A high-power graphite composite material and preparation method thereof

Through plasma technology, lithium-ion battery materials are doped with phosphorus and coated with fast ion conductors to form high-power graphite composite materials with a core-shell structure, which solves the problems of high-temperature performance and energy density of lithium-ion battery anode materials when improving power performance. , achieving efficient improvement and performance optimization of materials.

CN115347175BActive Publication Date: 2024-10-18新疆天宏基科技有限公司
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211065750.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-01
Publication Date
2024-10-18
Estimated Expiration
2042-09-01

AI Technical Summary

Technical Problem

It is difficult for existing lithium-ion battery anode materials to maintain high-temperature performance and energy density while improving power performance. Commonly used methods will cause adverse effects on material performance.

Method used

Plasma technology is used to dope phosphorus and coat fast ion conductors, suspend graphite powder through a plasma generator and deposit fast ion conductor composite materials to form high-power graphite composite materials with a core-shell structure.

Benefits of technology

It effectively improves the specific capacity, compaction density and structural stability of the material, improves the cycle performance and fast charging performance, reduces the impact of the energy density of the battery, and improves the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115347175B_ABST
    Figure CN115347175B_ABST
Patent Text Reader

Abstract

The present invention is a high-power graphite composite material and a preparation method thereof. A preparation method of a high-power graphite composite material comprises the following steps: putting graphite powder into a plasma generator, pumping to negative pressure, introducing phosphorus sulfide gas, blowing the graphite precursor to a suspended state, and spraying a binder solution to form a spherical structure; turning on the plasma generator, using a fast ion conductor composite material as an emission source, depositing a fast ion conductor on the surface of the spherical structure, and then carbonizing and crushing to obtain the graphite composite material. The high-power graphite composite material and the preparation method thereof described in the present invention utilize plasma technology to uniformly dope phosphorus in the precursor, which can improve energy density and electronic conductivity, and at the same time coat the fast ion conductor on its outer surface to improve the ionic conductivity of the material, reduce interface impedance, and improve rate and cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of lithium ion battery material preparation, and specifically relates to a high-power graphite composite material and a preparation method thereof. Background Art

[0002] As the market's requirements for the power performance of lithium-ion batteries increase, the negative electrode materials used in lithium-ion batteries are required to have high energy density while also improving the power performance of the materials. The measures to improve the power performance of negative electrode materials mainly include: reducing the particle size of the material, but this will reduce the energy density; coating the surface of the material with metals or oxides with high electronic conductivity, and doping the surface of the material with fast ion conductors to improve the ion conductivity of the material. The above methods are mainly prepared by solid-phase and liquid-phase methods. Although they can improve the power performance of the material, they have adverse effects on the high-temperature performance and energy density of the material.

[0003] In view of this, the present invention proposes a new high-power graphite composite material and a preparation method thereof, which improves the power performance of the material and avoids adverse effects on the high temperature performance, energy density and other aspects of the material. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a high-power graphite composite material, and to improve the power performance of the material by doping phosphorus and coating a fast ion conductor through plasma technology.

[0005] In order to achieve the above purpose, the technical solution adopted is:

[0006] A method for preparing a high-power graphite composite material comprises the following steps:

[0007] Putting graphite powder into a plasma generator, pumping to negative pressure, introducing phosphorus sulfide gas, blowing the graphite powder to a suspended state, and then spraying a binder solution to form a spherical structure;

[0008] The plasma generator is turned on, and the fast ion conductor composite material is used as an emission source to deposit the fast ion conductor on the surface of the spherical structure, and then carbonized and crushed to obtain the graphite composite material.

[0009] Furthermore, the negative pressure is -0.1Mpa;

[0010] The flow rate of the phosphorus sulfide is 100 ml / min, and the time is 10 to 60 minutes;

[0011] The flow rate of the adhesive solution is 10 ml / min, and the time is 10 to 60 minutes.

[0012] Furthermore, the binder solution is one of CMC, polyvinyl alcohol, polytetrafluoroethylene, PVDF, and LA136D solutions.

