with high filtering accuracy before extruding from the mold. The filtering accuracy of the filter material is preferably high, but from the perspective of the pressure resistance of the filter material and the increase in filtering pressure caused by the clogging of the filter material, the filtering accuracy is preferably 3μm to 30μm, more preferably 3μm to 20μm, and particularly preferably 3μm to 10μm. The precision filtering device is usually set at one place, but multiple places can also be set in series and / or in parallel to perform multi-stage filtration. From the perspective of being able to select a large filtering area and having high pressure resistance, the filter used is preferably provided with a filtering device combined with a blade-type disc filter. In order to withstand pressure and ensure the applicability of the filter life, the blade-type disc filter can adjust the number of loaded sheets.
[0270] The required filtration area varies depending on the melt viscosity of the resin to be filtered, but is preferably 5 to 100 g·cm -2 ·h -1 , more preferably 10 to 75 g·cm -2 ·h -1 , especially preferably 15 to 50 g·cm -2 ·h -1 Increasing the filtration area is advantageous from the viewpoint of increasing the filtration pressure, but it increases the retention time inside the filter and causes the generation of deterioration foreign matter, so it is necessary to select appropriate conditions.
[0271] From the viewpoint of being usable under high temperature and high pressure, the filter medium is preferably a steel material. Among steel materials, stainless steel or steel is more preferably used. From the viewpoint of corrosion, stainless steel is particularly preferably used.
[0272] As the structure of the filter material, in addition to the filter material formed by braiding wires, for example, a sintered filter material formed by sintering metal long fibers or metal powder is also used. In addition, a filter based on a wire of a single diameter is usually used, but in order to improve the filter life and filtering accuracy, filter materials with different wire diameters are sometimes stacked in the thickness direction of the filter or a filter material with a continuously changing wire diameter is used.
[0273] Furthermore, from the viewpoint of filtration accuracy, the thickness of the filter is preferably thick, while from the viewpoint of increased filtration pressure, the thickness of the filter is preferably thin. Therefore, as a range that can meet the conditions, the thickness of the filter is preferably 200 μm to 3 mm, more preferably 300 μm to 2 mm, and particularly preferably 400 μm to 1.5 mm.
[0274] The filter porosity is preferably 50% or more, particularly preferably 70% or more. If it is 50% or more, it can be operated for a long time because of low pressure loss and less clogging. The filter porosity is preferably 90% or less. If it is 90% or less, it can suppress the increase of the filter pressure because it can suppress the crushing of the filter material when the filter pressure rises.
[0275] The filtration accuracy of the filter medium, the wire diameter of the filter medium, the porosity of the filter medium, and the thickness of the filter medium are preferably appropriately selected according to the melt viscosity of the resin to be filtered and the filtration flow rate.
[0276] (Connection piping, etc.)
[0277] The pipes connecting the various parts of the film forming device (adapter pipes, switching valves, mixing devices) also require materials with excellent corrosion resistance and heat resistance, just like the barrel and screw of the extruder. Generally, chrome-molybdenum steel, nickel-chrome-molybdenum steel or stainless steel is used. In addition, in order to improve corrosion resistance, the polymer flow path is plated with HCr, Ni, etc.
[0278] Furthermore, in order to prevent accumulation inside the pipe, the surface roughness inside the pipe is preferably Ra=200 nm or less, and more preferably Ra=150 nm or less.
[0279] In addition, from the perspective of reducing pressure loss, the pipe diameter is preferably large, but on the other hand, it is easy to cause stagnation caused by the decrease in flow velocity in the pipe. Therefore, it is necessary to select an appropriate pipe diameter, preferably 5 to 200 kg·cm - 2 h -1 , more preferably 10 to 150 kg·cm -2 ·h -1 , especially preferably 15 to 100 Kg·cm -2 ·h -1 .
[0280] In order to stabilize the extrusion pressure of liquid crystal polymers whose melt viscosity is highly temperature-dependent, it is preferred to reduce the temperature fluctuation as much as possible in the piping part. Generally speaking, a belt heater with low equipment cost is generally used when heating the piping, but a cast aluminum heater with small temperature fluctuation and a method based on heat medium circulation are more preferred. In addition, from the viewpoint of reducing temperature unevenness, the piping is also preferably divided into multiple areas to control each area separately, similar to the pressure cylinder. In addition, regarding temperature control, PID control (Proportional-Integral-Differential Controller) is usually used, but it is more preferred to combine it with a method of variably controlling the heater output using an AC power regulator.
[0281] Furthermore, by providing a mixing device in the flow path of the extruder to homogenize the resin temperature and resin composition, it is also effective for homogenizing the film. As a mixing device, it is effective to use a spiral or stator type static mixer. A spiral static mixer is effective for homogenizing high-viscosity polymers. By using an n-stage static mixer, it is evenly divided into 2n, so the larger the n, the more the homogenization is promoted. However, on the other hand, there are also problems of pressure loss and the generation of a stagnation portion. Therefore, it is necessary to select according to the required uniformity. In the homogenization of the film, 5 to 20 stages are preferred, and 7 to 15 stages are more preferred. After homogenization based on a static mixer, it is preferred to extrude directly from a die to perform film formation.
[0282] In addition, a discharge valve is provided in the flow path of the extruder, which can discharge the deteriorated polymer inside the extruder without passing through the filter and the die. However, since the switching part is retained and becomes a cause of foreign matter, the switching valve part is required to have strict processing accuracy.
[0283] (Gear Pump)
[0284] In order to improve the thickness accuracy, it is preferred to reduce the variation of the discharge amount. A gear pump is set between the extruder and the mold, and a certain amount of resin is supplied from the gear pump, thereby improving the thickness accuracy. A gear pump refers to a device that is housed in a state where a pair of gears consisting of a driving gear and a driven gear are meshed with each other, and the driving gear is driven to rotate the two gears in meshing, thereby sucking the molten resin into the cavity from the suction port formed on the shell, and spitting out a certain amount of resin from the discharge port formed on the shell. Even if the resin pressure at the front end of the extruder changes slightly, the change is absorbed by using a gear pump, and the change of the resin pressure downstream of the film forming device becomes very small, and the thickness variation is improved. By using a gear pump, the pressure change on the 2nd stage side of the gear pump can be set to less than 1 / 5 of the 1st stage side, and the amplitude of the resin pressure change can be set to within ±1%. As another advantage, filtering based on a filter can be performed without increasing the pressure at the front end of the screw, so it can be expected to prevent the increase in resin temperature, improve the conveying efficiency and shorten the residence time in the extruder. Furthermore, it is also possible to prevent the amount of resin supplied by the screw from varying over time due to an increase in the filtration pressure of the filter.
[0285] Type, size
[0286] Usually, a two-gear type is used for quantitative rotation by meshing two gears, but when pulsation caused by the gears becomes a problem, a three-gear type is usually used to interfere with each other's pulsation to reduce the problem. The size of the gear pump used is usually selected to have a capacity of 5 to 50 rpm under extrusion conditions, and the speed is preferably 7 to 45 rpm, and particularly preferably 8 to 40 rpm.
[0287] By selecting the size of the gear pump so that the rotation speed falls within the above range, it is possible to suppress the increase in the resin temperature due to shear heat generation, and to suppress the degradation of the resin due to the stagnation inside the gear pump.
[0288] Furthermore, since the gear pump is constantly subjected to wear due to meshing of the gears, it is required to use a material having excellent wear resistance, and it is preferable to use a material having the same wear resistance as the screw and the barrel.
