A method for pre-alkaline metallization of negative electrode of alkali metal ion battery
By reacting the benzophenone-lithium/sodium/potassium solution with the carbon negative electrode material, the problem of low first Coulombic efficiency of the lithium/sodium/potassium ion battery negative electrode material is solved, and efficient pre-lithium/sodium/potassium treatment is achieved. Improved battery performance and suitable for industrial production.
Patent Information
- Application Number
- CN202110549227.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-20
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-05-20
Smart Images

Figure CN115377341B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of electrochemistry, and in particular relates to a method for preparing a pre-lithium, sodium or potassium solution for a negative electrode of a lithium, sodium or potassium ion battery. Background Art
[0002] In the past few decades, alkali metal ion batteries have developed rapidly, especially lithium ion batteries, which are widely used in portable electronic devices and electric vehicles due to their high energy density and excellent cycle performance. However, limited alkali metal resources and low first coulombic efficiency of the negative electrode inevitably hinder their further application. Therefore, improving the utilization rate of alkali metals in the cycle process is of great significance to improving battery performance and promoting the realization of carbon neutrality.
[0003] The negative electrode materials reported so far can be roughly divided into four categories: carbon materials, metal elements and alloy materials, metal compounds and organic materials. They have high capacity, good cycle life and rate performance; however, due to their negative lithium / sodium / potassium insertion potential, the charge and discharge process easily causes the electrolyte to decompose or some alkali metal ions cannot be removed after being embedded in the negative electrode, resulting in low first coulombic efficiency. In order to improve the first coulombic efficiency of the negative electrode, researchers often use methods such as reducing the specific surface area, increasing the synthesis temperature, reducing the surface functional groups and adjusting the electrolyte components. Although these modification methods have a certain effect on improving the first coulombic efficiency, they are still far from the first coulombic efficiency of more than 95% required for practical negative electrodes. Although lithium powder supplementation and electrochemical pre-lithium / sodium / potassium can effectively improve the coulombic efficiency of the negative electrode, there are problems such as complex operation process and low safety, which is not conducive to large-scale industrialization. Summary of the invention
[0004] The purpose of the present invention is to solve the problem of low first coulombic efficiency of existing carbon negative electrode materials for lithium / sodium / potassium ion batteries, and to provide a method for pre-alkali metallization of negative electrodes for alkali metal ion batteries, so as to greatly improve the first coulombic efficiency of negative electrode materials for lithium / sodium / potassium ion batteries.
[0005] The technical solution of the present invention is as follows:
[0006] A method for pre-alkali metallization of an alkali metal ion battery negative electrode comprises reacting a lithium / sodium / potassium ion battery carbon negative electrode (graphite / hard carbon) material with a benzophenone-lithium / sodium / potassium solution, washing, and vacuum drying to obtain a pre-lithium / sodium / potassium negative electrode, wherein the solute of the benzophenone-lithium / sodium / potassium solution is benzophenone-lithium, benzophenone-sodium or benzophenone-potassium, and the solvent of the benzophenone-lithium / sodium / potassium solution is an aprotic solvent.
[0007] Preferably, the negative electrode material of the lithium / sodium / potassium ion battery comprises a carbon negative electrode active material or a carbon negative electrode plate, and the method for reacting the negative electrode material of the battery with a benzophenone-lithium / sodium / potassium solution is as follows: in an inert atmosphere, the benzophenone-lithium / sodium / potassium solution is drop-coated on the carbon negative electrode of the lithium / sodium / potassium ion battery, washed, and vacuum dried to obtain a pre-lithium / sodium / potassium-treated lithium / sodium / potassium ion battery negative electrode.
[0008] The amount of benzophenone-lithium / sodium / potassium solution added in the method is 10 to 100 μL mg based on the mass of the active substance. -1 Preferably, the amount of benzophenone-lithium / sodium / potassium solution added is 35uLmg calculated by mass of active substance -1 .
[0009] Preferably, the concentration of the solute in the benzophenone-lithium / sodium / potassium solution is 0.001-2 mol L -1 , more preferably 0.2 mol L -1 .
[0010] Preferably, the solvent in the benzophenone-lithium / sodium / potassium solution is ethylene glycol dimethyl ether.
