Decorative sheet, decorative plate, method for producing original plate for transfer, and method for producing decorative sheet

By forming a concave-convex surface protective layer on the decorative sheet, the problem of fingerprint adhesion caused by gloss modifiers is solved, and a highly oleophobic and fingerprint-resistant decorative sheet is achieved, which combines the effects of matte feeling and fingerprint resistance.

CN115397660BActive Publication Date: 2024-10-08TOPPAN HOLDINGS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180026115.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-04-02
Filing Date
2021-01-06
Publication Date
2024-10-08
Estimated Expiration
2041-01-06

AI Technical Summary

Technical Problem

The use of gloss modifiers in existing decorative sheets will reduce the oleophobicity of the surface, making it easy to adhere to fingerprints, making it difficult to maintain fingerprint resistance and a matte feel.

Method used

A first surface protective layer with a concave and convex shape is used, and the concave and convex shape is formed by surface irradiation of an ionizing radiation curable resin, and a gloss modifier is avoided in the resin material to improve oleophobicity and fingerprint resistance.

Benefits of technology

It is possible to adjust the glossiness and improve the oleophobicity of the surface of the decorative sheet without using a gloss modifier, significantly reduce fingerprint adhesion, and enhance fingerprint resistance and stain resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115397660B_ABST
    Figure CN115397660B_ABST
Patent Text Reader

Abstract

A decorative sheet having excellent anti-fingerprint property on the surface of the decorative sheet, a decorative plate, a method for manufacturing a transfer original plate, and a method for manufacturing a decorative sheet. The decorative sheet comprises: a raw material layer, a colored pattern layer provided on one surface of the raw material layer, and a first surface protective layer provided on the surface of the colored pattern layer opposite to the raw material layer and having a concavo-convex shape on the surface. The decorative sheet is formed using a transfer original plate as a resin material having a concavo-convex shape for the original plate on the surface formed by: irradiating a surface coated with an ionizing radiation curing resin with a first ionizing radiation having an energy capable of cutting a polymer chain of the ionizing radiation curing resin to shrink the surface of the ionizing radiation curing resin, thereby forming a concavo-convex shape for the original plate on the surface of the ionizing radiation curing resin, and irradiating the shrunken ionizing radiation curing resin with a second ionizing radiation for curing the ionizing radiation curing resin to cure the ionizing radiation curing resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a decorative sheet, a decorative plate, a method for producing a transfer original plate, and a method for producing a decorative sheet. Background Art

[0002] Conventionally, for decorative sheets, a gloss adjuster (matting additive) is added to the surface protective layer of the decorative sheet to adjust the matte feeling of the decorative sheet surface from the viewpoint of design etc. (for example, see Patent Document 1).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2001-129959 Summary of the invention

[0006] Problems to be Solved by the Invention

[0007] However, the gloss adjuster reduces the oleophobicity of the layer formed of the resin material. Therefore, the decorative sheet having the surface protection layer containing the gloss adjuster has a problem that fingerprints are easily attached.

[0008] The present disclosure has been made in view of such problems, and an object of the present disclosure is to provide a decorative sheet having excellent anti-fingerprint properties on the surface of the decorative sheet, a decorative plate, a method for producing a transfer original plate, and a method for producing a decorative sheet.

[0009] Means for solving problems

[0010] In order to solve the above-mentioned problems, a decorative sheet involved in one embodiment of the present invention is characterized in that it comprises: a raw material layer, a colored pattern layer arranged on one surface of the raw material layer, and a first surface protection layer arranged on the surface of the colored pattern layer on the opposite side of the raw material layer and having a concave-convex shape on the surface.

[0011] In addition, a decorative board according to one aspect of the present disclosure is characterized by comprising: the decorative sheet described above; and a base material layer provided on a surface of the raw material layer on the opposite side to the colored pattern layer.