[0289] ・Measures for detention units
[0290] The fluidity of the polymer used for the bearing circulation of the gear pump deteriorates, and thus the close fit of the polymer between the driving part and the bearing part deteriorates, which sometimes produces the problem of increasing the variation of the measurement and liquid feeding extrusion pressure, so the gear pump needs to be designed to meet the melt viscosity of the liquid crystal polymer (especially the gap). In addition, depending on the situation, since the retained part of the gear pump becomes the cause of deterioration of the liquid crystal polymer, it is preferred to have a structure with as little retention as possible. In addition, a method is also adopted to prevent the retained polymer from being mixed into the film by discharging the polymer of the retained bearing part to the outside of the gear pump. In addition, when the shear heat in the gear pump is large and the resin temperature rises, it is also effective to cool the gear pump by air cooling and / or circulating the cooling medium.
[0291] Operating conditions
[0292] If the difference between the primary pressure (input pressure) and the secondary pressure (output pressure) of the gear pump is too large, the load of the gear pump becomes larger, and the shear heating becomes larger. Therefore, the pressure difference during operation is preferably within 20MPa, more preferably within 15MPa, and particularly preferably within 10MPa. In addition, in order to homogenize the film thickness, and in order to set the primary pressure of the gear pump to constant, it is also effective to control the screw rotation of the extruder, or to use a pressure control valve.
[0293] (Mold)
[0294] Type, structure, raw materials
[0295] Foreign matter is removed by filtration, and the molten resin whose temperature is further uniformed by the mixer is continuously conveyed to the mold. If the mold is designed to have less retention of the molten resin, any of the commonly used T-type molds, fishtail molds, and hanger molds can be used. Among them, a hanger mold is preferred from the viewpoint of thickness uniformity and less retention.
[0296] The gap at the exit of the T-die is preferably 1 to 20 times the thickness of the film, more preferably 1.5 to 15 times, and particularly preferably 2.0 to 10 times. If the lip gap is 1 times or more the thickness of the film, it is easy to control the film thickness because the increase in the internal pressure of the die can be suppressed, and a sheet with good surface morphology can be obtained by film formation. In addition, if the lip gap is 20 times or less the thickness of the film, it is possible to suppress the pull-off ratio from becoming too large, so the thickness accuracy of the sheet becomes good.
[0297] The thickness of the film is usually adjusted by adjusting the gap of the die at the front end of the die. From the viewpoint of thickness accuracy, a flexible lip is preferably used, but a choke valve may be used for adjustment depending on the situation.
[0298] The gap adjustment of the die can be changed using the adjustment bolts at the die outlet. The adjustment bolts are preferably arranged at intervals of 15 to 50 mm, more preferably at intervals of less than 35 mm, and preferably at intervals of less than 25 mm. If the interval is less than 50 mm, the thickness unevenness between the adjustment bolts can be suppressed. If the interval is more than 15 mm, the rigidity of the adjustment bolt becomes sufficient, so the internal pressure fluctuation of the mold can be suppressed, and the fluctuation of the film thickness can be suppressed. In addition, from the perspective of wall retention, the inner wall surface of the mold is preferably smooth, for example, the surface smoothness can be improved by grinding. Depending on the situation, after the inner wall surface is plated, the smoothness is improved by grinding or the releasability from the polymer is improved by vapor deposition.
[0299] Furthermore, the flow rate of the polymer flowing out of the die is preferably uniform in the width direction of the die. Therefore, it is preferred to change the manifold shape of the die used according to the shear rate dependency of the melt viscosity of the liquid crystal polymer used.
[0300] Furthermore, the temperature of the polymer flowing out of the die is preferably uniform in the width direction. Therefore, it is preferred to make the die uniform by setting the temperature of the die end portion where the heat release of the die is large to a higher level, or by taking measures such as suppressing the heat release of the die end portion.
[0301] In addition, since the quality of the film is significantly reduced due to the occurrence of die lines caused by insufficient processing accuracy of the mold or foreign matter attached to the die outlet, the die lip is preferably smooth, and its arithmetic mean surface roughness Ra is preferably 0.05 μm or less, preferably 0.03 μm or less, and particularly preferably 0.02 μm or less. In addition, the radius of curvature R of the edge of the die lip is preferably 100 μm or less, more preferably 70 μm or less, and particularly preferably 50 μm or less. In addition, a sharp edge processed to R = 20 μm or less by thermal spraying ceramics can also be used.
[0302] The automatic thickness adjustment die is also effective in reducing thickness variations during long-term continuous production by measuring the film thickness downstream, calculating the thickness deviation, and feeding the result back to the die for thickness adjustment.
[0303] The gap between the mold and the point where the polymer rolls land is called an air gap. In order to stabilize film formation based on improving thickness accuracy and reducing shrinkage (increasing the end thickness by reducing the film width), the air gap is preferably short. By setting the angle of the front end of the mold to an acute angle and thinning the mold thickness, interference between the roller and the mold can be prevented and the air gap can be shortened. However, on the other hand, the rigidity of the mold sometimes decreases, and the central part of the mold opens due to the pressure of the resin, resulting in a phenomenon in which the thickness accuracy decreases. Therefore, it is preferable to select a condition that can take into account both the rigidity of the mold and the shortening of the air gap.
[0304] Multilayer film formation
[0305] When manufacturing a thin film, a single-layer film-forming device with low equipment cost is usually used, but in order to set a functional layer on the outer layer, a multilayer film-forming device for manufacturing a thin film with two or more structures can also be used. Specifically, a method of multilayering using a multilayer feed block and a method using a multi-manifold mold can be cited. Generally speaking, it is preferred to thinly laminate the functional layer on the surface layer, but the lamination ratio is not particularly limited.
[0306] The residence time from the pellets entering the extruder from the supply port and flowing out from the supply mechanism (e.g., die) (the residence time from passing through the extruder to being discharged from the die) is preferably 1 to 30 minutes, more preferably 2 to 20 minutes, and particularly preferably 3 to 10 minutes. From the viewpoint of thermal degradation of the polymer, it is preferred to select equipment with a short residence time. Among them, in order to reduce the volume inside the extruder, for example, if the capacity of the filter is set too small, the filter life is sometimes shortened and the exchange frequency is increased. In addition, sometimes the piping diameter is set too small to increase the pressure loss. For this reason, it is preferred to select equipment of appropriate size.
[0307] Furthermore, by setting the residence time to within 30 minutes, it becomes easy to adjust the maximum circle-equivalent diameter of the bright portion to the above range.
[0308] (casting)
[0309] The film forming step preferably includes a step of supplying a molten liquid crystal polymer from a supply mechanism and a step of causing the molten liquid crystal polymer to land on a casting roll to form a film. The film may be directly wound as a film after being cooled and solidified, or may be formed into a film by passing the film between a pair of clamping surfaces and continuously clamping the film.
[0310] At this time, there is no particular limitation on the mechanism for supplying the molten liquid crystal polymer (melt). For example, as a specific mechanism for supplying the melt, there may be a method of using an extruder that extrude the molten liquid crystal polymer into a film, a method of using an extruder and a mold, or a method of melting the liquid crystal polymer into a film by solidifying it once and then melting it with a heating mechanism to form a melt and supplying it to the film forming step.
[0311] When a molten resin extruded into a sheet through a die is clamped by a device having a pair of clamping surfaces, not only can the surface morphology of the clamping surfaces be transferred to the film, but also the orientation can be controlled by imparting elongation deformation to the composition containing the liquid crystal polymer.