[0011] Advantages and beneficial effects of the present invention:
[0012] The present invention uses a benzophenone-lithium / sodium / potassium reagent with mild reaction and stable properties to perform pre-lithium / sodium / potassium treatment on the negative electrode material of the lithium / sodium / potassium ion battery. The method can be performed at room temperature, has simple operation, short process flow, rapid reaction, high safety, and is very easy to industrialize. At the same time, the pre-lithium / sodium / potassium negative electrode can greatly reduce the loss of active ions caused by SEI formation during the first cycle, and improve the first coulomb efficiency of the negative electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 is a scanning electron microscope image of the hard carbon obtained in Example 1;
[0014] Figure 2 is a scanning electron microscope image of the hard carbon after pre-sodium treatment obtained in Example 1;
[0015] Figure 3 The first week charge-discharge curve of the hard carbon negative electrode material before and after pre-sodiumization obtained in Example 1 (active material loading: ~1.5 mg cm -2 Current density: 50mAg -1 Pre-sodium solution concentration: 0.2 mol L -1 Pre-sodium solution volume: 35uLmg -1 Hard carbon);
[0016] Figure 4The long-term cycle stability diagram of the pre-sodium treated hard carbon negative electrode material electrode obtained in Example 1 (active material loading: ~1.5 mg cm -2 Current density: 50mAg -1 Pre-sodium solution concentration: 0.2 mol L -1 Pre-sodium solution volume: 35uLmg -1 Hard carbon);
[0017] Figure 5 The first week charge-discharge curve of the hard carbon negative electrode material before and after pre-sodiumization obtained in Example 2 (active material loading: ~1.5 mg cm -2 Current density: 50mAg -1 Pre-sodium solution concentration: 0.001 mol L -1 Pre-sodium solution volume: 35uLmg -1 Hard carbon);
[0018] Figure 6 The first week charge-discharge curve of the hard carbon negative electrode material before and after pre-sodiumization obtained in Example 3 (active material loading: ~1.5 mg cm -2 Current density: 50mA g -1 Pre-sodium solution concentration: 2 mol L -1 Pre-sodium solution volume: 35uLmg -1 Hard carbon);
[0019] Figure 7 The first week charge-discharge curve of the hard carbon negative electrode material before and after pre-sodiumization obtained in Example 4 (active material loading: ~1.5 mg cm -2 Current density: 50mAg -1 Pre-sodium solution concentration: 0.2 mol L -1 Pre-sodium solution volume: 10uLmg -1 Hard carbon);
[0020] Figure 8 The first week charge-discharge curve of the hard carbon negative electrode material before and after pre-sodiumization obtained in Example 5 (active material loading: ~1.5 mg cm -2 Current density: 50mAg -1 Pre-sodium solution concentration: 0.2 mol L -1 Pre-sodium solution volume: 100uLmg -1 Hard carbon);
[0021] Fig. 9 The first week charge-discharge curve of the pre-lithiation treated graphite negative electrode material obtained in Example 6 (active material loading: ~1.5 mg cm -2 Current density: 50mAg -1 Pre-lithiation solution concentration: 0.2 mol L-1 Pre-lithiation solution volume: 35uLmg -1 graphite);
[0022] Fig.10 The long-term cycle stability diagram of the pre-lithiation treated hard carbon negative electrode material obtained in Example 6 (active material loading: ~1.5 mg cm -2 Current density: 50mAg -1 Pre-lithiation solution concentration: 0.2 mol L -1 Pre-lithiation solution volume: 35uLmg -1 graphite);
[0023] Fig.11 The first week charge-discharge curve of the pre-potassium treated hard carbon negative electrode material obtained in Example 7 (active material loading: ~1.5 mg cm -2 Current density: 50mAg -1 Pre-potassium solution concentration: 0.2 mol L -1 Pre-potassium solution volume: 35uLmg -1 Hard carbon);
[0024] Fig.12 The long-term cycle stability diagram of the pre-potassium treated hard carbon negative electrode material electrode obtained in Example 7 (active material loading: ~1.5 mg cm -2 Current density: 50mAg -1 Pre-potassium solution concentration: 0.2 mol L -1 Pre-potassium solution volume: 35uLmg -1 hard carbon). DETAILED DESCRIPTION
[0025] The present invention is described in detail and completely below in conjunction with the accompanying drawings, but these embodiments are not intended to limit the scope of protection of the present invention. The reagents used in the examples are all purchased from the market or obtained by conventional synthesis methods in the art unless otherwise specified.
