Semiconductor structure and its fabrication method, three-dimensional memory

By setting a heat insulation layer on the semiconductor layer, the heat of annealing is concentrated, which solves the problem of thermal deformation of the semiconductor layer, improves the annealing efficiency and the performance of the semiconductor structure, especially the reliability of CMOS circuits.

CN115346991BActive Publication Date: 2026-11-10YANGTZE MEMORY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211007856.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-22
Publication Date
2026-11-10
Estimated Expiration
2042-08-22

AI Technical Summary

Technical Problem

The first semiconductor layer is prone to thermal deformation during annealing, which affects the performance of the semiconductor structure and the stability of the internal CMOS circuit.

Method used

A thermal insulation layer is set on the semiconductor layer to form a stacked structure and a channel structure. The thermal insulation layer concentrates the heat of the annealing process on the side away from the semiconductor layer, preventing heat from being conducted to the semiconductor layer. Laser annealing is used to improve the annealing efficiency.

Benefits of technology

It effectively prevents thermal expansion deformation of the semiconductor layer, improves annealing efficiency, enhances the stability of semiconductor structures and CMOS circuits, and improves overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115346991B_ABST
    Figure CN115346991B_ABST
Patent Text Reader

Abstract

This disclosure provides a semiconductor structure and its fabrication method, as well as a three-dimensional memory, relating to the field of semiconductor chip technology, and aims to solve the problem of easy thermal deformation of the first semiconductor layer. The semiconductor structure includes a first semiconductor layer, a thermal insulation layer, a stacked structure, and a channel structure. The thermal insulation layer is located on a first surface of the first semiconductor layer. The stacked structure is located on a second surface of the thermal insulation layer, the second surface being away from the first surface of the first semiconductor layer. The stacked structure includes alternately stacked dielectric layers and a first electrode layer. The channel structure penetrates the stacked structure. The channel structure includes a ferroelectric thin film layer, a second electrode layer, and the channel layer. The ferroelectric thin film layer and the second electrode layer are located between the stacked structure and the channel layer, with the ferroelectric thin film layer being closer to the stacked structure than the second electrode layer. The above semiconductor structure is applied in a three-dimensional memory to realize data read and write operations.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to the field of semiconductor chip technology, and in particular to a semiconductor structure and its fabrication method, a three-dimensional memory, a storage system, and an electronic device. Background Technology

[0002] Ferroelectric random access memory (FeRAM), as a new type of memory, is increasingly being used due to its advantages over traditional dynamic random access memory (DRAM), such as non-volatility, high speed, and low power consumption. Summary of the Invention

[0003] The embodiments of this disclosure provide a semiconductor structure and its fabrication method, as well as a three-dimensional memory, aimed at solving the problem that the first semiconductor layer is easily deformed by heat.

[0004] To achieve the above objectives, the embodiments of this disclosure adopt the following technical solutions:

[0005] On one hand, a semiconductor structure is provided. The semiconductor structure includes a first semiconductor layer, a thermal insulation layer, a stacked structure, and a channel structure. The thermal insulation layer is located on a first surface of the first semiconductor layer. The stacked structure is located on a second surface of the thermal insulation layer, the second surface being away from the first surface of the first semiconductor layer. The stacked structure includes alternately stacked dielectric layers and a first electrode layer. The channel structure extends through the stacked structure. The channel structure includes a ferroelectric thin film layer, a second electrode layer, and a channel layer. The ferroelectric thin film layer and the second electrode layer are located between the stacked structure and the channel layer.

[0006] The semiconductor structure provided in the above embodiments of this disclosure includes a thermal insulation layer above a first semiconductor layer. A stacked structure and a channel structure are then formed on the thermal insulation layer. That is, a thermal insulation layer is provided between the first semiconductor layer and the channel structure. During subsequent annealing of the ferroelectric thin film layer, the thermal insulation layer can concentrate the heat generated during annealing on the side of the thermal insulation layer away from the first semiconductor layer, preventing the heat from being conducted to the first semiconductor layer. On the one hand, by concentrating heat on the side of the thermal insulation layer away from the first semiconductor layer, i.e., concentrating heat on the ferroelectric thin film layer, the required temperature for annealing of the ferroelectric thin film layer can be reached more quickly, improving the efficiency of the annealing process. On the other hand, the thermal insulation layer can prevent heat conduction to the first semiconductor layer. This can prevent deformation caused by thermal expansion of the first semiconductor layer, which could affect the stability of the film layer above the first semiconductor layer. This is beneficial for improving the performance of the semiconductor structure.

[0007] In some embodiments, the second electrode layer is located between the ferroelectric thin film layer and the channel layer.

[0008] In some embodiments, the material of the insulation layer includes at least one of silicon dioxide, polyimide, or borosilicate.

[0009] In some embodiments, the thickness of the insulation layer ranges from 100 nm to 200 nm.

[0010] In some embodiments, the material of the ferroelectric thin film layer includes hafnium-based ferroelectric materials.

[0011] In some embodiments, the semiconductor structure further includes a circuit layer. The circuit layer is located within the first semiconductor layer. The second electrode layer is coupled to the circuit layer through vias in the ferroelectric thin film layer and vias in the thermal insulation layer.

[0012] On the other hand, a method for fabricating a semiconductor structure is provided, comprising:

[0013] A thermal insulation layer is formed on the first surface of the first semiconductor layer;

[0014] A stacked structure is formed on the second surface of the thermal insulation layer, the second surface being away from the first surface of the first semiconductor layer; the stacked structure includes alternately stacked dielectric layers and first electrode layers;

[0015] A channel structure is formed that runs through the stacked structure. The channel structure includes a ferroelectric thin film layer, a second electrode layer, and a channel layer. The ferroelectric thin film layer and the second electrode layer are located between the stacked structure and the channel layer. The ferroelectric thin film layer is closer to the stacked structure than the second electrode layer.

[0016] A protective layer is formed covering the channel structure and the stacked structure.

[0017] On the side of the protective layer away from the ferroelectric thin film layer, the ferroelectric thin film layer is annealed.

[0018] In some embodiments, the annealing process is laser annealing.

[0019] In some embodiments, the laser annealing process includes 20 to 50 laser irradiations, each lasting 100 to 250 ns.

[0020] In some embodiments, the energy range of the laser annealing treatment is 0.3 J / cm². 2 ~2J / cm 2 .

[0021] In some embodiments, the temperature range of the laser annealing is 800°C to 1400°C.

[0022] In some embodiments, the thickness of the protective layer ranges from 60 nm to 150 nm.

[0023] In some embodiments, the material of the protective layer includes polycrystalline silicon or amorphous silicon.

[0024] In another aspect, a three-dimensional memory is provided. The three-dimensional memory includes the semiconductor structure described in some of the embodiments above.

[0025] In another aspect, a storage system is provided, comprising: a three-dimensional memory as described above, and a controller coupled to the three-dimensional memory to control the three-dimensional memory to store data.

[0026] On the other hand, an electronic device is provided, including the storage system described above.

[0027] It is understood that the beneficial effects that the semiconductor structure fabrication method, three-dimensional memory, storage system and electronic device provided in the above embodiments of this disclosure can achieve can be referred to the beneficial effects of the semiconductor structure above, and will not be repeated here. Attached Figure Description

[0028] To more clearly illustrate the technical solutions in this disclosure, the accompanying drawings used in some embodiments of this disclosure will be briefly described below. Obviously, the drawings described below are only drawings of some embodiments of this disclosure, and those skilled in the art can obtain other drawings based on these drawings. In addition, the drawings described below can be regarded as schematic diagrams and are not intended to limit the actual size of the product, the actual flow of the method, the actual timing of the signals, etc. involved in the embodiments of this disclosure.