[0312] Film forming method and type
[0313] In the method of forming a molten liquid crystal polymer into a film, a high clamping pressure can also be applied. From the viewpoint of excellent film surface morphology, it is preferably passed between two rollers (for example, a contact roller and a cooling roller). In addition, in the present specification, in the case of a plurality of casting rollers for conveying the melt, the casting roller closest to the most upstream liquid crystal polymer supply mechanism (for example, a mold) is referred to as a cooling roller. In addition, a method of clamping metal belts with each other and a method of combining rollers and metal belts can also be used. And, depending on the situation, in order to improve the tightness between the roller and the metal belt, a film forming method such as an electrostatic application method, an air knife method, an air chamber method and a vacuum nozzle method can also be used in combination on the casting drum.
[0314] Furthermore, when obtaining a multilayer film, it is preferably obtained by clamping and pressing the molten polymer extruded from the die in multiple layers, but it is also possible to obtain a multilayer film by introducing a single-layer film into the clamping section in the manner of melt lamination. In addition, at this time, by changing the peripheral speed difference of the clamping section or the orientation axis direction, a film with different inclined structures in the thickness direction can be obtained, and by performing this process multiple times, a film with more than three layers can be obtained.
[0315] Furthermore, during the nip pressing, deformation may be imparted by periodically vibrating the touch roll in the TD direction or the like.
[0316] Roller type and raw material
[0317] From the viewpoint of surface roughness and uniformity of clamping pressure during clamping and uniformity of roller temperature, the casting roller is preferably a metal roller with rigidity. "Rigidity" is not only determined by the material of the clamping surface, but also by the ratio of the thickness of the rigid raw material used in the surface part to the thickness of the structure supporting the surface part. For example, in the case where the surface part is driven by a cylindrical support roller, the ratio of the outer cylinder thickness of the rigid raw material / the diameter of the support roller is shown to be about 1 / 80 or more.
[0318] The material used for the metal roller with rigidity is usually carbon steel and stainless steel, but chromium-molybdenum steel, nickel-chromium-molybdenum steel, and cast iron can be used according to the situation. In addition, in order to change the surface properties of the film such as the peelability, a plating treatment of chromium or nickel, or a ceramic thermal spraying process is sometimes performed. In the case of using a metal belt, in order to impart the necessary clamping pressure, the thickness of the belt is preferably 0.5 mm or more, more preferably 1 mm or more, and particularly preferably 2 mm or more. In addition, in the case of using a rubber roller or a roller composed of a rubber roller and a metal sleeve, since the hardness of the roller is low and the length of the clamping portion becomes longer, sometimes even if a high linear pressure is applied between the rollers, the effective clamping pressure will not increase. Therefore, in order to impart the necessary clamping pressure, it is preferred to use a rubber with extremely high hardness, specifically, the rubber hardness is preferably 80° or more, more preferably 90° or more. Among them, with respect to rubber rollers and metal rollers lined with rubber, due to the large unevenness of the rubber surface, the smoothness of the film sometimes decreases.
[0319] The nip length suitable for applying the nip pressure by the pair of rollers is preferably greater than 0 mm and within 5 m, more preferably greater than 0 mm and within 3 mm.
[0320] Roller diameter
[0321] As the casting roll, a roll with a large diameter is preferably used, and specifically, the diameter is preferably 200 to 1500 mm. If a roll with a large diameter is used, the deflection of the roll can be reduced, so a high clamping pressure can be uniformly applied during the clamping, which is preferred. In addition, in the manufacturing method of the present invention, the diameters of the two rolls for clamping can be the same or different.
[0322] Roller hardness
[0323] In order to provide the inter-roll pressure within the above range, the Shore hardness of the roll is preferably 45 HS or more, more preferably 50 HS or more, and particularly preferably 60 to 90 HS. The Shore hardness can be determined by the method of JIS Z 2246, and the average value of the values measured at 5 points in the roll width direction and 5 points in the circumferential direction.
[0324] Surface roughness, cylindricality, roundness, diameter deviation
[0325] The arithmetic mean surface roughness Ra of the surfaces of the casting roll and the touch roll is preferably 100 nm or less, more preferably 50 nm or less, and particularly preferably 25 nm or less.
[0326] The roundness is preferably 5 μm or less, more preferably 3 μm or less, and particularly preferably 2 μm or less. The cylindricality is preferably 5 μm or less, more preferably 3 μm or less, and particularly preferably 2 μm or less. The diameter deviation is preferably 7 μm or less, more preferably 4 μm, and particularly preferably 3 μm or less. The cylindricality, roundness, and diameter deviation can be obtained by the method of JIS B 0621.
[0327] Roller surface properties
[0328] The surfaces of the casting roll and the touch roll are preferably mirror-finished, and rolls obtained by mirror-finishing the hard chrome-plated surface are generally used. In addition, it is also preferred to laminate nickel plating on the hard chrome-plated base to prevent corrosion, or to use amorphous chrome plating to reduce adhesion to the roll. In addition, in order to improve wear resistance and thin film adhesion to the roll, titanium nitride (TiN), chromium nitride (CrN), DLC (Diamond Like Carbon) treatment, Al, Ni, W, Cr, Co, Zr or Ti-based ceramic thermal spraying and other surface processing can also be performed.
[0329] From the viewpoint of the smoothness of the film after film formation, the roller surface is preferably smooth, but in order to form the surface unevenness for giving the film smoothness, a mirror bag surface roller is used, or a sandblasted roller or a concave roller can be used to form fine unevenness on the film surface. Among them, from the viewpoint of the smoothness of the film, the unevenness of the roller is preferably Ra = 10μm or less. In addition, it is also possible to use a roller surface with a surface unevenness of 1mm per 1mm. 2 A roller with 50 to 1000 fine grooves and prism shapes with a depth of 0.1 to 10 μm engraved in it.
[0330] Roller temperature
[0331] The roller is preferably capable of quickly removing the heat supplied by the molten polymer and maintaining a constant roller surface temperature. Therefore, it is preferred to pass a medium of constant temperature into the roller. As the medium, water or heat medium oil is preferably used, and gas is used as appropriate, and the medium flow rate and medium viscosity that can perform sufficient heat exchange are selected. In addition, the mechanism for setting the roller surface temperature to be constant can use a known method, but a roller with a spiral flow path along the circumference of the roller is preferred. In addition, in order to make the temperature of the roller uniform, a heat pipe can also be used.
[0332] Molten polymer temperature
[0333] From the viewpoint of improving the moldability of the liquid crystal polymer and suppressing degradation, the discharge temperature (resin temperature at the outlet of the supply mechanism) is preferably (Tm of the liquid crystal polymer - 10)° C. to (Tm of the liquid crystal polymer + 40)° C. As an index of melt viscosity, 50 to 3500 Pa·s is preferred.
[0334] The molten polymer in the air gap is preferably cooled as little as possible, and the temperature drop due to cooling is preferably reduced by taking measures such as increasing the film forming speed and shortening the air gap.
[0335] Contact roller temperature
[0336] The temperature of the touch roller is preferably set to be below the Tg of the liquid crystal polymer component. If the temperature of the touch roller is below the Tg of the liquid crystal polymer, it is possible to suppress the adhesion of the molten polymer to the roller, so that the film appearance becomes good. For the same reason, the temperature of the cooling roller is also preferably set to be below the Tg of the liquid crystal polymer.