[0012] In addition, a method for manufacturing a transfer original plate involved in one embodiment of the present invention is characterized in that a first ionizing radiation having energy capable of cutting polymer chains of the ionizing radiation-curing resin is irradiated onto a surface coated with an ionizing radiation-curing resin to shrink the surface of the ionizing radiation-curing resin, thereby forming an original plate concave-convex shape on the surface of the ionizing radiation-curing resin, and a second ionizing radiation for curing the ionizing radiation-curing resin is irradiated onto the shrunken ionizing radiation-curing resin to cure the ionizing radiation-curing resin, thereby forming a transfer original plate as a resin material having an original plate concave-convex shape on its surface.

[0013] In addition, the method for manufacturing a transfer original plate involved in other embodiments of the present invention is characterized in that a first ionizing radiation having energy capable of cutting polymer chains of the ionizing radiation-curing resin is irradiated onto a surface coated with an ionizing radiation-curing resin to shrink the surface of the ionizing radiation-curing resin, thereby forming an original plate concave-convex shape on the surface of the ionizing radiation-curing resin, and the ionizing radiation-curing resin is cured by irradiating the shrunken ionizing radiation-curing resin with a second ionizing radiation for curing the ionizing radiation-curing resin, thereby forming a transfer original plate as a resin material having an original plate concave-convex shape on its surface.

[0014] In addition, a method for manufacturing a decorative sheet involved in one embodiment of the present invention is characterized in that a resin material is coated on one surface of an original material layer, a transfer original formed by the above-mentioned method for manufacturing a transfer original is used to transfer the original plate concave-convex shape arranged on the surface of the transfer original to the resin material, and the resin material is cured to form a first surface protective layer on one surface of the original material layer, wherein the surface of the resin material has a concave-convex shape corresponding to the concave-convex shape of the original plate.

[0015] Effects of the Invention

[0016] According to the aspects of the present disclosure, a decorative sheet, a decorative plate, a method for producing a transfer original plate, and a method for producing a decorative sheet that can achieve both a matte feeling and anti-fingerprint property on the surface of the decorative sheet can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] [ Figure 1 ] is a cross-sectional view showing a structural example of a decorative sheet involved in the first embodiment of the present disclosure.

[0018] [ Figure 2 ] is a cross-sectional photograph showing a configuration example of the first surface protection layer of the decorative sheet involved in the first embodiment of the present disclosure.

[0019] [ Figure 3 ] is a schematic diagram showing an example of a method for manufacturing a decorative sheet involved in the first embodiment of the present disclosure.

[0020] [ Figure 4 ] is a cross-sectional view showing a structural example of a decorative sheet involved in the second embodiment of the present disclosure.

[0021] [ Figure 5 ] is a planar photograph showing a structural example of the surface of the first surface protection layer of the decorative sheet involved in the second embodiment of the present disclosure.

[0022] [ Figure 6 ] is a cross-sectional photograph showing a configuration example of the first surface protection layer of the decorative sheet involved in the second embodiment of the present disclosure.

[0023] [ Figure 7 ] is an enlarged cross-sectional view showing a structural example of a decorative sheet involved in the second embodiment of the present disclosure.

[0024] [ Figure 8 ] is a process diagram showing an example of a method for manufacturing a transfer original plate used in the manufacture of a decorative sheet involved in the second embodiment of the present disclosure.

[0025] [ Fig. 9 ] is a schematic diagram showing an example of a method for manufacturing a decorative sheet involved in the second embodiment of the present disclosure.

[0026] [ Fig.10 ] is a cross-sectional view showing a configuration example of a decorative sheet according to a third embodiment which is a modified example of the decorative sheet according to the first embodiment of the present disclosure.

[0027] [ Fig.11 ] is a cross-sectional view showing a configuration example of a decorative sheet according to a third embodiment which is a modified example of the decorative sheet according to the first embodiment of the present disclosure.

[0028] [ Fig.12 ] is a cross-sectional view showing a configuration example of a decorative sheet according to a third embodiment which is a modified example of the decorative sheet according to the first embodiment of the present disclosure.