[0026] Embodiment 1:
[0027] Under the protection of an inert atmosphere, 0.002 mol of benzophenone and 0.002 mol of sodium were mixed and dispersed in 10 mL of ethylene glycol dimethyl ether solvent. After reaction at room temperature, a concentration of 0.2 mol L -1 Benzophenone-sodium ethylene glycol dimethyl ether solution, the amount of pre-sodium solution added to the hard carbon negative electrode is 35uLmg -1 After the reaction is complete, it is washed with DME three times and dried in vacuum at 80℃ for later use. The scanning electron microscope images of the hard carbon before and after pre-sodium treatment are shown in Figure 2. Figure 1 and Figure 2 As shown, the results show that pre-sodiumization has no effect on the particle size of the material.
[0028] At room temperature, constant current charge and discharge tests were performed using the Land CT2001A battery test system. Figure 3 As shown, the test voltage range is 0.01V-1.5V, and the current density is 50mAg -1 , Figure 3 The results show that after pre-sodiumization, the open circuit voltage of the half-cell decreases from 1.967V to 0.721V, indicating the successful realization of pre-sodiumization. As can be seen from the figure, the first charge and discharge capacity of the hard carbon negative electrode is 269.1 / 318.4mAh g -1 , while the first charge and discharge capacity of the pre-sodiumized hard carbon anode is 293.4 / 295.6 mAh g -1 Compared with the non-pre-sodiumized hard carbon electrode, the first coulombic efficiency of the pre-sodiumized electrode was significantly improved, from 84.49% to 99.24%. Figure 4 The long-term cycling stability of the hard carbon negative electrode after pre-sodium treatment is shown in the figure. The capacity retention rate for 70 cycles is 100%, and the coulombic efficiency is also close to 100%, indicating that the pre-sodium treatment has no effect on the cycling stability of the electrode material.
[0029] Embodiment 2:
[0030] Under the protection of an inert atmosphere, 0.002 mol of benzophenone and 0.002 mol of sodium were mixed and dispersed in 2 mL of ethylene glycol dimethyl ether solvent. After reaction at room temperature, a concentration of 0.001 mol L -1 Benzophenone-sodium ethylene glycol dimethyl ether solution, the amount of pre-sodium solution added to the hard carbon negative electrode is 35uLmg -1 After the reaction is complete, the hard carbon is washed with DME three times and dried in vacuum at 80°C for later use.
[0031] At room temperature, constant current charge and discharge tests were performed using the Land CT2001A battery test system. Figure 5 As shown, the test voltage range is 0.01V-1.5V, and the current density is 50mAg -1 , Figure 5 The results show that after pre-sodiumization, the open circuit voltage of the half-cell decreased from 1.967V to 1.136V, indicating the successful realization of pre-sodiumization. As can be seen from the figure, the first charge and discharge capacity of the hard carbon negative electrode is 269.1 / 318.4mAh g -1 , while the first charge and discharge capacity of the pre-sodiumized hard carbon anode is 280.8 / 315.2 mAh g -1 Compared with the non-pre-sodiumized hard carbon electrode, the first coulombic efficiency of the pre-sodiumized electrode was significantly improved, from 84.49% to 89.08%.
[0032] Embodiment 3:
[0033] Under the protection of an inert atmosphere, 0.02 mol of benzophenone and 0.02 mol of sodium were mixed and dispersed in 10 mL of ethylene glycol dimethyl ether solvent. After reaction at room temperature, a concentration of 2 mol L -1 Benzophenone-sodium ethylene glycol dimethyl ether solution, the amount of pre-sodium solution added to the hard carbon negative electrode is 35uLmg -1 After the reaction is complete, the hard carbon is washed with DME three times and dried in vacuum at 80°C for later use.