[0337] ·Difference between film forming speed and peripheral speed
[0338] From the viewpoint of keeping the melt warm in the air gap, the film forming speed is preferably 3 m / min or more, more preferably 5 m / min or more, and particularly preferably 7 m / min or more. When the line speed is increased, the melt can be suppressed from cooling in the air gap, and a more uniform clamping and shear deformation can be given in a state where the temperature of the melt is high. In addition, the above-mentioned film forming speed is defined as the second clamping surface speed when the molten polymer passes between the two clamped rollers, which is slow.
[0339] The moving speed of the first clamping surface is preferably set to be faster than the moving speed of the second clamping surface. In addition, the moving speed ratio of the first clamping surface to the second clamping surface of the clamping device is preferably adjusted to 0.60 to 0.99, and the molten resin is given shear stress when passing through the clamping device to manufacture the film of the present invention. The two clamping surfaces can be driven in conjunction or independently, but from the perspective of uniformity of film properties, they are preferably driven independently.
[0340] (Film formation sequence of polymer films)
[0341] Film formation sequence
[0342] In the film forming step, from the viewpoint of thin film forming step and stabilization of quality, the film forming is preferably performed in the following order.
[0343] The molten polymer discharged from the die lands on the casting roll to be formed into a film, and then is cooled and solidified to be wound up as a film.
[0344] When the molten polymer is sandwiched and pressed, the molten polymer is passed between the first sandwiching surface and the second sandwiching surface set to a predetermined temperature, and is cooled and solidified to be wound as a film.
[0345] Conveying tension
[0346] The film conveying tension can be appropriately adjusted according to the film thickness. The conveying tension per 1m width of the film is preferably 10 to 500 N / m, more preferably 20 to 300 N / m, and particularly preferably 30 to 200 N / m. Normally, if the film becomes thicker, the conveying tension needs to be increased. For example, in the case of a film with a thickness of 100 μm, it is preferably 30 to 150 N / m, more preferably 40 to 120 N / m, and particularly preferably 50 to 100 N / m. If the film conveying tension is above the lower limit, the bending of the film during the film conveying process can be suppressed, thereby suppressing the slippage between the guide roller and the film and causing scratches on the film. If the film conveying tension is below the upper limit, vertical wrinkles can be suppressed in the film, and the film can be suppressed from being forcibly stretched and broken.
[0347] The film tension control can be performed by any of the methods based on reciprocating shaking, the torque control method based on the servomotor, the method based on the powder clutch / brake, and the control method based on the friction roller, but from the viewpoint of control accuracy, the method based on reciprocating shaking is preferred. The conveying tension does not need to be set to the same value throughout the film forming process, and it is also useful to adjust it to an appropriate value in each tension cut area.
[0348] The conveying roller preferably has a smooth surface that does not cause roller bending deformation caused by conveying tension, has low mechanical loss, has sufficient friction with the film, and is not easily scratched during the conveying of the film. If a conveying roller with low mechanical loss is used, a large tension is not required for conveying the film, and scratches in the film can be suppressed. In addition, in order to rub against the film, the conveying roller preferably selects a larger contact angle of the film. The contact angle is preferably 90° or more, more preferably 100° or more, and particularly preferably 120° or more. In the case where a sufficient contact angle cannot be selected, it is preferred to use a rubber roller, or a roller with a texture, a pit shape or a groove on the roller surface to ensure friction.
[0349] Winding tension
[0350] The winding tension is also similar to the film conveying tension, and is preferably adjusted appropriately according to the film thickness. The tension per 1m width of the film is preferably 10 to 500 N / m, more preferably 20 to 300 N / m, and particularly preferably 30 to 200 N / m. Generally speaking, if the film becomes thicker, the tension needs to be increased. For example, in the case of a 100μm film, the winding tension is preferably 30 to 150 N / m, more preferably 40 to 120 N / m, and particularly preferably 50 to 100 N / m.
[0351] If the winding tension is above the lower limit, the bending of the film during the film conveying process can be suppressed, so that the film can be prevented from slipping and scratching in the middle of the winding. If the winding tension is below the upper limit, the film can be prevented from being brought into the vertical wrinkles, and the film can be prevented from being rolled very hard so that the curling appearance becomes good, and the concave and convex parts of the film can be prevented from extending through the creep phenomenon, so the film can be prevented from wrinkling. The winding tension is the same as the conveying tension, and it is preferably detected by tension control in the middle of the line, and the winding is performed while being controlled to a constant winding tension. When there is a temperature difference in the film according to the position of the film forming line, the length of the film is sometimes slightly different due to thermal expansion, so it is preferred to adjust the stretching ratio between the nip rollers (niproll), and the film will not be applied with a tension above the prescribed tension in the middle of the line. In addition, the winding tension can also be wound at a constant tension by tension control, but it is more preferred to add a dimension (taper) according to the diameter of the winding to make it an appropriate winding tension. Generally speaking, the tension is gradually reduced as the curling diameter increases, but it is sometimes preferred to increase the tension as the curling diameter increases depending on the situation. In addition, regarding the winding direction, there is no problem even if either the first clamping surface or the second clamping surface is set as the winding core side, but when curling occurs on the film, it is sometimes preferred to have a curl correction effect when winding in the opposite direction to the curling. In order to control the bending of the film during winding, EPC (Edge Position Control) is set, and it is also useful to perform oscillation curling to prevent the generation of curling bumps and to use a roller to remove the accompanying air during high-speed winding.
[0352] Winding core
[0353] As long as the winding core used for winding has the strength and rigidity required for winding the film, there is no need to use a special winding core. Usually, a paper tube with an inner diameter of 3 to 6 inches or a plastic winding core with an inner diameter of 3 to 14 inches is used. Generally speaking, from the perspective of low dust emission, a plastic winding core is widely used. Using a winding core with a small diameter is cost-effective, but sometimes the curling shape is poor due to deflection caused by insufficient rigidity, or curling of the film caused by creep deformation occurs in the winding core part. On the other hand, using a winding core with a large diameter is beneficial for maintaining the quality of the film, but from the perspective of operability and cost, it sometimes becomes disadvantageous. Therefore, it is preferable to select a winding core of an appropriate size. In addition, a cushioning layer can be provided on the outer periphery of the winding core to prevent the step difference in the film thickness corresponding to the starting part of the curling from being transferred to the film.
[0354] Slit
[0355] In order to set the film to a predetermined width, the two ends are preferably split. As a method of splitting, common methods such as shear blades, Goebel blades, razor blades and rotary blades can be used, but it is preferred to use a cutting method that does not generate dust during cutting and has less warping of the cut portion, preferably cutting based on a Goebel blade. The material of the cutting blade can be any of carbon steel and stainless steel, etc. Usually, if a hard blade or a ceramic blade is used, the life of the blade is long and the generation of cutting powder is suppressed, so it is preferred.
[0356] The parts cut off by segmentation can be crushed and used as raw materials again. After segmentation, they can be crushed and immediately put into the extruder, or they can be used by granulation once through the extruder. In addition, in the re-granulation process, foreign matter removal based on filtration can be performed. The blending amount is preferably 0-60%, more preferably 5-50%, and particularly preferably 10-40%. Since the melt viscosity of the molten polymer and the trace components caused by thermal degradation may be different from those of the original raw materials, care should be taken when using the recycled raw materials. It is also useful to appropriately adjust the blending amount according to the composition of the recycled raw materials to control the physical properties of the raw materials within a certain range. In addition, the film during thickness adjustment and switching can also be reused in the same way as the divided edges.