[0029] [ Fig.13 ] is a cross-sectional view showing a configuration example of a decorative sheet according to a third embodiment which is a modified example of the decorative sheet according to the first embodiment of the present disclosure.

[0030] [ Fig.14 ] is a cross-sectional view showing a structural example of a decorative panel involved in the fourth embodiment of the present disclosure. DETAILED DESCRIPTION

[0031] The present disclosure is described below through embodiments, but the following embodiments do not limit the invention involved in the claims. In addition, not all combinations of the features described in the embodiments are necessary for the solution of the invention. In addition, the drawings schematically illustrate the invention involved in the claims, and the dimensions such as the width and thickness of each part are different from the actual situation, and their ratios are also different from the actual situation.

[0032] The decorative sheet of the present disclosure is described. The decorative sheet involved in the present disclosure is, for example, a decorative sheet applied to a wall surface, a door or window, a piece of furniture, etc. It should be noted that in the following description, the side of the decorative sheet in contact with the substrate is sometimes referred to as "lower" and the side (surface) opposite to the side in contact with the substrate is sometimes referred to as "upper".

[0033] Below, refer to Figures 1 to 14 Each mode of each embodiment of the present disclosure will be described.

[0034] 1. First Implementation

[0035] use Figures 1 to 3 A decorative sheet 1 according to a first embodiment of the present disclosure will be described.

[0036] (1.1) Basic composition of decorative sheets

[0037] use Figure 1 A basic configuration of a decorative sheet according to a first embodiment of the present disclosure will be described. Figure 1 1 is a cross-sectional view for explaining a configuration example of the decorative sheet 1 according to the first embodiment of the present disclosure. Figure 1 As shown, the decorative sheet 1 includes a raw material layer 11, a colored pattern layer 12, and a first surface protection layer 13. The decorative sheet 1 is composed of the raw material layer 11, the colored pattern layer 12, and the first surface protection layer 13 stacked in this order.

[0038] The raw material layer 11 is a layer that becomes the base material of the decorative sheet 1, and is a layer used to absorb the unevenness or step difference of the pasting surface to complete the construction of the decorative sheet 1 well and conceal the color / pattern of the pasting surface. The colored pattern layer 12 is a layer that gives at least one of color and pattern to the decorative sheet 1. The first surface protection layer 13 is a layer used to protect the raw material layer 11 and the colored pattern layer 12 from damage.

[0039] Hereinafter, each of the raw material layer 11 , the colored pattern layer 12 , and the first surface protection layer 13 will be described in detail.

[0040] <Raw material layer>

[0041] The raw material layer 11 is a layer (sheet) serving as a base material of the decorative sheet 1 .

[0042] The raw material layer 11 is, for example, a paper material mainly composed of pulp or cellulose fibers, or a resin layer or a resin sheet formed of a resin material.

[0043] When the raw material layer 11 is a paper material, additives such as a paper strength enhancer, an additive for improving concealment, cellulose nanofibers, and a colorant may be added.

[0044] In addition, when the raw material layer 11 is a resin material, it is preferable to use a thermoplastic resin represented by polypropylene, polyethylene, and polyester as the resin material. The thermoplastic resin may contain, for example, an inorganic material such as titanium oxide and calcium carbonate as an additive. By using at least one of polypropylene, polyethylene, and polyester as the thermoplastic resin, the dispersibility of the inorganic material is improved. In addition, by using polypropylene as the thermoplastic resin, the dispersibility of the inorganic material is further improved.

[0045] In addition, when the raw material layer 11 is a resin film, as the resin film, a film material mainly composed of polyethylene terephthalate is preferred. The resin film may contain the above-mentioned inorganic material as an additive. In addition, when the raw material layer 11 is a resin film, the raw material layer 11 may be a resin film formed by uniaxial or biaxial stretching. The raw material layer 11 formed by the resin film formed by uniaxial or biaxial stretching may contain voids inside.