[0013] Furthermore, the concentration of the binder solution is 1 to 5 wt %.

[0014] Furthermore, the fast ion conductor composite material includes: a fast ion conductor, nano silver powder, porous carbon, and asphalt.

[0015] Furthermore, the mass ratio of the graphite powder, the fast ion conductor, the nano silver powder, the porous carbon and the asphalt is 100:60-90:1-10:1-10:1-10.

[0016] Furthermore, the fast ion conductor is one of lithium ceria, lithium strontium oxide, and lithium yttrium oxide.

[0017] Furthermore, the power of the plasma generator is 100 to 300 W, and the deposition time is 10 to 60 minutes.

[0018] Another object of the present invention is to provide a high-power graphite composite material, which is prepared by the above-mentioned preparation method and has good power performance.

[0019] In order to achieve the above purpose, the technical solution adopted is:

[0020] Furthermore, the graphite composite material is a core-shell structure, wherein the core is phosphorus-doped graphite and the shell is a fast ion conductor composite material.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] Plasma technology is to deposit materials through a plasma generator and dope them inside or on the surface of the material. It has the advantages of high efficiency, high consistency, strong flexibility, and high density. It can significantly improve efficiency and performance when applied to lithium battery materials. Specifically:

[0023] 1. The present invention uses plasma technology to dope phosphorus sulfide into graphite to improve the specific capacity and compaction density of the material; at the same time, sulfur and carbon form a -CS- bond to improve the structural stability of the material, improve the cycle performance and reduce the impedance.

[0024] 2. The present invention uses plasma technology to deposit fast ion conductors on its outer shell, relying on the high lithium ion conductivity of the fast ion conductor to improve the fast charging performance of the material; at the same time, the fast ion conductor deposited by plasma has the advantages of high density and high deposition efficiency, and is deposited evenly and thinly, which has little effect on the energy density of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is the SEM image of the graphite composite material prepared in Example 1. DETAILED DESCRIPTION

[0026] In order to further illustrate the high-power graphite composite material and its preparation method of the present invention and achieve the expected purpose of the invention, the following is a detailed description of the high-power graphite composite material and its preparation method according to the present invention, its specific implementation, structure, characteristics and efficacy in combination with the preferred embodiment. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics in one or more embodiments can be combined in any suitable form.

[0027] The following will further introduce a high-power graphite composite material and its preparation method in detail in conjunction with specific embodiments of the present invention:

[0028] The present invention is a high-power graphite composite material and a preparation method thereof. The preparation method is as follows: placing graphite precursor powder in a plasma generator and evacuating to negative pressure, then introducing phosphorus sulfide gas, blowing the graphite powder in a suspended state, and making the graphite powder and phosphorus sulfide fully mixed and uniform; then spraying a binder solution to form a spherical structure; finally turning on the plasma generator, depositing a fast ion conductor composite material on the surface of the spherical structure, carbonizing and crushing, and obtaining a graphite composite material. The present invention utilizes plasma technology to uniformly mix phosphorus doping in the graphite precursor, thereby increasing energy density and electronic conductivity; at the same time, coating the fast ion conductor on its outer surface to increase the ionic conductivity of the material, reduce interface impedance, and increase rate and cycle performance.

[0029] Example 1.

[0030] The specific steps are as follows:

[0031] (1) 100 g of artificial graphite powder was placed in a plasma generator, and then the plasma generator chamber was evacuated to -0.1 MPa; then phosphorus sulfide gas was introduced into the generator through pipeline A (flow rate 100 ml / min, time 30 min), and the precursor was blown to a suspended state; then, a 1 wt% CMC binder aqueous solution was sprayed through pipeline B (flow rate 10 ml / min, time 30 min) to form a spherical structure.

[0032] (2) Then, the plasma generator is turned on, and the lithium cerate fast ion composite material is used as the emission source. The power is adjusted to generate plasma (power 200 W, time 30 min), and the fast ion conductor composite material is deposited on the surface of the spherical structure. Then, it is carbonized at 800°C for 3 h in an argon inert atmosphere and crushed to obtain a graphite composite material.