[0029] Figure 1 This is a schematic diagram of the three-dimensional structure of a three-dimensional memory according to some embodiments;

[0030] Figure 2 for Figure 1 A cross-sectional view of a string of storage cells in a three-dimensional memory along section line AA';

[0031] Figure 3A This is a schematic diagram of a semiconductor structure provided according to some embodiments;

[0032] Figure 3B This is a schematic diagram of a semiconductor structure provided according to some other embodiments;

[0033] Figure 4A This is a schematic diagram of a semiconductor structure provided according to some other embodiments;

[0034] Figure 4BThis is a schematic diagram of a semiconductor structure provided according to some other embodiments;

[0035] Figure 5A This is a flowchart of a method for fabricating a semiconductor structure according to some embodiments;

[0036] Figures 5B to 5G for Figure 5A Structural diagrams corresponding to some steps in the process;

[0037] Figure 6A This is a simulation diagram of temperature changes in a semiconductor structure provided according to some embodiments;

[0038] Figure 6B A simulation diagram of temperature changes of a semiconductor structure according to some other embodiments;

[0039] Figure 6C A simulation diagram of temperature changes of a semiconductor structure according to some other embodiments;

[0040] Figure 6D A simulation diagram showing the energy density variation of a semiconductor structure according to some other embodiments;

[0041] Figure 7 This is a block diagram of a storage system according to some embodiments;

[0042] Figure 8 This is a block diagram of a storage system according to some other embodiments. Detailed Implementation

[0043] The technical solutions in some embodiments of this disclosure will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this disclosure, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments provided in this disclosure are within the scope of protection of this disclosure.

[0044] In the description of this disclosure, it should be understood that the terms “center,” “upper,” “lower,” “front,” “rear,” “left,” “right,” “vertical,” “horizontal,” “top,” “bottom,” “inner,” and “outer,” etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing this disclosure and simplifying the description, and are not intended to indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this disclosure.

[0045] Unless the context otherwise requires, throughout the specification and claims, the term "comprising" is interpreted as open-ended and encompassing, meaning "including, but not limited to." In the description of the specification, terms such as "one embodiment," "some embodiments," "exemplary embodiment," "illustrated," or "some examples" are intended to indicate that a particular feature, structure, material, or characteristic associated with that embodiment or example is included in at least one embodiment or example of this disclosure. The illustrative representations of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics mentioned may be included in any suitable manner in any one or more embodiments or examples.

[0046] Hereinafter, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of embodiments of this disclosure, unless otherwise stated, "a plurality of" means two or more.

[0047] In describing some embodiments, the terms "coupled" and "connected," and their derivative expressions, may be used. For example, the term "connected" may be used in describing some embodiments to indicate that two or more components have direct physical or electrical contact with each other. Similarly, the term "coupled" may be used in describing some embodiments to indicate that two or more components have direct physical or electrical contact. However, the term "coupled" may also refer to two or more components that do not have direct contact with each other but still cooperate or interact with each other. The embodiments disclosed herein are not necessarily limited to the content of this document.

[0048] "At least one of A, B and C" has the same meaning as "at least one of A, B or C", both including the following combinations of A, B and C: only A, only B, only C, combinations of A and B, combinations of A and C, combinations of B and C, and combinations of A, B and C.

[0049] As used herein, “about” includes the value stated and the average value within an acceptable range of deviation from the given value, wherein the acceptable range of deviation is determined by a person skilled in the art taking into account the measurement under discussion and the error associated with the measurement of the given quantity (i.e., the limitations of the measurement system).

[0050] In this disclosure, the meanings of “on,” “above,” and “above” should be interpreted in the broadest possible sense, such that “on” means not only “directly on” something, but also includes “on” something with intermediate features or layers in between, and that “above” or “above” means not only “above” or “above” something, but also “above” or “above” something without intermediate features or layers in between (i.e., directly on something).

[0051] This document describes exemplary embodiments with reference to cross-sectional views and / or plan views, which are idealized exemplary drawings. In the drawings, the thickness of layers and regions is enlarged for clarity. Therefore, variations in shape relative to the drawings are contemplated due to, for example, manufacturing techniques and / or tolerances. Thus, exemplary embodiments should not be construed as limited to the shapes of the regions shown herein, but rather include shape deviations due to, for example, manufacturing processes. For example, etched regions shown as rectangular would typically have curved features. Therefore, the regions shown in the drawings are schematic in nature, and their shapes are not intended to show the actual shapes of the regions of the device, nor are they intended to limit the scope of the exemplary embodiments.

[0052] As used herein, the term "substrate" refers to a material on which subsequent material layers can be added. The substrate itself may be patterned. The material added to the substrate may be patterned or may remain unpatterned. Furthermore, the substrate may include a variety of semiconductor materials such as silicon, germanium, gallium arsenide, indium phosphide, etc. Alternatively, the substrate may be made of a non-conductive material such as glass, plastic, or sapphire wafer.

[0053] The term "three-dimensional memory" refers to a semiconductor device formed by arrays of memory cell transistors (referred to herein as "memory cell strings," e.g., ferroelectric memory cell strings, FeRAM) arranged in an array on the main surface of a substrate or source layer and extending in a direction perpendicular to the substrate or source layer. As used herein, the term "perpendicularly" means nominally perpendicular to the main surface of the substrate or source layer (i.e., the lateral surface).

[0054] Figure 1 This is a schematic diagram of the three-dimensional structure of a three-dimensional memory provided in some embodiments of this disclosure. Figure 2 for Figure 1 A cross-sectional view of a storage cell string in a three-dimensional memory along section line AA'.

[0055] It should be noted that, in Figure 1In this embodiment, the three-dimensional memory 200 extends in the XY plane. The first direction X and the second direction Y are, for example, two orthogonal directions in the plane where the semiconductor structure 100 is located (e.g., the plane where the source layer SL is located): the first direction X is, for example, the extension direction of the word line WL, and the second direction Y is, for example, the extension direction of the bit line BL. The third direction Z is perpendicular to the plane where the semiconductor structure 100 is located, that is, perpendicular to the XY plane.

[0056] As used in this disclosure, whether a component (e.g., a layer, structure, or device) is "on," "above," or "below" another component (e.g., a layer, structure, or device) of a semiconductor device (e.g., a three-dimensional memory) is determined relative to the substrate or source layer of the semiconductor device in the third direction Z, when the substrate or source layer is located in the lowest plane of the semiconductor device in the third direction Z. The same concepts are applied throughout this disclosure to describe spatial relationships.

[0057] See Figure 1 Some embodiments of this disclosure provide a three-dimensional memory 200. The three-dimensional memory 200 may include a semiconductor structure 100. The three-dimensional memory 200 may also include a source layer SL coupled to the semiconductor structure 100.

[0058] The source layer SL may include a semiconductor material, such as single-crystal silicon, single-crystal germanium, group III-V compound semiconductor materials, group II-VI compound semiconductor materials, and other suitable semiconductor materials. The source layer SL may be partially or completely doped. For example, the source layer SL may include doped regions doped with p-type dopant. The source layer SL may also include undoped regions.

[0059] Semiconductor structure 100 may include arrayed strings of memory cell transistors (referred herein to as "ferroelectric memory cell strings," such as ferroelectric memory cell strings FeRAM) 300. Source layer SL may be coupled to the source ends of multiple ferroelectric memory cell strings 300.

[0060] Specifically, see Figure 2 The ferroelectric memory cell string 300 may include multiple ferroelectric memory cells T. These ferroelectric memory cells T are connected together to form a ferroelectric memory cell string.

[0061] It should be noted that, Figure 1 and Figure 2 The number of ferroelectric storage cells is only illustrative. The ferroelectric storage cell string of the three-dimensional memory provided in this embodiment may also include other numbers of ferroelectric storage cells, such as 4, 16, 32, and 64.

[0062] Furthermore, the ferroelectric memory cell string 300 may also include a first electrode layer G (gate electrode), a source selection gate, and a drain selection gate. Multiple first electrode layers G (gate electrodes) may also be configured as multiple word lines WL. By writing different voltages onto the word lines WL, data writing, reading, and erasing of each ferroelectric memory cell in the ferroelectric memory cell string 300 can be accomplished. Along the third direction Z, the source selection gate may be located on the side of the lowermost first electrode G closest to the gate line of the source layer SL. The source selection gate is configured to control the conduction state of the first selection transistor, thereby controlling the conduction state of the source channel in the ferroelectric memory cell string 300. Along the third direction Z, the drain selection gate may be located on the side of the uppermost first electrode G away from the source layer SL. The drain selection gate is configured to control the conduction state of the second selection transistor, thereby controlling the conduction state of the drain channel in the memory cell string.