[0046] When the raw material layer 11 is a resin material or a resin film, the content of the inorganic material relative to the raw material layer 11 is preferably set in the range of 1 mass % to 90 mass %, more preferably in the range of 5 mass % to 80 mass %, and further preferably in the range of 20 mass % to 80 mass %. By setting the content of the inorganic material in the above range, sufficient non-combustibility or sufficient flame retardancy can be reliably obtained, while the printing adaptability and lamination adaptability can be reliably improved, and cracks generated in the curved portion of the sheet can be reliably reduced.

[0047] The thickness of the raw material layer 11 is preferably within a range of 20 μm to 250 μm, more preferably within a range of 25 μm to 250 μm, and further preferably within a range of 70 μm to 200 μm. When the thickness of the raw material layer 11 is within the above range, lamination adaptability can be improved and cracks generated in the bent portion of the sheet can be reduced.

[0048] The surface of the raw material layer 11 may be subjected to a surface treatment such as a corona treatment or a plasma treatment. This improves the adhesion (closeness) between the raw material layer 11 and the colored pattern layer 12.

[0049] <Coloring pattern layer>

[0050] The colored pattern layer 12 is provided on one surface of the raw material layer 11. The colored pattern layer 12 includes, for example, a colored layer 12A provided on the raw material layer 11 and a pattern layer 12B provided on the colored layer 12A. It should be noted that the colored pattern layer 12 may include at least one of the colored layer 12A and the pattern layer 12B according to the desired design.

[0051] The colored layer 12A is a layer for imparting a desired color design to the decorative sheet 1 and concealing the color and pattern of the base material to which the decorative sheet 1 is attached. The colored layer 12A is formed by, for example, solid application of ink.

[0052] The pattern layer 12B is provided on the surface side of the decorative sheet 1 more than the colored layer 12A, and is a layer that imparts a desired pattern to the decorative sheet 1. The pattern layer 12B is formed on the colored layer 12A, and is formed by printing, for example, a wood grain pattern, a stone grain pattern, a sand grain pattern, a tile pattern, a brick pattern, a cloth grain pattern, a leather grain pattern, a geometric pattern, or other patterns.

[0053] The coloring layer 12A and the pattern layer 12B are formed by, for example, screen printing using ink. As the ink used to form the coloring layer 12A and the pattern layer 12B, for example, isoindolinone yellow, polyazo red, phthalocyanine blue, carbon black, iron oxide, titanium oxide, or a mixture thereof can be used as a pigment. In addition, these inks may be aqueous solvents or organic solvents. As the organic solvent, for example, ethyl acetate, n-butyl acetate, isobutyl alcohol, methyl isobutyl ketone, etc. can be used.

[0054] The thickness of the colored layer 12A and the pattern layer 12B of the colored pattern layer 12 can be any thickness that fully expresses the desired degree of design. The thickness of the colored layer 12A is preferably set in a range of 2 μm to 20 μm, for example. By setting the thickness of the colored layer 12A within the above range, for example, even when colored in white or light colors, the color and stains of the original material layer 11 can be sufficiently concealed, and the reduction in the adhesion strength between the ink layers constituting the colored layer 12A can be prevented, so that sufficient durability can be obtained. In addition, the thickness of the pattern layer 12B is preferably set in a range of 0.1 μm to 10 μm, for example. Here, the "thickness of the pattern layer 12B" refers to the thickness of the portion printed with ink. The pattern layer 12B may not be provided on the entire surface of the colored layer 12A, and the colored layer 12A may be exposed from the pattern layer 12B. By setting the thickness of the pattern layer 12B within the above range, the pattern can be clearly expressed, or the design can be improved by adding gradations to the pattern. In addition, when multiple colors are printed in an overlapping manner, the color of the upper layer overlaps with the color of the lower layer, thereby increasing the color width that can be expressed by limited colors.