[0033] The fast ion composite material is prepared as follows: 70g of lithium cerate fast ion conductor, 5g of nano silver powder, 5g of porous carbon, and 5g of asphalt are evenly mixed and ground in a sand mill for 3h, and then carbonized at 200°C and pressed into blocks to obtain the lithium cerate fast ion composite material.

[0034] Example 2.

[0035] The specific steps are as follows:

[0036] (1) 100 g of artificial graphite powder was placed in a plasma generator, and then the plasma generator chamber was evacuated to -0.1 MPa; then phosphorus sulfide gas flow rate (100 ml / min, time 10 min) was introduced into the generator through pipeline A, and the precursor was blown to a suspended state; then a 2 wt% polyvinyl alcohol aqueous solution was sprayed through pipeline B (flow rate 10 ml / min, time 10 min) to form a spherical structure.

[0037] (2) Turn on the plasma generator, use the fast ion composite material as the emission source, adjust the power (power 100 W, time 60 min) to generate plasma, deposit the fast ion conductor composite material on the surface of the spherical structure, and then carbonize it at 800 ° C for 3 h in an argon inert atmosphere, crush it, and obtain a graphite composite material.

[0038] The fast ion composite material is prepared by mixing 60 g of lithium strontium oxide, 10 g of nano silver powder, 10 g of porous carbon and 10 g of asphalt evenly, grinding them in a sand mill for 3 hours, and then carbonizing and briquetting them at 200° C. to obtain a lithium strontium oxide fast ion composite material.

[0039] Example 3.

[0040] The specific steps are as follows:

[0041] (1) 100 g of artificial graphite powder was placed in a plasma generator, and then the plasma generator chamber was evacuated to -0.1 MPa; then phosphorus sulfide gas (100 ml / min, time 60 min) was introduced into the generator through pipeline A, and the precursor was blown to a suspended state; then 5 wt% LA136D aqueous solution (flow rate 10 ml / min, time 60 min) was sprayed through pipeline B to form a spherical structure.

[0042] (2) Turn on the plasma generator, use the lithium yttrium oxide fast ion composite material as the emission source, adjust the power (power 300 W, time 10 min) to generate plasma, deposit the fast ion conductor composite material on the surface of the spherical structure, and then carbonize it at 800 ° C for 3 h in an argon inert atmosphere, crush it, and obtain a graphite composite material.

[0043] The preparation process of the fast ion composite material is as follows: 90g of lithium yttrium oxide fast ion conductor, 1g of nano silver powder, 1g of porous carbon, and 1g of asphalt are mixed evenly, and ground in a sand mill for 3h, and then carbonized at 200°C and pressed into blocks to obtain the lithium yttrium oxide fast ion composite material.

[0044] Example 4.

[0045] The operation steps of Example 4 are the same as those of Example 1, except that PVDF is used as the binder solution.

[0046] Example 5.

[0047] The operation steps of Example 5 are the same as those of Example 1, except that PVDF is used as the binder solution.

[0048] Comparative Example:

[0049] 10 g of lithium cerate was added to 500 g of a 1% phenolic resin aqueous solution and dispersed uniformly to obtain solution A. Then 100 g of artificial graphite was added, added to a ball mill and mixed uniformly, spray dried, and then transferred to a tube furnace, heated to 800° C. in an argon atmosphere for carbonization for 3 h, and then naturally cooled to room temperature to obtain a graphite composite material coated with lithium cerate and amorphous carbon (abbreviated as: graphite composite material).

[0050] Experimental test:

[0051] 1) SEM test

[0052] The composite material prepared in Example 1 was subjected to SEM testing, and the results are as follows: Figure 1 shown.

[0053] Depend on Figure 1 It can be seen that the obtained composite material presents a spherical structure, the particle size is between 10 and 20 μm, and the size distribution is uniform.