[0063] See also Figure 1 and Figure 2 In some embodiments, the semiconductor structure 100 may further include an array interconnect layer 290. The array interconnect layer 290 may be coupled to the ferroelectric memory cell string 300. The array interconnect layer 290 may include the drain (i.e., bit line BL) of the ferroelectric memory cell string 300, which may be coupled to the semiconductor channel of each ferroelectric memory cell T in at least one ferroelectric memory cell string 300.

[0064] The array interconnect layer 290 may include one or more first interlayer insulating layers, and may also include a plurality of contacts insulated from each other by these first interlayer insulating layers. The contacts may include, for example, a bit line contact BL-CNT coupled to the bit line BL, and a drain select gate contact SGD-CNT coupled to the drain select gate. The array interconnect layer 290 may also include one or more first interconnect conductor layers. The first interconnect conductor layer may include multiple interconnect lines, such as the bit line BL, and word line interconnect lines WL-CL coupled to the word line WL. The materials of the first interconnect conductor layers and the contacts may be conductive materials, such as tungsten, cobalt, copper, aluminum, and combinations of one or more metal silicides, or other suitable materials. The materials of the first interlayer insulating layers are insulating materials, such as silicon oxide, silicon nitride, and combinations of one or more high-dielectric-constant insulating materials, or other suitable materials.

[0065] Figure 3A This is a schematic diagram of a semiconductor structure provided according to some embodiments. Figure 3B This is a schematic diagram of a semiconductor structure provided according to some other embodiments.

[0066] In some embodiments, such as Figure 3A and Figure 3BAs shown, the semiconductor structure 100 includes a first semiconductor layer 10, a thermal insulation layer 20, and a ferroelectric memory cell T. Wherein, Figure 3A The following is an illustration of a semiconductor structure 100 including one ferroelectric memory cell T. Figure 3B The semiconductor structure includes multiple ferroelectric memory cells T connected in series along a direction perpendicular to the first semiconductor layer 10, forming a ferroelectric memory cell string 300. In this embodiment, the number of ferroelectric memory cells T in the semiconductor structure 100 is not limited and can be set according to actual conditions.

[0067] In some embodiments, such as Figure 3A As shown, the semiconductor structure 100 includes a first semiconductor layer 10, a thermal insulation layer 20, a stacked structure 30, and a channel structure 40. The stacked structure 30 and the channel structure 40 form at least one ferroelectric memory cell T.

[0068] The first semiconductor layer 10 may be a substrate. The material of the first semiconductor layer 10 may include single-crystal silicon (Si), single-crystal germanium (Ge), gallium arsenide, indium phosphide, III-V compound semiconductor materials, II-VI compound semiconductor materials, or at least one of other semiconductor materials known in the art. Alternatively, the first semiconductor layer 10 may also be made of a non-conductive material such as glass, plastic, or sapphire wafer.

[0069] In some examples, such as Figure 3A As shown, between the formation of the thermal insulation layer 20 on the first semiconductor layer 10, a complementary metal-oxide-semiconductor (CMOS) circuit, hereinafter referred to as a CMOS circuit, can be formed within the first semiconductor layer 10. In some examples, the CMOS circuit may also be located outside the semiconductor structure 100.

[0070] The stacked structure 30 is located on one side of the first semiconductor layer 10. The stacked structure 30 includes alternating dielectric layers 31 and a first electrode layer G.

[0071] In some examples, such as Figure 3A As shown, the material of dielectric layer 31 may include an insulating material. Insulating materials may be, for example, one or more combinations of silicon oxide, silicon nitride, silicon oxynitride, doped silicon oxide, organosilicon glass, dielectric metal oxides (e.g., aluminum oxide, hafnium dioxide, etc.) and their silicates, and organic insulating materials. The materials of each dielectric layer 31 may be the same or different. For example, the materials of each dielectric layer 31 are the same, and all are silicon oxide.

[0072] In some examples, such as Figure 3AAs shown, the material of the first electrode layer G may include polycrystalline silicon.

[0073] In some examples, such as Figure 3A As shown, a stacked structure 30 can be formed on the first surface V1 of the first semiconductor layer 10 using a thin film deposition process. For example, the thin film deposition process may include one or a combination of chemical vapor deposition (CVD), physical vapor deposition (PVD), and atomic layer deposition (ALD).

[0074] In the embodiments of this disclosure, the number of layers in the stacking structure 30 is not limited. For example, the number of layers in the stacking structure can be 8, 64, 128, etc. The more layers in the stacking structure 30, the higher the integration density of the ferroelectric memory cell string 300, and the more ferroelectric memory cells it forms.

[0075] The channel structure 40 extends through the stacked structure 30. The channel structure 40 includes a ferroelectric thin film layer 41, a second electrode layer P, and a channel layer 42. The ferroelectric thin film layer 41 and the second electrode layer P are located between the stacked structure 30 and the channel layer 42.

[0076] In some examples, such as Figure 3A As shown, the material of the ferroelectric thin film layer 41 includes hafnium-based ferroelectric materials.

[0077] In other examples, to improve the ferroelectric properties of the ferroelectric thin film layer 41, the hafnium-based ferroelectric material can be doped. For example, the material of the ferroelectric thin film layer 41 may include hafnium oxide (HfO2) doped with one or any combination of silicon (Si), aluminum (Al), or zirconium (Zr). This disclosure does not specifically limit the doping material of the ferroelectric thin film layer 41; it can be adjusted according to actual needs.

[0078] In some examples, such as Figure 3A As shown, the material of the second electrode layer P may include titanium nitride (TiN). In other examples, the material of the second electrode layer P may also be tantalum nitride (TaN) or platinum (Pt).

[0079] In some examples, such as Figure 3A As shown, the material of the channel layer 42 may include tungsten (W). The channel layer 42 can be used to connect to the bit line BL.

[0080] In this embodiment, the materials of the second electrode layer P and the channel layer 42 are not specifically limited; the above is merely illustrative.

[0081] In some examples, each ferroelectric memory cell T in the ferroelectric memory cell string 300 includes a first electrode layer G, a second electrode layer P, and a ferroelectric thin film layer 41.

[0082] The ferroelectric storage cell T stores data based on the ferroelectric effect of the ferroelectric material in the ferroelectric thin film layer 41. For example, the basic storage principle of hafnium-based ferroelectric materials currently relies on the change in the position of its oxygen atoms, which results in different polarization directions of electric dipoles. Whether the polarization is reversed or not during reading will result in different current magnitudes, which can represent "0" and "1" in the stored data.

[0083] In some feasible methods, after forming the ferroelectric thin film layer 41, an annealing treatment is required. This involves using an annealing process during the preparation of the ferroelectric thin film layer 41 material to crystallize the amorphous hafnium oxide material into a ferroelectric orthorhombic hafnium oxide. For example, the ferroelectric phase exhibiting ferroelectricity in hafnium-based ferroelectric materials is the orthorhombic (O-phase) Pca21 space group.

[0084] However, on the one hand, the Pca21 space group in hafnium-based ferroelectric materials needs to be obtained through annealing and crystallization, which requires high annealing temperatures and rapid heating and cooling rates. This can easily lead to thermal expansion of the first semiconductor layer 10, affecting the stability of other films formed on the first semiconductor layer 10 and potentially impacting the performance of the semiconductor structure 100. For example, when the first semiconductor layer 10 includes CMOS circuitry, the high-temperature environment can also affect the performance of the CMOS circuitry, thereby reducing the performance of the semiconductor structure 100.

[0085] In this embodiment, the semiconductor structure 100 further includes a thermal insulation layer 20. The thermal insulation layer 20 is located on the second surface V2 of the first semiconductor layer 10. The stacked structure 30 and the channel structure 40 are formed on the second surface V2 of the thermal insulation layer 20, which is away from the first surface V1 of the first semiconductor layer 10. That is, the thermal insulation layer 20 is disposed between the first semiconductor layer 10 and the stacked structure 30 and the channel structure 40. The thermal insulation layer 20 can concentrate the heat generated during the annealing process on the side of the thermal insulation layer 20 away from the first semiconductor layer 10, preventing the heat from being conducted to the first semiconductor layer 10. On the one hand, the thermal insulation layer 20 concentrates the heat on the side of the thermal insulation layer away from the first semiconductor layer 10, that is, concentrates the heat on the ferroelectric thin film layer 41. The temperature required by the ferroelectric thin film layer 41 during the annealing process can be reached more quickly, improving the efficiency of the annealing process. On the other hand, the thermal insulation layer 20 can prevent the heat from being conducted to the first semiconductor layer 10. This can prevent deformation caused by thermal expansion of the first semiconductor layer 10, which could affect the stability of the film layer above the first semiconductor layer. This is beneficial to improving the performance of the semiconductor structure 100.