[0055] <First surface protective layer>

[0056] The first surface protection layer 13 is arranged on the surface of the colored pattern layer 12 on the opposite side of the raw material layer 11, and has a concavo-convex shape on the surface. The first surface protection layer 13 includes a core 13A as a lower layer (back side) area in the layer, and a protrusion 13B (an example of a convex protrusion) as an upper layer (surface side) area in the layer, and has a concavo-convex shape on the surface. The first surface protection layer 13 has a core 13A and a protrusion 13B that is arranged to protrude in a ridge shape from one surface of the core 13A. Thus, a concavo-convex shape is formed on the surface of the first surface protection layer 13.

[0057] Figure 2 It is a cross-sectional photograph which shows the structure of the surface (upper surface) of the first surface protection layer 13 . Figure 2 13B is a cross-sectional photograph and a cross-sectional view showing a cross section in the width direction of the protruding portion 13B. Figure 2 These are plan and cross-sectional photographs obtained using an optical microscope (digital microscope, VHX-6000 manufactured by KEYENCE).

[0058] like Figure 2 As shown in the cross-sectional photograph of , the protrusion 13B has a concave-convex shape formed by mechanical processing such as embossing. The height of such a protrusion 13B is preferably greater than 15 μm, for example. In addition, the period p of adjacent protrusions 13B (for example, the interval between the vertices of the protrusion 13B) is preferably greater than 50 μm.

[0059] The first surface protection layer 13 is formed of a resin material. The resin material may be any of an ionizing radiation curable resin, a thermosetting resin, a thermoplastic resin, and the like.

[0060] For example, as the ionizing radiation curable resin, for example, an ultraviolet curable resin can be used. As the ultraviolet curable resin, for example, (meth) acrylic resin, silicone resin, polyester resin, urethane resin, amide resin, epoxy resin can be used. The ultraviolet curable resin can be any of a water-based resin or a non-aqueous (organic solvent-based) resin.

[0061] The first surface protection layer 13 may contain inorganic particles. As inorganic particles, for example, microparticles formed by inorganic materials such as silicon dioxide, glass, aluminum oxide, titanium dioxide, zirconium oxide, calcium carbonate, and barium sulfate can be listed. Preferably, relative to 100 parts by mass of ionizing radiation curing resin, the amount of inorganic particles added in the first surface protection layer 13 is more than 0% by mass and less than 5% by mass, preferably more than 0% by mass and less than 3% by mass, more preferably more than 0% by mass and less than 1% by mass, and further preferably in the range of more than 0.1% by mass and less than 0.5% by mass. The first surface protection layer 13 is preferably preferred because the wear resistance and damage resistance are improved by containing the above-mentioned amount of inorganic particles. In addition, when the first surface protection layer 13 contains inorganic particles, the damage resistance is improved compared with the case where no inorganic particles are contained, but when the content of inorganic particles is too much, the inorganic particles fall off from the surface of the first surface protection layer 13, or the fingerprint resistance such as fingerprint attachment is adversely affected. Therefore, the amount of inorganic particles added is preferably more than 0 mass % and less than 3 mass %.

[0062] As required, for example, one or more additives selected from colorants, matte agents, fillers, ultraviolet absorbers, light stabilizers, heat stabilizers, antioxidants, antistatic agents, lubricants, flame retardants, antibacterial agents, mildew-proof agents, friction reducers, and light scattering agents may be added to the first surface protection layer 13. However, the first surface protection layer 13 does not contain a gloss regulator that reduces oleophobicity and makes fingerprints more likely to adhere.

[0063] The first surface protection layer 13 only needs to completely cover the colored pattern layer 12, and can function as a surface protection layer on the entire surface of the decorative sheet 1. In addition, the density of the first surface protection layer 13 can be adjusted according to the target gloss and performance.

[0064] The thickness of the first surface protective layer 13 is preferably set in the range of 20 μm or more and 50 μm or less. By setting the thickness of the first surface protective layer 13 in the above range, the design can be protected by protecting the raw material layer 11 and the colored pattern layer 12 to prevent damage. When the thickness of the first surface protective layer 13 is 20 μm or more, it can fully have the functions such as wear resistance required as a surface protective layer. In addition, when the thickness of the first surface protective layer 13 is 50 μm or less, the first surface protective layer 13 will not be unnecessarily thickened, thereby having the effect of not excessively increasing the manufacturing cost.