[0054] 2) Physical and chemical testing

[0055] The powder conductivity, specific surface area, degree of graphitization, and main element content (cerium, strontium, and yttrium) of the composite materials obtained in Examples 1 to 3 and the comparative example were tested according to the test method in the national standard GB / T-24533-2019 "Graphite Negative Electrode Materials for Lithium Ion Batteries". The test results are shown in Table 1.

[0056] 3) Button battery test

[0057] The composite materials prepared in Examples 1 to 3 and the comparative example were used as negative electrode active materials and assembled into button batteries according to the following method:

[0058] Add LA132 binder, SP conductive agent, and deionized water solvent to the negative electrode material, stir and mix evenly to form negative electrode slurry, apply the negative electrode slurry on copper foil, dry, roll, and cut to form negative electrode sheets. The weight ratio of negative electrode material, LA132 binder, SP conductive agent, and deionized water is 95:4:1:220.

[0059] A metallic lithium sheet was used as the counter electrode, a polyethylene (PE) film was used as the separator, the electrolyte was a LiPF6 solution with a concentration of 1.3 mol / L, and the solvent was a mixture of EC and DEC in a volume ratio of 1:1. The button cell was assembled in an argon-filled glove box.

[0060] The prepared button batteries were installed on the Wuhan Blue Electric CT2001A battery tester, and charged and discharged at a rate of 0.1C. The charge and discharge voltage range was 0.005V to 2.0V. The first discharge capacity and first discharge efficiency were measured, and the ratio of the 3C rate discharge capacity to the 0.2C rate discharge capacity was tested.

[0061] The test results are shown in Table 1:

[0062] Table 1 Performance of the composite materials of Examples 1 to 3 and Comparative Examples

[0063]

[0064] It can be seen from Table 1 that the discharge specific capacity and first efficiency of the graphite composite negative electrode materials prepared in Examples 1 to 3 are significantly higher than those of the comparative example. The reason is that the lithium salt is deposited on the graphite surface by the ion deposition method, and the irreversible capacity of the material is reduced and the first efficiency and rate performance are improved by relying on the high ion conductivity of the lithium salt itself and the lithium ions provided by it; and the ion deposition method has the characteristics of high and uniform deposition density, which can improve the conductivity of the powder.

[0065] 4) Soft pack battery test

[0066] The graphite composite negative electrode materials prepared in Examples 1 to 3 and the comparative example were respectively used as negative electrode active materials, and a binder, a conductive agent, and a solvent were added to the negative electrode active materials, and the mixture was stirred and mixed to form a negative electrode slurry, and the negative electrode slurry was coated on a copper foil, dried, rolled, and cut to form a negative electrode sheet. The binder was LA132 binder, the conductive agent was SP conductive agent, and the solvent was double distilled water, and the weight ratio of the negative electrode active material, SP conductive agent, LA132 binder, and double distilled water was 95:1:4:220.

[0067] Ternary materials (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3O2) is a positive electrode active material, a binder, a conductive agent, and a solvent are added to the positive electrode active material, stirred and mixed to form a positive electrode slurry, and the positive electrode slurry is coated on an aluminum foil, dried, rolled, and cut to form a positive electrode sheet; the binder is PVDF, the conductive agent is SP, and the solvent is N-methylpyrrolidone. The weight ratio of the positive electrode material, the conductive agent, the binder, and the solvent is 93:3:4:140.

[0068] A 2Ah soft-pack battery was prepared using a 1.3 mol / L LiPF6 solution as the electrolyte, in which the solvent was a mixture of EC and DEC in a volume ratio of 1:1, and celegard2400 as the separator.