[0086] Furthermore, when CMOS circuitry is included in the first semiconductor layer 10, the thermal insulation layer 20 is located on the first surface V1 of the first semiconductor layer 10. This also prevents the CMOS circuitry from failing due to high temperatures. This solves the problem of thermal budget limitation in the circuit region of the first semiconductor layer 10 in the semiconductor structure 100, which is beneficial for improving the performance of the semiconductor structure 100 and the reliability of its internal CMOS circuitry.

[0087] In some embodiments, continue as follows Figure 3A As shown, with the ferroelectric thin film layer 41 and the second electrode layer P located between the stacked structure 30 and the channel layer 42, the second electrode layer P is positioned between the ferroelectric thin film layer 41 and the channel layer 42. That is, the channel structure 40 includes the channel layer 42, the second electrode layer P, and the ferroelectric thin film layer 41 from the inside out.

[0088] In some examples, forming the channel structure 40 may include forming a channel hole by an etching process, and then forming the channel structure 40 within the channel hole by a thin film deposition process. For example, a ferroelectric thin film layer 41, a second electrode layer P, and a channel layer 42 may be formed within the channel hole, i.e., on the sidewall of the stacked structure 30, by a thin film deposition process.

[0089] In some embodiments, continue as follows Figure 3A As shown, the material of the thermal insulation layer 20 includes at least one of silicon dioxide (SiO2), polyimide (PI), or borosilicate. Since silicon dioxide, polyimide, and borosilicate all have extremely low thermal conductivity and coefficients of thermal expansion, they can effectively provide thermal insulation. This allows the heat generated during the annealing process to be concentrated on the side of the thermal insulation layer 20 away from the first semiconductor layer 10, preventing the heat from being conducted to the first semiconductor layer 10. This improves the efficiency of the annealing process while preventing the first semiconductor layer 10 from deforming due to thermal expansion.

[0090] It is understood that in other embodiments, the material of the insulation layer 20 may also be other materials with low thermal conductivity. This disclosure does not specifically limit the material of the insulation layer 20.

[0091] In some embodiments, continue as follows Figure 3A As shown, the thickness of the insulation layer 20 ranges from 100nm to 200nm.

[0092] In some examples, when the thickness of the insulation layer 20 is equal to or close to 100nm to 150nm, it can achieve the insulation effect while preventing the insulation layer 20 from being too thick, wasting resources, and hindering the subsequent drilling process. When the thickness of the insulation layer 20 is equal to or close to 150nm to 200nm, it can achieve the insulation effect better while preventing the insulation layer 20 from being too thick, wasting resources, and hindering the subsequent drilling process.

[0093] In other examples, when the thickness of the insulation layer 20 is equal to or close to 100 nm, it is possible to achieve a thinner semiconductor structure while providing insulation. When the thickness of the insulation layer 20 is equal to or close to 200 nm, it is possible to achieve a better insulation effect while preventing the insulation layer 20 from being too thick, wasting resources, and hindering subsequent drilling processes.

[0094] For example, the thickness of the thermal insulation layer 20 can be approximately 100nm, 120nm, 140nm, 150nm, 160nm, 180nm, or 200nm. The specific value of the thickness of the thermal insulation layer 20 in this embodiment is not limited and can be adjusted according to the parameters of the laser used in actual laser annealing.

[0095] In addition, it should be noted that due to certain uncontrollable errors (such as manufacturing process errors, equipment precision, measurement errors, etc.), when the thickness fluctuation range of the insulation layer 20 does not exceed 10% of the thickness H3 of the insulation layer 20, the insulation layer 20 can also be considered to meet the equality constraint.

[0096] In some embodiments, continue as follows Figure 3A and Figure 3B As shown, the material of the ferroelectric thin film layer 41 includes hafnium-based ferroelectric materials.

[0097] In some examples, such as Figure 3A As shown, the ferroelectric storage cell T includes a ferroelectric capacitor. (As...) Figure 3B As shown, the ferroelectric memory cell string (FeRAM) 400 includes multiple ferroelectric capacitors connected in series. Each ferroelectric capacitor includes a first electrode layer G, a second electrode layer P, and a ferroelectric thin film layer 41 formed between the first electrode layer G and the second electrode layer P for storing data information.

[0098] When a ferroelectric capacitor is working, it can change the polarity of the hafnium-based ferroelectric material according to the electric field formed between the first electrode layer G and the second electrode layer P, and store "0" and "1" according to the polarization direction.

[0099] For example, when a positive write voltage is applied to the first electrode layer G, the ferroelectric thin film layer 41 becomes polarized and stores the logic value "1". When a negative write voltage is applied to the first electrode layer G, the ferroelectric thin film layer 41 becomes depolarized and stores the logic value "0".

[0100] In other embodiments, to improve the ferroelectric properties of the ferroelectric thin film layer 41, the hafnium-based ferroelectric material can be doped. For example, the material of the ferroelectric thin film layer 41 may include hafnium oxide (HfO2) doped with one or any combination of silicon (Si), aluminum (Al), or zirconium (Zr). This disclosure does not specifically limit the doping material of the ferroelectric thin film layer 41; it can be adjusted according to actual needs.

[0101] In some examples, such as Figure 3A As shown, the ferroelectric memory cell T includes a ferroelectric transistor. (As...) Figure 3B As shown, the ferroelectric memory cell string (FeRAM) 400 includes multiple ferroelectric transistors connected in series. For example, a first electrode layer G, a ferroelectric thin film layer 41, a second electrode layer P, and a channel layer 42 together form multiple ferroelectric transistors connected in series. The gate and channel layer 42 of the ferroelectric transistors are separated by the ferroelectric thin film layer 41.

[0102] The source and drain of the ferroelectric memory cell string (FeRAM) 400 are located at the top and bottom ends of the ferroelectric memory cell string (FeRAM) 400, respectively. For example, the source of the ferroelectric memory cell string (FeRAM) 400 is located at the end of the second electrode layer P closest to the first semiconductor layer 10. The drain of the ferroelectric memory cell string (FeRAM) 400 is located at the end of the second electrode layer P furthest from the first semiconductor layer 10.

[0103] The channel layer 42 is part of the ferroelectric transistor. Its resistance can be changed by altering the polarization in the ferroelectric thin film layer 41 through the voltage applied to the first electrode layer G, thereby enabling conduction and cutoff, and thus storing and accessing data.

[0104] For example, the first electrode layer G, the second electrode layer P, and the channel layer 42 are all film structures. For instance, they can be formed by processes such as deposition or sputtering, rather than by doping in the first semiconductor layer. In this way, the ferroelectric memory cell T can be 3D stacked on the first semiconductor layer 10, achieving high-density integration of the ferroelectric memory cell.

[0105] Figure 4A This is a schematic diagram of a semiconductor structure provided according to some other embodiments. Figure 4B This is a schematic diagram of a semiconductor structure provided according to some other embodiments.

[0106] In other embodiments, such as Figure 4A and Figure 4B As shown, the semiconductor structure 100 also includes a circuit layer 50. The circuit layer 50 is located within the first semiconductor layer 10. The second electrode layer P is coupled to the circuit layer 50 through vias in the ferroelectric thin film layer 41 and the thermal insulation layer 20.

[0107] Circuit layer 50 is configured to control and sense the array device. Circuit layer 50 can be any suitable digital, analog, and / or mixed-signal control and sensing circuitry used to support the operation (or function) of the array device, including but not limited to page buffers, decoders (e.g., row decoders and column decoders), sense amplifiers, drivers (e.g., word line drivers), charge pumps, current or voltage references, or any active or passive components of the circuitry (e.g., transistors, diodes, resistors, or capacitors). Circuit layer 50 may also include any other circuitry compatible with advanced logic processes, including logic circuitry (e.g., processors and programmable logic devices (PLDs)) or memory circuitry (e.g., static random-access memory (SRAM)).