[0065] (1.2) Method for manufacturing decorative sheet

[0066] Figure 3 1 is a schematic diagram for explaining a method for manufacturing a decorative sheet 1. Figure 3As shown, the decorative sheet 1 is formed by extrusion molding using metal rollers 101 and 102 with flat surfaces, a metal roller 110 with a desired concavo-convex shape on the surface, a T-die 104, and an ultraviolet lamp 105. The resin material constituting the first surface protection layer 13 of the decorative sheet 1 may be any of ionizing radiation curing resin, thermosetting resin, or thermoplastic resin, but the case of using an ultraviolet curing resin as an ionizing radiation curing resin is described below.

[0067] First, a resin film is used as the raw material layer 11, and a desired color ink is printed on the raw material layer 11 to form the coloring layer 12A. Next, a desired color ink is printed in a desired pattern on the coloring layer 12A to form the pattern layer 12B. In this way, the laminate 50 is formed.

[0068] Then, if Figure 3 As shown, the ultraviolet curing resin 13' is ejected toward the laminated body 50 using, for example, a T-die 104. At this time, the ultraviolet curing resin 13' is ejected so as to be on the side of the metal roller 110 having a desired concavo-convex shape on the surface.

[0069] The concavoconvex shape on the surface of the metal roller 110 is transferred to the ultraviolet curing resin 13' ejected onto the laminate 50. Then, ultraviolet rays having a wavelength of 400 nm or less are irradiated by the ultraviolet lamp 105 to cure the ultraviolet curing resin 13'.

[0070] Thus, the decorative sheet 1 including the first surface protection layer 13 having a concavo-convex shape and having the core portion 13A and the protruding portion 13B provided to protrude in a ridge shape from one surface of the core portion 13A is formed.

[0071] It should be noted that the first surface protection layer 13 formed in this way is formed of a resin material having a substantially uniform composition throughout the first surface protection layer 13 .

[0072] In the above, the decorative sheet 1 including the first surface protection layer 13 having the protruding portion 13B has been described, but the present invention is not limited to such a configuration.

[0073] For example, the first surface protection layer 13 may also have a concave-convex shape formed by providing a concave groove on the surface instead of a protrusion (an example of a convex protrusion). In this case, the depth of the concave groove is equivalent to the height of the protrusion 13B recorded in this embodiment, and the spacing of the concave groove is equivalent to the spacing of the protrusion 13B.

[0074] <Effects of the First Embodiment>

[0075] The decorative sheet 1 according to the present embodiment has the following effects.

[0076] (1) The decorative sheet 1 of the present embodiment includes the first surface protection layer 13 having a concavo-convex shape formed on the surface.

[0077] According to this configuration, even if the first surface protective layer 13 does not contain a gloss regulator (matting additive), the gloss (glossiness) of the first surface protective layer 13 can be adjusted. The gloss regulator reduces the oleophobicity of the layer formed by the resin material, so fingerprints are easily attached. Since the first surface protective layer 13 does not contain a gloss regulator, it does not absorb oil and the oleophobicity is relatively improved. Therefore, in various occasions such as on-site construction, furniture assembly, and daily life of residents, it is difficult for fingerprints to adhere to the decorative sheet 1 having the first surface protective layer 13.

[0078] (2) The decorative sheet 1 of the present embodiment includes the first surface protection layer 13 having a concavo-convex shape formed on the surface.

[0079] According to this configuration, the oil repellency of the first surface protection layer 13 is improved, and adsorption of oil stains and contaminants on the surface of the decorative sheet 1 can be suppressed.

[0080] 2. Second Implementation

[0081] use Figures 4 to 9 A decorative sheet 2 according to a second embodiment of the present disclosure will be described.