[0069] a. Rate performance test

[0070] The charge and discharge voltage range is 2.8~4.2V, the test temperature is 25±3.0℃, and the charging is performed at 1.0C, 2.0C, 3.0C, and 5.0C, and the discharge is performed at 1.0C. The constant current ratio and temperature of the battery under different charging modes are tested. The results are shown in Table 2:

[0071] Table 2 Rate performance of the composite materials of Examples 1 to 3 and Comparative Examples

[0072]

[0073] As can be seen from Table 2, the rate charging performance of the soft-pack battery of the present invention is significantly better than that of the comparative example, and the charging time is shorter, indicating that the composite negative electrode material of the present invention has good fast charging performance. The reason is that since a high-density fast ion conductor is deposited on its surface by an ion deposition method, the insertion and extraction rate of lithium ions during the charging and discharging process can be increased, and the rate performance can be improved; at the same time, the embodiment material has a high specific surface area, which can improve its kinetic performance, thereby improving the constant current ratio of its battery and reducing the temperature rise.

[0074] b. Cycle performance test

[0075] The soft-pack batteries prepared with the negative electrode materials in Examples 1 to 3 and the comparative example were subjected to the following experiment: 100, 300, and 500 charge and discharge cycles were performed at a 2C / 2C charge and discharge rate and a voltage range of 2.8 to 4.2 V, respectively, to test the capacity retention rate. The results are shown in Table 3:

[0076] Table 3 Cycling performance of lithium ion batteries made from composite materials of Examples 1 to 3 and Comparative Example

[0077]

[0078] As can be seen from Table 3, the cycle performance of the lithium-ion battery prepared by the composite negative electrode material prepared by the present invention is significantly better than that of the comparative example in all stages. The reason is that the fast ion conductor is coated on the graphite surface, and the lithium ions of the fast ion conductor itself are used to improve the insertion and extraction rate of lithium ions and the structural stability during the charge and discharge process, thereby improving the cycle performance.

[0079] The above is only a preferred embodiment of the embodiment of the present invention, and does not impose any form of limitation on the embodiment of the present invention. Any simple modification, equivalent changes and modifications made to the above embodiment based on the technical essence of the embodiment of the present invention are still within the scope of the technical solution of the embodiment of the present invention.

Claims

1. A method for preparing a high-power graphite composite material, characterized in that: The following steps are involved: Putting graphite powder into a plasma generator, pumping to negative pressure, introducing phosphorus sulfide gas, blowing the graphite powder to a suspended state, and then spraying a binder solution to form a spherical structure; The plasma generator is turned on, and the fast ion conductor composite material is used as an emission source to deposit the fast ion conductor on the surface of the spherical structure, and then carbonized and crushed to obtain the graphite composite material.

2. The preparation method according to claim 1, characterized in that: The negative pressure is -0.1Mpa; The flow rate of the phosphorus sulfide is 100 ml / min, and the time is 10 to 60 minutes; The flow rate of the binder solution is 10 ml / min, and the time is 10 to 60 minutes.

3. The preparation method according to claim 1, characterized in that: The binder solution is one of CMC, polyvinyl alcohol, polytetrafluoroethylene, PVDF and LA136D solution.

4. The preparation method according to claim 3, characterized in that: The concentration of the binder solution is 1-5wt%.

5. The preparation method according to claim 1, characterized in that: The fast ion conductor composite material comprises: a fast ion conductor, nano silver powder, porous carbon and asphalt.

6. The preparation method according to claim 5, characterized in that: The mass ratio of the graphite powder, the fast ion conductor, the nano silver powder, the porous carbon and the asphalt is 100:60-90:1-10:1-10:1-10.

7. The preparation method according to claim 5, characterized in that: The fast ion conductor is one of lithium cerate, lithium strontium oxide and lithium yttrium oxide.

8. The preparation method according to claim 1, characterized in that: The power of the plasma generator is 100-300W, and the deposition time is 10-60 minutes.

9. A high-power graphite composite material, characterized in that: The graphite composite material is prepared by the preparation method described in any one of claims 1 to 8.

10. The graphite composite material according to claim 9, characterized in that: The graphite composite material is a core-shell structure, the core is phosphorus-doped graphite, and the shell is a fast ion conductor composite material.

Citation Information

Patent Citations

  • Ion-electron co-conductive material, preparation method and device thereof

    CN113644273A

  • Sulfur-containing fast ion conductor coated graphite composite material and preparation method thereof

    CN114709398A