[0108] In some examples, circuit layer 50 may include complementary metal-oxide-semiconductor (CMOS) circuitry, hereinafter referred to as CMOS circuitry. Circuit layer 50 may also include source lines SL. When CMOS circuitry is included in the first semiconductor layer 10, a thermal insulation layer 20 is located on the first surface V1 of the first semiconductor layer 10. This also prevents the CMOS circuitry from experiencing high-temperature performance failure. This is beneficial for improving the performance of the semiconductor structure 100 and the reliability of its internal CMOS circuitry.

[0109] The source line SL is located on the side of the CMOS circuit near the channel structure 40. The source line SL can be connected to both the second electrode layer P and the CMOS circuit. For example, the source line SL can be coupled to the second electrode layer P through via K1. The source line SL can be coupled to the CMOS circuit through via K2. This enables the transmission of electrical signals between the circuit layer 50 and the ferroelectric memory cell string 300 in the semiconductor structure 100.

[0110] For example, a CMOS circuit includes at least one transistor. Any transistor includes a gate, a source, and a drain, wherein the definitions of the source and drain in a CMOS circuit can be interchanged. The following description is only one example. For instance, the source line SL can be connected to the source of the transistor in the CMOS circuit through a via K2, but it is not limited to being connected to the source. In other embodiments, it can also be connected to the drain of the transistor in the CMOS circuit.

[0111] In some examples, such as Figure 4A As shown, the source line SL can be located between the thermal insulation layer 20 and the ferroelectric thin film layer 41. The source line SL can be coupled to the second electrode layer P through the via K1a on the ferroelectric thin film layer 41. Since the number of film layers between the source line SL and the second electrode layer P is small, it simplifies the formation of the via K1a and facilitates the drilling process.

[0112] In other examples, such as Figure 4B As shown, the source line SL can be located within the thermal insulation layer 20, and the source line SL can be coupled to the second electrode layer P through the via K1b. The via K1b penetrates the ferroelectric thin film layer 41 and part of the thermal insulation layer 20 until the source line SL is exposed.

[0113] The source line SL can be located within the thermal insulation layer 20. On one hand, the thermal insulation layer 20 can simultaneously protect the source line SL, preventing its performance from being affected by high temperatures and thus reducing the performance of the semiconductor structure 100. On the other hand, the via K1b penetrates the ferroelectric thin film layer 41 and part of the thermal insulation layer 20. The relatively small number of film layers between the source line SL and the second electrode layer P simplifies the formation of the via K1b and facilitates the drilling process. Simultaneously, the source line SL can be coupled to the source S of the CMOS circuit through the via K2, which exposes the CMOS circuit by penetrating part of the thermal insulation layer 20. The partial thermal insulation layer separating the source line SL and the CMOS circuit reduces the thickness of the film layers between them, further simplifying the formation of the via K2 and facilitating the drilling process.

[0114] In some other embodiments, the circuit layer 50 is located outside the semiconductor structure 100. For example, the circuit layer 50 may be located on the side of the channel structure 40 away from the first semiconductor layer 10 and coupled to the channel layer 42. The specific location of the circuit layer 50 is not limited in the embodiments of this disclosure and can be adjusted according to actual needs.

[0115] Figure 5A This is a flowchart of a method for fabricating a semiconductor structure according to some embodiments. Figures 5B to 5G for Figure 5A The structural diagrams corresponding to some of the steps are shown.

[0116] In some embodiments, such as Figure 5A and Figure 5B As shown, this embodiment provides a method for fabricating a semiconductor structure, including:

[0117] S1: A thermal insulation layer is formed on the first surface of the first semiconductor layer.

[0118] Before step S1, the first semiconductor layer 10 is formed.

[0119] In some examples, the material of the first semiconductor layer 10 may include single-crystal silicon (Si), single-crystal germanium (Ge), gallium arsenide, indium phosphide, III-V compound semiconductor materials, II-VI compound semiconductor materials, or at least one of other semiconductor materials known in the art. Alternatively, the first semiconductor layer 10 may also be made of a non-conductive material such as glass, plastic, or sapphire wafer.

[0120] In step S1, as Figure 5B As shown in S1, a thermal insulation layer 20 is formed on the first surface V1 of the first semiconductor layer 10.

[0121] In some examples, a thin-film deposition process can be used to form the thermal insulation layer 20 on the first semiconductor layer 10. For example, the thin-film deposition process may include one or a combination of chemical vapor deposition (CVD), physical vapor deposition (PVD), and atomic layer deposition (ALD).

[0122] In some examples, the material of the thermal insulation layer 20 includes silicon dioxide. Since silicon dioxide (SiO2) has extremely low thermal conductivity and coefficient of thermal expansion, it provides excellent thermal insulation. This allows the heat generated during the annealing process to be concentrated on the side of the thermal insulation layer 20 away from the first semiconductor layer 10, preventing the heat from being conducted to the first semiconductor layer 10. This improves the efficiency of the annealing process while preventing the first semiconductor layer 10 from deforming due to thermal expansion.

[0123] It is understood that in some embodiments, the material of the insulation layer 20 may be other materials with lower thermal conductivity. This disclosure does not specifically limit the material of the insulation layer 20.

[0124] In some examples, the thickness of the insulation layer 20 ranges from 100 nm to 200 nm.

[0125] In some examples, when the thickness of the insulation layer 20 is equal to or close to 100nm to 150nm, it can achieve the insulation effect while preventing the insulation layer 20 from being too thick, wasting resources, and hindering the subsequent drilling process. When the thickness of the insulation layer 20 is equal to or close to 150nm to 200nm, it can achieve the insulation effect better while preventing the insulation layer 20 from being too thick, wasting resources, and hindering the subsequent drilling process.

[0126] In other examples, when the thickness of the insulation layer 20 is equal to or close to 100 nm, it is possible to achieve a thinner semiconductor structure while providing insulation. When the thickness of the insulation layer 20 is equal to or close to 200 nm, it is possible to achieve a better insulation effect while preventing the insulation layer 20 from being too thick, wasting resources, and hindering subsequent drilling processes.

[0127] For example, the thickness of the thermal insulation layer 20 can be approximately 100nm, 120nm, 140nm, 150nm, 160nm, 180nm, or 200nm. The specific value of the thickness of the thermal insulation layer 20 in this embodiment is not limited and can be adjusted according to the parameters of the laser used in actual laser annealing.

[0128] In addition, it should be noted that due to certain uncontrollable errors (such as manufacturing process errors, equipment precision, measurement errors, etc.), when the thickness fluctuation range of the insulation layer 20 does not exceed 10% of the thickness H3 of the insulation layer 20, the insulation layer 20 can also be considered to meet the equality constraint.

[0129] S2: A stacked structure is formed on the second surface of the thermal insulation layer, the second surface being away from the first surface of the first semiconductor layer. The stacked structure includes alternating dielectric layers and a first electrode layer.

[0130] In step S2, as Figure 5B As shown in S2, a stacked structure 30 is formed on the second surface V2 of the thermal insulation layer 20, which is away from the first surface V1 of the first semiconductor layer 10. The stacked structure 30 includes alternating dielectric layers 31 and first electrode layers G.

[0131] In some examples, the material of the first electrode layer G may include polycrystalline silicon.

[0132] In some examples, the material of dielectric layer 31 may include an insulating material. Insulating materials may be, for example, one or more combinations of silicon oxide, silicon nitride, silicon oxynitride, doped silicon oxide, organosilicon glass, dielectric metal oxides (e.g., aluminum oxide, hafnium dioxide, etc.) and their silicates, and organic insulating materials. The materials of the various dielectric layers 31 may be the same or different.

[0133] In step S2, alternating dielectric layers 31 and first electrode layers G can be directly formed on the second surface V2 of the insulation layer 20. This eliminates the need to first form the alternating dielectric layers 31 and sacrificial layers, and then subsequently etch the sacrificial layer to form the first electrode layer G. This simplifies the manufacturing process of the semiconductor structure 100 and saves resources.

[0134] In some examples, a thin-film deposition process can be used to form a stacked structure 30 on the first semiconductor layer 10. For example, the thin-film deposition process may include one or a combination of chemical vapor deposition (CVD), physical vapor deposition (PVD), and atomic layer deposition (ALD).