[0034] At room temperature, constant current charge and discharge tests were performed using the Land CT2001A battery test system. Figure 6 As shown, the test voltage range is 0.01V-1.5V, and the current density is 50mAg -1 , Figure 6 The results show that after pre-sodiumization, the open circuit voltage of the half-cell decreased from 1.967V to 0.492V, indicating the successful realization of pre-sodiumization. As can be seen from the figure, the first charge and discharge capacity of the hard carbon negative electrode is 269.1 / 318.4mAh g -1 , while the first charge and discharge capacity of the pre-sodiumized hard carbon anode is 405.5 / 270.6 mAh g -1 Compared with the non-pre-sodiumized hard carbon electrode, the first coulombic efficiency of the pre-sodiumized electrode was significantly improved, from 84.49% to 149.85%.
[0035] Embodiment 4:
[0036] Under the protection of an inert atmosphere, 0.002 mol of benzophenone and 0.002 mol of sodium were mixed and dispersed in 10 mL of ethylene glycol dimethyl ether solvent. After reaction at room temperature, a concentration of 0.2 mol L -1 Benzophenone-sodium ethylene glycol dimethyl ether solution, the amount of pre-sodium solution added to the hard carbon negative electrode is 10uLmg -1 After the reaction is complete, the hard carbon is washed with DME three times and dried in vacuum at 80°C for later use.
[0037] At room temperature, constant current charge and discharge tests were performed using the Land CT2001A battery test system. Figure 7 As shown, the test voltage range is 0.01V-1.5V, and the current density is 50mAg -1 , Figure 7 The results show that after pre-sodiumization, the open circuit voltage of the half-cell decreased from 1.967V to 1.621V, indicating the successful realization of pre-sodiumization. As can be seen from the figure, the first charge and discharge capacity of the hard carbon anode is 269.1 / 318.4mAh g -1 , while the first charge and discharge capacity of the pre-sodiumized hard carbon anode is 334.2 / 294.5 mAh g -1Compared with the non-pre-sodiumized hard carbon electrode, the first coulombic efficiency of the pre-sodiumized electrode was significantly improved, from 84.49% to 88.12%.
[0038] Embodiment 5:
[0039] Under the protection of an inert atmosphere, 0.002 mol of benzophenone and 0.002 mol of sodium were mixed and dispersed in 10 mL of ethylene glycol dimethyl ether solvent. After reaction at room temperature, a concentration of 0.2 mol L -1 The amount of benzophenone-sodium ethylene glycol dimethyl ether solution added to the hard carbon negative electrode is 100uL mg -1 After the reaction is complete, the hard carbon is washed with DME three times and dried in vacuum at 80°C for later use.
[0040] At room temperature, constant current charge and discharge tests were performed using the Land CT2001A battery test system. Figure 8 As shown, the test voltage range is 0.01V-1.5V, and the current density is 50mAg -1 , Figure 8 The results show that after pre-sodiumization, the open circuit voltage of the half-cell decreased from 1.967V to 0.502V, indicating the successful realization of pre-sodiumization. As can be seen from the figure, the first charge and discharge capacity of the hard carbon negative electrode is 269.1 / 318.4mAh g -1 , while the first charge and discharge capacity of the pre-sodiumized hard carbon anode is 282.2 / 252.4 mAh g -1 Compared with the non-pre-sodiumized hard carbon electrode, the first coulombic efficiency of the pre-sodiumized electrode was significantly improved, from 84.49% to 118.80%.
[0041] Embodiment 6:
[0042] Under the protection of an inert atmosphere, 0.002 mol of benzophenone and 0.002 mol of lithium were mixed and dispersed in 10 mL of ethylene glycol dimethyl ether solvent. After reaction at room temperature, a benzophenone-lithium ethylene glycol dimethyl ether solution with a concentration of 0.2 mol / L was obtained. The amount of the pre-lithiation solution added to the graphite negative electrode was 35 uL mg -1 After the reaction is complete, the graphite is washed with DME three times and dried under vacuum at 80°C for later use.