[0357] Knurling
[0358] It is also preferred to perform thickening processing (knurling) on one or both ends of the film. The height of the concavo-convex due to the thickening processing is preferably 1 to 50 μm, more preferably 2 to 30 μm, and particularly preferably 3 to 20 μm. During the thickening processing, both sides can be set to a convex shape, or only one side can be set to a convex shape. The width of the thickening processing is preferably 1 to 50 mm, and particularly preferably 3 to 30 mm. The thickening processing can use either cold processing or hot processing, as long as an appropriate method is selected according to the droop of the concavo-convex formed in the film and the state of dust during the thickening processing. In addition, it is also useful to be able to identify the film forming direction and film surface of the film through knurling.
[0359] Masking film
[0360] In order to prevent film scratches and improve workability, a laminate film (masking film) is preferably provided on one or both sides. The thickness of the laminate film is preferably 5 to 100 μm, more preferably 10 to 70 μm, and particularly preferably 25 to 50 μm.
[0361] The masking film is preferably composed of two layers, a base material layer and an adhesive layer. LDPE (low-density polyethylene), LLDPE (linear low-density polyethylene), HDPE (high-density polyethylene), PP (polypropylene), polyester, etc. can be used for the base material layer. EVA (ethylene vinyl acetate), acrylic rubber, styrene elastomer, natural rubber, etc. can be used for the adhesive layer. In addition, any type based on the co-extrusion method and the type in which the adhesive material is applied to the film can be used.
[0362] The adhesive force is preferably 0.2 to 2.0 N / 25 mm, more preferably 0.3 to 1.5 N / 25 mm, and particularly preferably 0.4 to 1.0 N / 25 mm. The adhesive force can be determined according to the method of JIS Z 0237.
[0363] Generally speaking, colorless masking films are often used, but in order to identify the front and back sides of the film, masking films with different colors on the front and back sides are sometimes used. As another method for identifying the front and back sides of the film, a method of attaching masking films with different thicknesses, adhesive strengths, and glossiness of the film surface is also effective.
[0364] Eliminate static electricity
[0365] When the film is charged, dust in the atmosphere is attracted to the film and becomes foreign matter attached to the film. Therefore, it is preferable that the film is not charged during film formation, transportation, and winding.
[0366] The charged voltage is preferably 3 KV or less, more preferably 0.5 KV or less, and particularly preferably 0.05 KV or less.
[0367] As a method for preventing the film from being charged, the following various well-known methods can be used: a method of preventing the generation of static electricity by kneading or applying an antistatic agent into the film, a method of suppressing the generation of static electricity by controlling the temperature and humidity in the atmosphere, a method of releasing the static electricity charged on the film by grounding, and a method of neutralizing the static electricity with an ion generator using a charge with a sign opposite to the charged charge, etc. Among them, the method of using an ion generator is generally used. The ion generator has a soft X-ray irradiation type and a corona discharge type, and either type can be used. The soft X-ray irradiation type is used when explosion protection is required, and generally speaking, the corona discharge type is widely used. The corona discharge method includes DC (direct current) type, AC (alternating current) type and pulse AC type. From the perspective of performance and cost, the pulse AC type is widely used. The static elimination device can be used in one type or in combination of multiple types. As long as it does not hinder film formation, there is no special restriction on the number of settings.
[0368] Furthermore, in order to enhance the effect of preventing dust from adhering to the film due to static elimination, the film forming environment is preferably below Class 10000 of the US Federal Standard Fed. Std. 209D, more preferably below Class 1000, and particularly preferably below Class 100.
[0369] Dust removal
[0370] Foreign matter attached to the surface of the film can be removed by the following methods, namely, a method of using an extrusion scraper and a brush, a method of ejecting pressurized air that has been neutralized at a pressure of about tens of Kpa in order to reduce the attraction effect caused by static electricity, a method based on attraction, and a method combining injection and attraction. In addition, a method of removing foreign matter by transferring the foreign matter to the adhesive roller by pressing an adhesive roller against the film and a method of applying ultrasound close to the film to remove the foreign matter by attraction can be used, and other well-known dust removal mechanisms. In addition, a method of spraying a liquid onto the film and a method of immersing the film in a liquid to wash away foreign matter can also be used. In addition, in the case where film powder is generated by cutting the cut portion or the knurled portion, it is also preferable to install a removal device such as a vacuum nozzle to prevent foreign matter from adhering to the film.
[0371] (Stretching and relaxing)
[0372] In addition, after the unstretched film is formed by the above method, it can be stretched and / or relaxed. For example, the following (a) to (g) can be combined to implement each process. In addition, the order of longitudinal stretching and transverse stretching can be reversed, each process of longitudinal stretching and transverse stretching can be performed in multiple stages, or oblique stretching or simultaneous biaxial stretching can be combined.
[0373] (a) Transverse stretching
[0374] (b) Horizontal stretching → relaxation
[0375] (c) Longitudinal stretching
[0376] (d) Longitudinal stretching → relaxation
[0377] (e) Longitudinal (transverse) stretching → transverse (longitudinal) stretching
[0378] (f) Longitudinal (transverse) stretching → transverse (longitudinal) stretching → relaxation
[0379] (g) Transverse stretching → relaxation → longitudinal stretching → relaxation
[0380] ·Longitudinal stretch
[0381] Longitudinal stretching can be achieved by heating between two pairs of rollers while making the circumferential speed on the outlet side faster than the circumferential speed on the inlet side. From the viewpoint of curling of the film, the film temperature on the front and back sides is preferably the same temperature, but when the optical properties are controlled in the thickness direction, stretching can be performed even at different temperatures on the front and back sides. In addition, the stretching temperature is defined as the temperature on the lower side of the film surface. The longitudinal stretching process can be implemented in one stage or in multiple stages. The film is usually preheated by a temperature-controlled heating roller, but a heater can also be used to heat the film depending on the situation. In addition, in order to prevent the film from adhering to the roller, a ceramic roller with improved adhesion can also be used.
[0382] [Horizontal stretch]
[0383] As the transverse stretching process, a common transverse stretching can be used. That is, the common transverse stretching refers to a transverse stretching method in which the two ends of the film are held with clips and the clips are widened while being heated in an oven using a tenter. For example, the methods described in Japanese Utility Model Publication No. 62-035817, Japanese Patent Publication No. 2001-138394, Japanese Patent Publication No. 10-249934, Japanese Utility Model Publication No. 6-270246, Japanese Utility Model Publication No. 4-30922 and Japanese Patent Publication No. 62-152721 can be used.
[0384] The stretching temperature in the transverse stretching process can be controlled by sending wind of the desired temperature into the tenter. For the same reason as the longitudinal stretching process, the film temperature can be the same on the front and back sides or different. The stretching temperature used here is defined as the temperature on the lower side of the film surface. The transverse stretching process can be implemented in one stage or in multiple stages. Moreover, when the transverse stretching is performed in multiple stages, it can be performed continuously or intermittently with an area that is not widened set in between. In addition to the usual transverse stretching in which the clips are widened in the width direction in the tenter, the following stretching method in which the clips are held and widened can also be applied in the same manner.
[0385] Oblique stretch
[0386] The clips are expanded in the horizontal direction as in the conventional horizontal stretching, but the stretching in the oblique direction can be performed by changing the conveying speed of the left and right clips. For example, the methods described in Japanese Patent Publication No. 2002-22944, Japanese Patent Publication No. 2002-086554, Japanese Patent Publication No. 2004-325561, Japanese Patent Publication No. 2008-23775, and Japanese Patent Publication No. 2008-110573 can be used.