[0135] In the embodiments of this disclosure, the number of layers in the stacking structure 30 is not limited. For example, the number of layers in the stacking structure can be 8, 64, 128, etc. The more layers in the stacking structure 30, the higher the integration density of the ferroelectric memory cell string 300, and the more ferroelectric memory cells it forms.

[0136] S3: Forming a channel structure that runs through the stacked structure. The channel structure includes a ferroelectric thin film layer, a second electrode layer, and a channel layer. The ferroelectric thin film layer and the second electrode layer are located between the stacked structure and the channel layer, with the ferroelectric thin film layer being closer to the stacked structure than the second electrode layer.

[0137] In step S3, such as Figures 5C to 5F As shown in S3, a channel structure 40 is formed that penetrates the stacked structure 30. The channel structure 40 includes a ferroelectric thin film layer 41, a second electrode layer P, and a channel layer 42. The ferroelectric thin film layer 41 and the second electrode layer P are located between the stacked structure 30 and the channel layer 42; the ferroelectric thin film layer 41 is closer to the stacked structure 30 than the second electrode layer P.

[0138] In step S3, forming the channel structure 40 may include forming a channel hole 43 by an etching process. Then, the channel structure 40 is formed within the channel hole by a thin film deposition process. For example, a ferroelectric thin film layer 41, a second electrode layer P, and a channel layer 42 are formed within the channel hole by a thin film deposition process.

[0139] Step S3 includes:

[0140] like Figure 5C As shown, S31: A channel hole 43 is formed on the stacked structure 30 by an etching process, and the channel hole 43 exposes the thermal insulation layer 20.

[0141] like Figure 5D As shown, S32: A ferroelectric thin film layer 41 is formed on the channel hole 43. For example, a ferroelectric thin film layer 41 is deposited on the channel hole 43.

[0142] In some examples, the material of the ferroelectric thin film layer 41 includes hafnium-based ferroelectric materials.

[0143] like Figure 5E As shown, S33: A second electrode layer P is formed on the ferroelectric thin film layer 41. For example, a second electrode layer P is deposited on the ferroelectric thin film layer 41.

[0144] In some examples, the material of the second electrode layer P may include titanium nitride (TiN). In other examples, the material of the second electrode layer P may also be tantalum nitride (TaN) or platinum (Pt).

[0145] like Figure 5F As shown, S34: A channel layer 42 is formed on the second electrode layer P to fill the channel holes 43. For example, a channel layer 42 is deposited on the second electrode layer P.

[0146] In some examples, the material of the channel layer 42 may include tungsten (W).

[0147] S4: Forms a protective layer covering the trench structure and stacked structure.

[0148] In step S4: as follows Figure 5G As shown in S4, a protective layer 60 is formed that covers the channel structure 40 and the stacked structure 30.

[0149] In some examples, the material of the protective layer 60 includes polycrystalline silicon, amorphous silicon, or platinum. This disclosure does not specifically limit the material of the protective layer 60; other materials with high absorption and high thermal conductivity to the laser wavelength can be selected. For example, the material of the protective layer 60 can also be phosphorus-doped or boron-doped polycrystalline silicon.

[0150] S5: On the side of the protective layer away from the ferroelectric thin film layer, the ferroelectric thin film layer is annealed.

[0151] In step S5: (e.g.) Figure 5G As shown in S5, the ferroelectric thin film layer 41 is annealed on the side of the protective layer 60 away from the ferroelectric thin film layer 41.

[0152] On the one hand, the annealing process directly acts on the protective layer 60, and then conducts heat through the protective layer to the ferroelectric thin film layer 41 in the channel structure 40. This can meet the high-temperature environment requirements of the ferroelectric thin film layer 41, causing the amorphous hafnium oxide material in the ferroelectric thin film layer 41 to crystallize and transform into the ferroelectric orthorhombic hafnium oxide. For example, the ferroelectric phase exhibiting ferroelectricity in hafnium-based ferroelectric materials is the orthorhombic (O-phase) Pca21 space group. Among them, the orthorhombic phase conversion rate of the ferroelectric thin film 41 in the two-dimensional semiconductor structure (the stacked structure 30 includes a dielectric layer 31 and a first electrode layer G) can reach more than 70%, and the orthorhombic phase conversion rate of the ferroelectric thin film 41 in the three-dimensional semiconductor structure (multiple alternating dielectric layers 31 and first electrode layers G) can reach more than about 60%.

[0153] On the other hand, since the melting point of the first electrode layer G in the stacked structure 30 is relatively low, and a protective layer 60 is provided on top of the stacked structure 30, the annealing process directly acts on the protective layer 60, and then conducts heat through the protective layer to the ferroelectric thin film layer 41 in the channel structure 40. The protective layer 60 can prevent the annealing process from directly acting on the stacked structure 30, thus preventing the stacked structure 30 from easily melting.

[0154] Figure 6A This is a simulation diagram of temperature changes in a semiconductor structure provided according to some embodiments. Figure 6B This is a simulation diagram of temperature changes in a semiconductor structure provided according to some other embodiments. Figure 6C This is a simulation diagram of temperature changes of a semiconductor structure provided according to some other embodiments. Figure 6D This is a simulation diagram showing the energy density variation of a semiconductor structure according to some other embodiments. Figure 6A The following is an illustration of the temperature changes of the semiconductor structure at different times. Figure 6B and Figure 6C The temperature change at different locations of the film layer in a semiconductor structure is illustrated as an example. Figure 6D The variation in energy density at different locations of the film layer in a semiconductor structure is illustrated as an example.

[0155] In step S5, when annealing the ferroelectric thin film layer 41, as... Figure 6A As shown, the temperature can be raised to 1000℃ in approximately 100 ns and to 1200℃ in 150 ns. This indicates that the annealing process can raise the temperature to 1000℃ within an extremely short nanosecond. That is, the ferroelectric thin film layer 41 can reach a very high temperature in a short time, which is beneficial for the amorphous hafnium oxide material in the ferroelectric thin film layer 41 to crystallize and transform into a ferroelectric orthorhombic hafnium oxide phase.

[0156] In some implementations, such as Figure 6B and Figure 6C The diagram shows the temperatures at various film layer locations in the semiconductor structure 100 without the protective layer 60 and the thermal insulation layer 20. Since the semiconductor structure 100 lacks the thermal insulation layer 20, the ferroelectric thin film layer 41 and the first semiconductor layer 10 are in direct contact. This results in the temperature of the side of the first semiconductor layer 10 closest to the ferroelectric thin film layer 41 being approximately equal to the temperature of the side of the ferroelectric thin film layer 41 closest to the first semiconductor layer 10. Consequently, the temperatures of the first semiconductor layer 10 and the ferroelectric thin film layer 41 become approximately equal, placing the first semiconductor layer 10 in a high-temperature environment, which can easily lead to expansion and deformation.

[0157] Among them, due to the lack of a thermal insulation layer 20, Figure 6BThe thick dashed line shown does not indicate temperature at the location of the insulation layer. This does not mean that the temperature between the ferroelectric thin film layer 41 and the first semiconductor layer 10 is disconnected. For example, the temperature of the side of the first semiconductor layer 10 closest to the ferroelectric thin film layer 41 may be approximately equal to the temperature of the side of the ferroelectric thin film layer 41 closest to the first semiconductor layer 10.

[0158] In the embodiments disclosed herein, such as Figures 6A to 6C As shown, a thermal insulation layer 20 is formed between the first semiconductor layer 10 and the stacked structure 30. The thermal insulation layer 20 has a low thermal conductivity and can provide a good thermal insulation effect.

[0159] like Figure 6B As shown in the semiconductor structure 100 with a heat insulation layer 20, during annealing, the temperature of the ferroelectric thin film layer 41 can reach approximately 1400°C, while the presence of the heat insulation layer 20 allows the temperature of the first semiconductor layer 10 to be maintained at approximately 400°C. Figure 6B The semiconductor structure 100, which has a heat insulation layer 20, may also have a protective layer 60.

[0160] like Figure 6C As shown in the semiconductor structure 100 with a protective layer 60 and a thermal insulation layer 20, the temperature density of the ferroelectric thin film layer 41 can reach 1.4 × 10⁻⁶ during annealing. 3 The temperature density of the first semiconductor layer 10 can be maintained at around 0.5 × 10⁻⁶ due to the presence of the thermal insulation layer 20. 3 about.