[0043] At room temperature, constant current charge and discharge tests were performed using the Land CT2001A battery test system. Fig. 9 As shown, the test voltage range is 0.01V-1.5V, and the current density is 50mAg -1 , Fig. 9The results show that after pre-lithiation, the open circuit voltage of the half-cell decreased from 2.658V to 1.947V, indicating the successful realization of pre-lithiation. As can be seen from the figure, the first charge and discharge capacity of the graphite anode is 321.8 / 411.3mAh g -1 , while the first charge and discharge capacity of the pre-lithiated graphite anode is 364.3 / 425.6 mAh g -1 Compared with the non-pre-lithiated graphite electrode, the first coulombic efficiency of the pre-lithiated electrode was significantly improved, from 75.23% to 85.61%. Fig.10 The long-term cycle stability of the graphite negative electrode after pre-lithiation is shown in Figure 2. The capacity retention rate after 70 cycles is close to 100%, and the coulombic efficiency is 100%, indicating that the pre-lithiation treatment has no effect on the cycle stability of the electrode material.
[0044] Embodiment 7:
[0045] Under the protection of an inert atmosphere, 0.002 mol of benzophenone and 0.002 mol of potassium were mixed and dispersed in 10 mL of ethylene glycol dimethyl ether solvent. After reaction at room temperature, a concentration of 0.2 mol L -1 Benzophenone-potassium ethylene glycol dimethyl ether solution, the amount of pre-potassium solution added to the hard carbon negative electrode is 35uLmg -1 After the reaction is complete, the hard carbon is washed with DME three times and dried in vacuum at 80°C for later use.
[0046] At room temperature, constant current charge and discharge tests were performed using the Land CT2001A battery test system. Fig.11 As shown, the test voltage range is 0.01V-1.5V, and the current density is 50mAg -1 , Fig.11 The results show that after pre-potassium treatment, the open circuit voltage of the half-cell decreased from 1.789 V to 0.887 V, indicating the successful implementation of pre-potassium treatment. As can be seen from the figure, the first charge and discharge capacity of the hard carbon negative electrode is 233.1 / 310.7 mAh g -1 , while the first charge and discharge capacity of the pre-sodiumized hard carbon anode is 211.9 / 211.8 mAh g -1 Compared with the non-pre-sodiumized hard carbon electrode, the first coulombic efficiency of the pre-sodiumized electrode was significantly improved, from 71.87% to 100.10%. Fig.12 The long-term cycling stability of the hard carbon negative electrode after pre-potassium treatment is shown in the figure. The capacity retention rate after 70 cycles is close to 100%, and the coulombic efficiency is also close to 100%, indicating that the pre-lithiation treatment has no effect on the cycling stability of the electrode material.
[0047] In summary, the method of pre-lithiation / sodium / potassiumization of the negative electrode of lithium / sodium / potassium ion battery using benzophenone-lithium / sodium / potassium reagent is effective, highly safe, and has no effect on the subsequent electrochemical properties of the material. The negative electrode material obtained by this method has high efficiency in the first week and stable cycle process, and has broad research prospects and application value. The above-described embodiments are only preferred examples of the present invention and are not intended to limit the present invention in any form. There are other variants and modifications without exceeding the technical solutions described in the claims.
Claims
1. A method for pre-alkali metallization of negative electrodes of alkali metal ion batteries, It is characterized in that The sodium or potassium ion battery hard carbon negative electrode material is reacted with a benzophenone-sodium or benzophenone-potassium solution in an argon-filled glove box at room temperature, and the benzophenone-sodium or benzophenone-potassium solution is drop-coated on the sodium or potassium ion battery hard carbon negative electrode, respectively, and washed and vacuum dried to obtain a pre-sodium or pre-potassium hard carbon negative electrode, wherein the solute of the solution is benzophenone-sodium or benzophenone-potassium, respectively, and the solvent of the solution is an aprotic solvent, specifically ethylene glycol dimethyl ether; the concentration of the solute in the benzophenone-sodium or benzophenone-potassium solution is 0.001-2 mol L -1 The amount of the benzophenone-sodium or benzophenone-potassium solution added is 10 to 100 μL mg based on the mass of the active substance. -1 .
2. The method for pre-alkali metallization of the negative electrode of an alkali metal ion battery according to claim 1, It is characterized in that The concentration of the solute in the benzophenone-sodium or benzophenone-potassium solution is 0.2 mol L -1 The amount of benzophenone-sodium / potassium solution added is 35uLmg calculated by the mass of active substance. -1 .