[0387] Simultaneous biaxial stretching
[0388] Simultaneous biaxial stretching is similar to conventional transverse stretching in that the clip is expanded in the transverse direction, but at the same time stretched or contracted in the longitudinal direction. For example, the methods described in Japanese Utility Model Application Laid-Open No. 55-093520, Japanese Patent Application Laid-Open No. 63-247021, Japanese Patent Application Laid-Open No. 6-210726, Japanese Patent Application Laid-Open No. 6-278204, Japanese Patent Application Laid-Open No. 2000-334832, Japanese Patent Application Laid-Open No. 2004-106434, Japanese Patent Application Laid-Open No. 2004-195712, Japanese Patent Application Laid-Open No. 2006-142595, Japanese Patent Application Laid-Open No. 2007-210306, Japanese Patent Application Laid-Open No. 2005-022087, Japanese Patent Application Laid-Open No. 2006-517608, and Japanese Patent Application Laid-Open No. 2007-210306 can be used.
[0389] Improvement of warpage (axis misalignment)
[0390] In the above-mentioned transverse stretching process, the ends of the film are held by clips, so the deformation of the film caused by the thermal shrinkage stress generated during the heat treatment becomes larger in the central part of the film and smaller at the ends, resulting in the distribution of the characteristics in the width direction. Before the heat treatment process, when a straight line is drawn in the transverse direction on the surface of the film, the straight line on the surface of the film after the heat treatment process becomes an arched shape with the center concave toward the downstream. This phenomenon is called the warping phenomenon, which becomes the cause of disturbing the isotropy of the film and the uniformity in the width direction.
[0391] As an improvement method, the deviation of the orientation angle accompanying the warping can be reduced by preheating before such transverse stretching and heat fixing after stretching. Either preheating or heat fixing can be performed, and both are more preferably performed. These preheating and heat fixing are preferably performed by clamping, that is, they are preferably performed continuously with the stretching.
[0392] Preheating is preferably performed at a temperature about 1 to 50° C. higher than the stretching temperature, more preferably 2 to 40° C. higher, and particularly preferably 3 to 30° C. higher. The preheating time is preferably 1 second to 10 minutes, more preferably 5 seconds to 4 minutes, and particularly preferably 10 seconds to 2 minutes.
[0393] During preheating, the width of the tenter is preferably kept substantially constant, wherein "substantially" means ±10% of the width of the unstretched film.
[0394] Thermal fixing is preferably performed at a temperature 1 to 50° C. lower than the stretching temperature, more preferably 2 to 40° C. lower, and further preferably 3 to 30° C. lower. In particular, it is preferably set at a temperature lower than the stretching temperature and lower than the Tg of the liquid crystal polymer.
[0395] The preheating time is preferably 1 second to 10 minutes, more preferably 5 seconds to 4 minutes, and particularly preferably 10 seconds to 2 minutes. During heat fixing, the width of the tenter is preferably kept approximately constant. Among them, "approximately" means 0% (the same width as the width of the tenter after stretching) to -30% (30% reduction in width than the width of the tenter after stretching = reduced width) of the tenter after the end of stretching. When widening is performed with a width greater than the stretching width, it becomes easy to generate residual strain in the film. As other known methods, the methods described in Japanese Patent Publication No. 1-165423, Japanese Patent Publication No. 3-216326, Japanese Patent Publication No. 2002-018948 and Japanese Patent Publication No. 2002-137286 can be cited.
[0396] Relaxation treatment
[0397] After the stretching, the heat shrinkage can be reduced by performing a heat relaxation treatment based on the following conditions. The heat relaxation treatment is preferably performed at least one of after film formation, after longitudinal stretching, and after transverse stretching. The relaxation treatment can be performed continuously online after stretching, or offline after winding after stretching.
[0398] (Surface treatment)
[0399] The film can be surface treated to improve adhesion to the copper foil or copper plating layer used in the copper-clad laminate. For example, glow discharge treatment, ultraviolet irradiation treatment, corona treatment, flame treatment, and acid or alkali treatment can be used. The glow discharge treatment mentioned here can be 10 -3 Low-temperature plasma generated under low-pressure gas of 20 Torr or less is preferably used as plasma treatment under atmospheric pressure.
[0400] Plasma excited gas refers to a gas excited by plasma under the above conditions, and examples thereof include freons such as argon, helium, neon, krypton, xenon, nitrogen, carbon dioxide, tetrafluoromethane, and mixtures thereof. In order to bond the copper foil or the copper-plated layer, it is also preferred to provide a primer layer. This layer can be applied after the above-mentioned surface treatment, or it can be applied without the surface treatment. These surface treatment and primer coating steps can also be introduced at the end of the film forming step, can be implemented separately, or can be implemented during the process of imparting the copper foil or the copper-plated layer.
[0401] (aging)
[0402] In order to improve the mechanical properties, thermal dimensional stability, and winding posture of the wound film, it is also useful to age the film at a temperature below the Tg of the liquid crystal polymer.
[0403] (Storage conditions)
[0404] In order to prevent the wound film from producing wrinkles and bumps caused by residual strain relaxation, it is preferred to store the film in a temperature environment below the Tg of the liquid crystal polymer. In addition, the temperature preferably fluctuates little, and the temperature fluctuation per hour is preferably 30°C or less, more preferably 20°C or less, and particularly preferably 10°C or less. Similarly, in order to prevent changes in the moisture absorption rate of the film and condensation, the humidity is preferably 10-90%, more preferably 20-80%, and particularly preferably 30-70%, and the temperature fluctuation per hour is preferably 30% or less, more preferably 20% or less, and particularly preferably 10% or less. In the case of storage in a location where temperature and humidity fluctuations are required, it is also effective to use a material with moisture-proof and heat-insulating properties in the packaging material.
[0405] In the above description, the thin film is a single layer, but may have a laminated structure in which a plurality of layers are laminated.
[0406] [Application of polymer films]
[0407] The liquid crystal polymer film of the present invention can be used in the form of a film alone, a copper-clad laminate laminated with copper foil, a printed wiring board, a flexible printed wiring board (FPC), etc., and can be used as a material included in a communication substrate. That is, the communication substrate of the present invention has the polymer film of the present invention.
[0408] Example
[0409] Below, based on embodiment, the present invention is further described in detail.As long as the material, usage amount, ratio, processing content and processing sequence etc. shown in the following examples do not depart from the purpose of the present invention, then can be changed appropriately.Therefore, the scope of the present invention should not be interpreted restrictively by the embodiment shown below.
[0410] [Example 1]
[0411] 〔Granulation process〕
[0412] As the liquid crystal polymer, a thermotropic liquid crystal polyester manufactured by Polyplasrics Co., Ltd. (product name "LAPEROSA-950", melting point 280°C, refer to the following formula (I). In Table 1, it is marked as "LCPA") was used, and as component A, silica particles 1 manufactured by Admatechs. (product name "ADMANANO", average primary particle size 100 nm) were used.
[0413] 10 parts by mass of component A was added to 90 parts by mass of the liquid crystal polymer, and kneaded and granulated using a twin-screw extruder. The shear rate of the twin-screw extruder during kneading and granulation (hereinafter also referred to as "shear rate (granulation)") was set to 300 seconds. -1 .
[0414] The kneaded pellets were dried at 80° C. for 12 hours using a dehumidified hot air dryer having a dew point temperature of −45° C. so that the moisture content in the kneaded pellets became 50 mass ppm or less.