[0161] Therefore, it can be seen that a heat insulation layer 20 is provided on the side of the first semiconductor layer 10 near the channel structure 40 in the semiconductor structure 100. This allows the heat generated during annealing to be concentrated on the side of the heat insulation layer 20 away from the first semiconductor layer 10, that is, concentrated on the ferroelectric thin film layer 41. This allows the ferroelectric thin film layer 41 to reach the required temperature during annealing more quickly, improving the efficiency of the annealing process. At the same time, it also prevents the heat from being conducted to the first semiconductor layer 10, preventing the first semiconductor layer 10 from deforming due to thermal expansion, while also improving the efficiency of the annealing process.

[0162] In some implementations, such as Figure 6D As shown in the semiconductor structure 100 without the protective layer 60 and the thermal insulation layer 20, since the semiconductor structure 100 does not have a thermal insulation layer, the laser directly irradiates the stacked structure 30 and the channel structure 40, which will result in a high laser density in the first electrode layer G of the top layer of the stacked structure 30, and will also result in a high temperature at this location. This will easily cause the first electrode layer G to melt in a high-temperature environment, affecting the performance of the semiconductor structure 100.

[0163] The embodiments disclosed herein, such as Figure 6D As shown in the semiconductor structure 100, which includes a protective layer 60 and a thermal insulation layer 20, the protective layer 60 is deposited on top of the semiconductor structure 100. In step S5, when the ferroelectric thin film layer 41 is annealed, the laser first acts on the protective layer 60. Because the protective layer 60 has good thermal conductivity, high thermal stability (high boiling point, high melting point), and good laser absorption, it can effectively absorb the heat from the laser and conduct it to the ferroelectric thin film layer 41, causing the amorphous hafnium oxide material in the ferroelectric thin film layer 41 to crystallize and transform into a ferroelectric orthorhombic hafnium oxide phase. Simultaneously, it can prevent the channel structure 40 and the stacked structure 30 near the laser from being directly exposed to the laser, thus preventing melting and other problems, and improving the performance of the semiconductor structure 100.

[0164] In summary, the semiconductor structure fabrication method provided in this disclosure involves forming a thermal insulation layer 20 between the first semiconductor layer 10 and the stacked structure 30, and depositing a protective layer 60 on top of the semiconductor structure 100. During the annealing process, the thermal insulation layer 20 can concentrate high temperatures in the ferroelectric thin film layer 41, preventing damage to the first semiconductor layer 10. Furthermore, the protective layer 60 can prevent direct laser radiation to the channel structure 40 and the stacked structure 30, keeping their temperatures below their melting points, thus preventing any impact on their performance and improving the performance of the semiconductor structure 100.

[0165] In some embodiments, continue as follows Figure 6A As shown, in step S5: on the side of the protective layer 60 away from the ferroelectric thin film layer 41, the ferroelectric thin film layer 41 is subjected to laser annealing.

[0166] Laser annealing utilizes a focused, small-area, high-energy laser to raise the temperature of a localized area within an extremely short time (nanoseconds / microseconds / seconds). Laser annealing of the ferroelectric thin film layer 41 concentrates the laser at that location, raising its temperature within microseconds. This facilitates the crystallization of amorphous hafnium oxide in the ferroelectric thin film layer 41 into a ferroelectric orthorhombic hafnium oxide phase, while preventing the high-temperature environment caused by the laser from affecting the film structure in other areas and thus impacting the performance of the semiconductor structure 100.

[0167] In some embodiments, such as Figure 6A As shown, the laser annealing process includes 20 to 50 laser irradiations, with each irradiation lasting 100 to 250 ns.

[0168] During laser annealing, a region of the ferroelectric thin film layer 41 can be continuously irradiated with lasers 20 to 50 times, with each irradiation lasting 100 ns to 250 ns.

[0169] That is, a region of the ferroelectric thin film layer 41 can be cumulatively irradiated with laser for microseconds, causing it to reach a temperature above 1000°C and maintain it for a period of time. This allows the required annealing temperature of the ferroelectric thin film layer 41 to be reached in a shorter time, which is beneficial for the amorphous hafnium oxide material in the ferroelectric thin film layer 41 to crystallize and transform into a ferroelectric orthorhombic hafnium oxide phase, thereby improving the performance of the semiconductor structure 100.

[0170] In some examples, laser annealing involves 30 to 50 laser irradiations. Alternatively, laser annealing may involve 30 to 40 laser irradiations. For instance, laser annealing may involve 20, 30, 40, or 50 laser irradiations on a single area.

[0171] In some examples, the duration of each laser irradiation is 150 ns to 200 ns. For example, the duration of each laser irradiation can be one of 100 ns, 150 ns, 200 ns, or 250 ns.

[0172] Taking the first region of the ferroelectric thin film layer 41 as an example:

[0173] like Figure 6A As shown, taking an example where the duration of each laser irradiation of the first region is 250 ns, the temperature of the first region of the ferroelectric thin film layer 41 can be raised to over 1000°C within 250 ns. Further irradiation of the first region of the ferroelectric thin film layer 41 with 20 to 50 250 ns laser irradiations can maintain the temperature of the first region of the ferroelectric thin film layer 41 at a high temperature, which is beneficial for the crystallization of the amorphous hafnium oxide material in the ferroelectric thin film layer 41 into a ferroelectric orthorhombic hafnium oxide phase. In this embodiment, the number of laser irradiations of the first region of the ferroelectric thin film layer 41 is not limited and can be 20, 30, 40, or 50 times.

[0174] Understandably, in the next stage, the laser can be irradiated to the second region of the ferroelectric thin film layer 41. Such partitioned irradiation can facilitate local high-temperature annealing, that is, the high temperature can be concentrated in the ferroelectric thin film layer 41 for ferroelectric material crystallization, preventing the film structure in other regions from being affected.

[0175] In some embodiments, the energy range of the laser annealing process is 0.3 J / cm². 2 ~2J / cm 2 .

[0176] When the energy of the laser is equal to or close to 0.3 J / cm 2At this time, the annealing treatment of the ferroelectric thin film layer 41 can be performed to crystallize the amorphous hafnium oxide material in the ferroelectric thin film layer 41 into a ferroelectric orthorhombic hafnium oxide phase, while also saving energy and resources. When the laser energy is equal to or close to 2J / cm 2 At the same time, the temperature can be increased more quickly and the efficiency of annealing can be improved without wasting resources.

[0177] For example, the energy of the laser is approximately 0.3 J / cm². 2 0.5J / cm 2 1J / cm 2 1.5J / cm 2 or 2J / cm 2 The embodiments disclosed herein do not limit the specific value of the laser energy.

[0178] In addition, it should be noted that due to certain uncontrollable errors (such as manufacturing process errors, equipment precision, measurement errors, etc.), the laser energy can also be considered to meet the condition of equality when the energy fluctuation range does not exceed 10% of the laser energy.

[0179] In some embodiments, such as Figure 6A As shown, the temperature range for laser annealing is 800℃~1400℃.

[0180] When the laser annealing temperature is equal to or close to 800℃, the relatively low temperature allows the amorphous hafnium oxide material in the ferroelectric thin film layer 41 to crystallize and transform into the ferroelectric orthorhombic hafnium oxide phase, while also saving energy and resources. When the laser annealing temperature is equal to or close to 1400℃, the relatively high temperature allows for faster crystallization and transformation of the amorphous hafnium oxide material in the ferroelectric thin film layer 41 into the ferroelectric orthorhombic hafnium oxide phase, while preventing resource waste and improving the efficiency of the annealing process.

[0181] For example, the laser annealing temperature is approximately 800°C, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, or 1400°C. The specific value of the laser annealing temperature in this embodiment is not limited.

[0182] In some embodiments, such as Figure 6B As shown, the thickness of the protective layer 60 ranges from 60 nm to 150 nm.

[0183] When the thickness of the protective layer 60 is equal to or close to 60 nm, the relatively thin protective layer 60 can effectively protect the stacked structure 30 (first electrode layer G), reducing the energy requirement for the laser and thus conserving energy and resources. When the thickness of the protective layer 60 is equal to or close to 150 nm, the relatively thick protective layer 60 can better protect the stacked structure 30 (first electrode layer G) while preventing resource waste, preventing it from melting in high-temperature environments and improving the performance of the semiconductor structure 100.

[0184] For example, the thickness of the protective layer 60 can be 60 nm, 100 nm, or 150 nm. In other examples, the thickness of the protective layer 60 can also be 70 nm, 80 nm, 90 nm, 110 nm, 120 nm, 130 nm, or 140 nm. This disclosure does not specifically limit the thickness of the protective layer 60.

[0185] In some examples, the thickness of the protective layer 60 can be adjusted according to the wavelength of the laser. The longer the wavelength of the laser, the thicker the protective layer 60 can be. For example, when the laser is green, that is, when the wavelength of the laser is approximately 500 nm, the thickness of the protective layer 60 can be less than 100 nm.

[0186] Figure 7 This is a block diagram of a storage system according to some embodiments. Figure 8 This is a block diagram of a storage system according to some other embodiments.

[0187] Please see Figure 7 and Figure 8 Some embodiments of this disclosure also provide a storage system 500. The storage system 500 includes a controller 510 and a three-dimensional memory 200 as described in some of the embodiments above, the controller 510 being coupled to the three-dimensional memory 200 to control the three-dimensional memory 200 to store data.

[0188] The storage system 500 can be integrated into various types of storage devices, for example, included in the same package (e.g., a Universal Flash Storage (UFS) package or an Embedded Multi Media Card (eMMC) package). In other words, the storage system 500 can be applied to and packaged into different types of electronic products, such as mobile phones (e.g., cell phones), desktop computers, tablets, laptops, servers, in-vehicle devices, game consoles, printers, positioning devices, wearable devices, smart sensors, power banks, virtual reality (VR) devices, augmented reality (AR) devices, or any other suitable electronic device containing storage.

[0189] In some embodiments, see Figure 7 The storage system 500 includes a controller 510 and a three-dimensional memory 200, and the storage system 500 can be integrated into a memory card.

[0190] Among them, memory cards include any one of the following: PC card (PCMCIA, Personal Computer Memory Card International Association), Compact Flash (CF) card, Smart Media (SM) card, memory stick, Multimedia Card (MMC), Secure Digital Memory Card (SD) card, and UFS.

[0191] In other embodiments, see Figure 8 The storage system 500 includes a controller 510 and multiple three-dimensional storage devices 200, and the storage system 500 is integrated into a solid state drive (SSD).

[0192] In some embodiments of the storage system 500, the controller 510 is configured to operate in a low duty cycle environment, such as an SD card, CF card, Universal Serial Bus (USB) flash drive, or other media used in electronic devices such as personal calculators, digital cameras, and mobile phones.

[0193] In other embodiments, controller 510 is configured to operate in a high duty cycle environment in an SSD or eMMC, which is used as data storage for mobile devices such as smartphones, tablets, and laptops, as well as enterprise storage arrays.

[0194] In some embodiments, controller 510 may be configured to manage data stored in 3D memory 200 and communicate with external devices (e.g., a host). In some embodiments, controller 510 may also be configured to control operations of 3D memory 200, such as read, erase, and program operations. In some embodiments, controller 510 may also be configured to manage various functions relating to data stored or to be stored in 3D memory 200, including at least one of bad block management, garbage collection, logical-to-physical address translation, and wear leveling. In some embodiments, controller 20 is also configured to process error correction codes relating to data read from or written to 3D memory 200.

[0195] Of course, the controller 510 can also perform any other suitable function, such as formatting the three-dimensional memory 200; for example, the controller 510 can communicate with external devices (e.g., a host) through at least one of various interface protocols.

[0196] It should be noted that the interface protocol includes at least one of the following: USB protocol, MMC protocol, Peripheral Component Interconnect (PCI) protocol, PCI High Speed ​​(PCI-E) protocol, Advanced Technology Attachment (ATA) protocol, Serial ATA protocol, Parallel ATA protocol, Small Computer Small Interface (SCSI) protocol, Enhanced Small Disk Interface (ESDI) protocol, Integrated Drive Electronic Device (IDE) protocol, and Firewire protocol.

[0197] Some embodiments of this disclosure also provide an electronic device. The electronic device can be any of the following: mobile phone, desktop computer, tablet computer, laptop computer, server, in-vehicle equipment, wearable device (e.g., smartwatch, smart bracelet, smart glasses, etc.), power bank, game console, digital multimedia player, etc.

[0198] The electronic device may include the storage system 500 described above, and may also include at least one of a central processing unit (CPU) and a cache.

[0199] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any variations or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention should be included within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.

Claims

1. A semiconductor structure, characterized in that, include: First semiconductor layer; A thermal insulation layer is located on the first surface of the first semiconductor layer; A stacked structure is located on the second surface of the insulation layer; The second surface is away from the first surface of the first semiconductor layer; the stacked structure includes alternately stacked dielectric layers and first electrode layers; as well as, A channel structure extends through the stacked structure; the channel structure includes a ferroelectric thin film layer, a second electrode layer, and a channel layer; the ferroelectric thin film layer and the second electrode layer are located between the stacked structure and the channel layer; The source electrode line is located within the thermal insulation layer and is coupled to the second electrode layer.

2. The semiconductor structure according to claim 1, characterized in that, The second electrode layer is located between the ferroelectric thin film layer and the channel layer.

3. The semiconductor structure according to claim 1, characterized in that, The material of the insulation layer includes at least one of silicon dioxide, polyimide, or borosilicate.

4. The semiconductor structure according to claim 1, characterized in that, The thickness of the insulation layer ranges from 100nm to 200nm.

5. The semiconductor structure according to claim 1, characterized in that, The material of the ferroelectric thin film layer includes hafnium-based ferroelectric materials.

6. The semiconductor structure according to claim 1, characterized in that, It also includes the circuit layer; The circuit layer is located within the first semiconductor layer; The second electrode layer is coupled to the circuit layer through the vias in the ferroelectric thin film layer and the thermal insulation layer.

7. A method for fabricating a semiconductor structure, characterized in that, include: A thermal insulation layer and a source line are formed on a first surface of a first semiconductor layer, wherein the source line is located within the thermal insulation layer; A stacked structure is formed on the second surface of the thermal insulation layer, the second surface being away from the first surface of the first semiconductor layer; the stacked structure includes alternately stacked dielectric layers and first electrode layers; A channel structure is formed that runs through the stacked structure. The channel structure includes a ferroelectric thin film layer, a second electrode layer, and a channel layer. The ferroelectric thin film layer and the second electrode layer are located between the stacked structure and the channel layer. The ferroelectric thin film layer is closer to the stacked structure than the second electrode layer. The second electrode layer is coupled to the source line. A protective layer is formed covering the channel structure and the stacked structure. On the side of the protective layer away from the ferroelectric thin film layer, the ferroelectric thin film layer is annealed.

8. The preparation method according to claim 7, characterized in that, The annealing process includes laser annealing.

9. The preparation method according to claim 8, characterized in that, The laser annealing process includes 20 to 50 laser irradiations, with each irradiation lasting 100 to 250 ns.

10. The preparation method according to claim 8, characterized in that, The energy range of the laser annealing process is 0.3 J / cm2 to 2 J / cm2.

11. The preparation method according to claim 8, characterized in that, The temperature range for laser annealing is 800℃~1400℃.

12. The preparation method according to claim 8, characterized in that, The thickness of the protective layer ranges from 60 nm to 150 nm.

13. The preparation method according to claim 8, characterized in that, The material of the protective layer includes polycrystalline silicon or amorphous silicon.

14. A three-dimensional memory, characterized in that, include: A semiconductor structure, wherein the semiconductor structure is the semiconductor structure as described in any one of claims 1 to 6.

15. A storage system, characterized in that, include: A three-dimensional memory, wherein the three-dimensional memory is the three-dimensional memory as described in claim 14; A controller is coupled to the three-dimensional memory to control the storage of data in the three-dimensional memory.

16. An electronic device, characterized in that, Includes the storage system as described in claim 15.

Citation Information

Patent Citations

  • Three-dimensional NAND type ferroelectric field effect transistor memory and preparation method thereof

    CN111799265A

  • Method of processing a semiconductor device

    US9023688B1