[0415] [Chemical formula 1]
[0416]
[0417] 〔Film forming process〕
[0418] 100 parts by mass of dried kneaded particles, 0.1 parts by mass of a solid lubricant (stearic acid) and 0.1 parts by mass of a solid heat stabilizer (Irganox 1010 (manufactured by BASF)) were supplied to the cylinder from the same supply port of a twin-shaft extruder having a screw diameter of 50 mm, and after heating and kneading at 305 to 315° C. to obtain a kneaded product, a film-like kneaded product in a molten state was discharged from a die having a die width of 750 mm and a slit interval of 300 μm. The time from when the kneaded product passed through the twin-shaft extruder to when the film-like kneaded product was discharged from the die (hereinafter also referred to as “residence time (film formation)”) was set to 8 minutes.
[0419] The thickness unevenness in the width direction of the film was improved by finely adjusting the gap of the die lip. In this way, a polymer film of Example 1 having a thickness of 100 μm was obtained.
[0420] [Example 2, Example 3, Comparative Example 1]
[0421] Polymer films of Example 2, Example 3 and Comparative Example 1 were obtained in the same manner as in Example 1, except that silica particles 2 (product name "ADMAFINE", average primary particle size 1,000 nm), silica particles 3 (product name "ADMAFUSE", average primary particle size 10,000 nm) or silica particles 4 (product name "ADMAFUSE", average primary particle size 11,000 nm) manufactured by Admatechs. were used instead of silica particles 1.
[0422] [Comparative Example 2]
[0423] A polymer thin film of Comparative Example 2 was obtained in the same manner as in Example 1 except that the residence time (at the time of film formation) was changed to the time shown in Table 1.
[0424] [Examples 4 to 5]
[0425] Polymer films of Examples 4 to 5 were obtained in the same manner as in Example 1, except that COC (cyclic olefin copolymer, product name "Tupas", manufactured by Polyplastics Co., Ltd.) or SEBS (polystyrene-poly(ethylene-butylene)-polystyrene triblock copolymer, product name "Tuftec", manufactured by Asahi Kasei Corporation) was used instead of silica particles 1.
[0426] [Example 6]
[0427] A polymer film of Example 6 was obtained in the same manner as in Example 1 except that PE (polyethylene resin, product name "NOVATEC", manufactured by Japan Polyethylene Corporation) was used instead of silica particles 1, and the shear rate (during granulation) and residence time (during film formation) were changed to the speeds shown in Table 1.
[0428] [Example 7]
[0429] A polymer film of Example 7 was obtained in the same manner as in Example 1 except that PE (polyethylene resin, product name “NOVATEC”, manufactured by Japan Polyethylene Corporation) was used instead of the silica particles 1.
[0430] [Comparative Example 3]
[0431] A polymer film of Comparative Example 3 was obtained in the same manner as in Example 6 except that the shear rate (during granulation) was changed to the rate shown in Table 1.
[0432] [Comparative Example 4]
[0433] A polymer film of Comparative Example 4 was obtained in the same manner as in Example 1 except that Component A was not used.
[0434] [Examples 8 to 9]
[0435] Polymer films of Examples 8 and 9 were obtained in the same manner as in Example 2 except that the amount of component A added was adjusted so that the area ratio of the island-shaped regions would become the value shown in Table 1.
[0436] [Examples 10 to 13]
[0437] Polymer films of Examples 10 to 13 were obtained in the same manner as in Example 2 except that the speed of the casting roll was adjusted so that the thickness of the polymer film would become the value shown in Table 1.
[0438] [Physical property measurement]
[0439] The polymer films were subjected to the following measurements and evaluations.
[0440] 〔The maximum equivalent circle diameter of the bright part〕
[0441] A microtome is used to cut 20 different locations of the polymer film along a direction parallel to the main surface of the polymer film (i.e., a direction perpendicular to the thickness direction of the polymer film), and thin sheet samples of a specified thickness (e.g., 10 μm) are cut out to obtain 20 samples for observation.
[0442] Next, 20 observation images corresponding to the observation area were obtained by observing from the normal direction of the main surface of the observation sample under an orthogonal Nicol environment using a polarizing microscope (product name "BH-2", manufactured by Olympus Corporation). In addition, the magnification during observation was selected to be an appropriate magnification within the range of 10 to 1000 times.
[0443] Next, for each of the 20 observation images, the outer periphery of the bright portion was traced, and the diameter of a circle having the same area as the traced area (equivalent circle diameter) was measured by an image analysis device. The maximum value of the equivalent circle diameter of the bright portion obtained from the 20 observation images was defined as the maximum equivalent circle diameter of the bright portion.
[0444] 〔Area ratio of bright part〕
[0445] For each of the 20 observation images obtained by the above-mentioned method for measuring the maximum equivalent circular diameter of the bright portion, the total area of the equivalent circular diameter of the bright portion was calculated, and the ratio (%) of the total area of the equivalent circular diameter of the bright portion to the total area of the observation image was calculated. Furthermore, the arithmetic mean value of the 20 observation images was calculated and was set as the area ratio of the bright portion.
[0446] 〔Circle-equivalent diameter of island area〕
[0447] The polymer film was cut at 10 different locations of the polymer film so as to obtain a fracture cross section parallel to the width direction of the polymer film and perpendicular to the surface of the polymer film. Furthermore, the polymer film was cut at 10 different locations of the polymer film so as to obtain a fracture cross section parallel to the long side direction of the polymer film and perpendicular to the surface of the polymer film.
[0448] Next, a scanning electron microscope (SEMEDX Type H, manufactured by Hitachi, Ltd.) was used to observe the fracture cross sections of a total of 20 locations, and 20 observation images corresponding to the observation area were obtained. In addition, an appropriate magnification within the range of 100 to 100,000 times was selected during the observation, and the entire range in the thickness direction of the polymer film was observed.
[0449] For any 200 island-shaped areas in the 20 observation images, the periphery of the island-shaped area was traced, and the diameter of a circle having the same area as the traced area (equivalent circle diameter) was measured by an image analysis device. Furthermore, the arithmetic mean of the equivalent circle diameters of the 200 island-shaped areas was set as the equivalent circle diameter of the island-shaped area.
[0450] 〔Area ratio of island regions〕
[0451] A square region (selected region) of 10 μm in length×10 μm in width was selected from each of 20 observed images obtained by the above-mentioned method for measuring the equivalent circle diameter of the island-shaped region.
[0452] Next, the outer periphery of the island-shaped area existing in the selected area is traced, and the total area occupied by the island-shaped area is measured by an image analysis device, and the ratio (%) of the total area of the island-shaped area to the area of the selected area is calculated. In addition, the arithmetic mean value of the 20 observed images is calculated and is set as the area ratio of the island-shaped area.
[0453] 〔Distance between islands〕
[0454] A square region (selected region) of 10 μm in length×10 μm in width was selected from each of 20 observed images obtained by the above-mentioned method for measuring the equivalent circle diameter of the island-shaped region.
[0455] Next, the outer periphery of the island-shaped region existing in the selected region was traced, and the shortest distance between different island-shaped regions was measured by an image analysis device. Furthermore, the arithmetic mean value of the 20 observed images was calculated and used as the distance between the island-shaped regions.
[0456] 〔thickness〕
[0457] The arithmetic mean of the thickness of the polymer film at 100 different points was determined using a contact thickness meter (manufactured by Mitutoyo Corporation), and this was defined as the thickness of the polymer film.
[0458] 〔Young's modulus ratio〕
[0459] The Young's modulus of the polymer film was measured by a tensile test in JIS K 7127. In addition, the central part of the polymer film was measured at 5 locations in the MD direction and TD direction, and the value obtained by dividing the average value in the MD direction by the average value in the TD direction was set as the Young's modulus ratio. It can be said that the closer this value is to 1, the smaller the anisotropy of the Young's modulus in the polymer film.
[0460] 〔Dielectric loss tangent ratio, dielectric constant ratio〕
[0461] The dielectric loss tangent and dielectric constant were measured by the resonance perturbation method at a frequency of 10 GHz. Specifically, a 1 GHz cavity resonator (KANTO Flectronic Application and Development Inc.) was connected to a network analyzer ("E8362B" manufactured by Agilent Technology), and a tiny material (width: 2.7 mm × length: 45 mm) was inserted into the cavity resonator. The dielectric loss tangent and dielectric constant of the material were measured from the change in the resonant frequency before and after 96 hours of insertion under a temperature of 20°C and a humidity of 65% RH. In addition, the central part of the polymer film at 5 locations in the MD direction and the TD direction was measured, and the value obtained by dividing the average value in the MD direction by the average value in the TD direction was set as the dielectric loss tangent ratio and the dielectric constant ratio. It can be said that the closer the value is to 1, the smaller the anisotropy of the dielectric loss tangent and the dielectric constant in the polymer film.
[0462] 〔CTE ratio〕
[0463] The CTE (coefficient of linear expansion) of the polymer film was measured according to JIS K 7197. The center portion of the polymer film was measured at five locations in the MD direction and five locations in the TD direction, and the average value in the MD direction was divided by the average value in the TD direction, and the value obtained was defined as the CTE ratio.
[0464] From the obtained CTE ratio, the anisotropy of the linear expansion coefficient in the polymer film was evaluated according to the following evaluation criteria.
[0465] A: 0.8<CTE ratio<1.5
[0466] B: 0.5<CTE ratio ≤ 0.8 or 1.5 ≤ CTE ratio < 2.0
[0467] C: CTE ratio ≤ 0.5 or 2.0 ≤ CTE ratio
[0468] 〔Arithmetic mean surface roughness Ra〕
[0469] The arithmetic mean surface roughness Ra of the polymer film was measured using a stylus roughness meter in accordance with JIS B 0601. In addition, the measurement was performed at five randomly selected locations within a 10 cm×10 cm area in the center of the film, and the average value was calculated.
[0470] Based on the obtained values, evaluation was performed according to the following criteria.
[0471] A: less than 300nm
[0472] B: 300nm or more and less than 400nm
[0473] C: 400nm or more
[0474] In Table 1, "shear rate (granulation)" refers to the shear rate of the twin-screw extruder during kneading and granulation in the above-mentioned granulation step, and "residence time (film formation)" refers to the time from the time when the kneaded material passes through the twin-screw extruder to the time when the kneaded material in a film-like state is discharged from the die in the above-mentioned film formation step.
[0475] [Table 1]
[0476]
[0477] As shown in Table 1, it is shown that the anisotropy of the linear expansion coefficient of the polymer film having the maximum circle-equivalent diameter of the bright portion of 10 μm or less is small (Example).
[0478] Comparison of Examples 1 to 3 shows that when inorganic particles are used as Component A, the anisotropy of the linear expansion coefficient can be reduced if the circle-equivalent diameter of the island-shaped region is within the range of 0.01 to 1 μm (Examples 1 and 2).
[0479] Comparison of Examples 4 to 7 shows that the equivalent circle diameter of the island-shaped region can be controlled by the type of polymer when a polymer is used as component A. It also shows that the anisotropy of the linear expansion coefficient can be reduced by using a polymer having an equivalent circle diameter of 0.01 to 1 μm in the island-shaped region (Examples 5 to 7).
[0480] Comparison between Examples 2, 8, and 9 shows that when the area ratio of the island-shaped regions is within the range of 1 to 50% (Examples 2 and 8), the balance between the reduction in anisotropy of the linear expansion coefficient and the reduction in the surface roughness Ra is excellent.
[0481] Comparison between Examples 2 and 10 to 13 shows that when the thickness of the polymer film is within the range of 5 to 1000 μm (Examples 2 and 10 to 12), the anisotropy of the linear expansion coefficient can be reduced and the surface roughness Ra can also be reduced.
[0482] As shown in Table 1, it is shown that the anisotropy of the linear expansion coefficient of the polymer film in which the maximum circle-equivalent diameter of the bright portion exceeds 10 μm is high (Comparative Example).
Claims
1. A polymer film comprising a liquid crystal polymer, wherein: When the surface of the polymer film is observed under crossed Nicols by a polarizing microscope, a plurality of bright portions are observed in the observed area. The bright portion having the largest circle equivalent diameter among the plurality of bright portions has a circle equivalent diameter of 10 μm or less. The polymer film includes a component selected from inorganic particles and a polymer different from the liquid crystal polymer, and the content of the component is 5 mass % to 20 mass % relative to the total mass of the polymer film. When a vertical cross section relative to the surface of the polymer film is observed by a scanning electron microscope, a plurality of island-shaped regions composed of the component are observed in the observed region, and the circle-equivalent diameter of the island-shaped regions is 0.001 μm to 10 μm. When the polymer film includes the inorganic particles, the average primary particle size of the inorganic particles is 5 nm to 100 nm or 1000 nm to 10000 nm.
2. The polymer film according to claim 1, wherein A ratio of a total area of the bright portions to an area of the observation region in the polarizing microscope is 60% or less.
3. The polymer film according to claim 1, wherein The ratio of the total area of the island-shaped regions to the area of the observation region in the scanning electron microscope is 1% to 60%.
4. The polymer film according to claim 1, wherein The material constituting the inorganic particles is at least one selected from silicon dioxide, titanium oxide, barium sulfate, talc, zirconium oxide, aluminum oxide, silicon nitride, silicon carbide, calcium carbonate, silicate, glass beads, graphite, tungsten carbide, carbon black, clay, mica, carbon fiber, glass fiber and metal powder. The polymer is at least one selected from thermoplastic resins and elastomers.
5. The polymer film according to claim 1, wherein The distance between the island regions is 0.0001 μm to 5 μm.
6. The polymer film according to claim 1 or 2, wherein: The ratio of the Young's modulus in a second direction in the plane of the polymer film orthogonal to the first direction to the Young's modulus in a first direction in the plane of the polymer film is 0.5 to 1.
9.
7. The polymer film according to claim 1 or 2, wherein: A ratio of a dielectric loss tangent in a second direction in the plane of the polymer film orthogonal to the first direction to a dielectric loss tangent in a first direction in the plane of the polymer film is 0.5 to 1.
5.
8. The polymer film according to claim 1 or 2, wherein: The ratio of the dielectric constant in a second direction in the plane of the polymer film orthogonal to the first direction to the dielectric constant in a first direction in the plane of the polymer film is 0.5 to 1.
5.
9. The polymer film according to claim 1 or 2, wherein: The ratio of the linear expansion coefficient in a second direction in the plane of the polymer film orthogonal to the first direction to the linear expansion coefficient in a first direction in the plane of the polymer film is 0.5 to 1.
8.
10. The polymer film according to claim 1 or 2, wherein: The surface of the polymer film has an arithmetic mean surface roughness Ra of 400 nm or less.
11. The polymer film according to claim 1 or 2, which has a thickness of 5 μm to 1100 μm. 12 . A communication substrate comprising the polymer film according to claim 1 .