[0082] The decorative sheet 2 according to the second embodiment has the same structure as the decorative sheet 1 according to the first embodiment. The decorative sheet 2 according to the second embodiment is different from the decorative sheet 1 according to the first embodiment in that the decorative sheet 2 is formed using a transfer original plate manufactured by a method different from the method for manufacturing the transfer original plate used in manufacturing the decorative sheet 1 according to the first embodiment.

[0083] Hereinafter, the structure of the decorative sheet 2 according to the second embodiment, the method for producing the transfer original plate, and the method for producing the decorative sheet 2 will be described. The basic structure of the decorative sheet 2 is the same as that of the decorative sheet 1 according to the first embodiment, and only the different parts will be described.

[0084] (2.1) Basic composition of decorative sheets

[0085] like Figure 4 As shown, the decorative sheet 2 includes a raw material layer 11, a colored pattern layer 12, and a first surface protection layer 23. The raw material layer 11 and the colored pattern layer 12 are the same as those of the decorative sheet 1 according to the first embodiment, and thus their description is omitted.

[0086] <First Surface Protective Layer>

[0087] The first surface protection layer 23 is provided on the surface of the colored pattern layer 12 on the opposite side to the raw material layer 11. The first surface protection layer 23 includes a core portion 23A as a lower layer (back side) region within the layer, and a ridge portion 23B (an example of a convex protrusion) as an upper layer (surface side) region within the layer.

[0088] Figure 5 This is a plan view showing the structure of the surface (upper surface) of the first surface protection layer 23. Figure 6 2 is a cross-sectional photograph showing the structure of the surface (upper surface) of the first surface protection layer 23. Figure 7 It is a cross-sectional view schematically showing the structure of the surface (upper surface) of the first surface protection layer 23 . Figure 6 and Figure 7 2 is a cross-sectional photograph and a cross-sectional view showing a cross section in the width direction of the ridge portion 23B. Here, Figure 5 and Figure 6 These are plan and cross-sectional photographs obtained using an optical microscope (digital microscope, VHX-6000 manufactured by KEYENCE).

[0089] like Figure 5 As shown, the ridge 23B is a shape that is slenderly raised and connected in a linear shape in a plan view. As described later, the ridge 23B is formed using a transfer master formed by irradiating the surface of the ionizing radiation curing resin with ionizing radiation of a specific wavelength to shrink the surface of the ionizing radiation curing resin.

[0090] Here, in the decorative sheet 2 of the present embodiment, "ridge-like" means a shape that is elongated and connected in a linear shape in a plan view. The ridge-like portion 23B may be curved or straight in a plan view, but Figure 6 and Figure 7 As shown, from the viewpoint of anti-fingerprint property of the surface of the decorative sheet 2, it is preferably in a curved shape. In addition, in the present disclosure, the ridge portion 23B is, for example, a portion from the lowest portion to the top of the concave-convex shape provided on the surface of the first surface protection layer 23, and the core portion 23A refers to the portion of the first surface protection layer 23 other than the ridge portion 23B.

[0091] The height of such a ridge 23B is, for example, preferably less than 15 μm, more preferably less than 8 μm. In addition, the period p of adjacent ridges 23B (for example, the interval between the vertices of the ridge 23B) is preferably less than 50 μm, preferably less than 10 μm, and more preferably less than 6.5 μm. Compared with the concave-convex shape formed on the surface of the surface protection layer by mechanical processing such as embossing, the concave-convex shape (ridge 23B) on the surface of the first surface protection layer 23 manufactured by using a transfer original plate formed by irradiating high-energy ionizing radiation to an ionizing radiation-curing resin has a fine structure. By forming such a fine concave-convex shape on the surface of the first surface protection layer 23, the fingerprint resistance can be improved while maintaining the matte feel of the surface of the decorative sheet 2.

[0092] As the ionizing radiation curable resin, for example, an ultraviolet curable resin can be used. As the ultraviolet curable resin, for example, a (meth) acrylic resin, a silicone resin, a polyester resin, a urethane resin, an amide resin, and an epoxy resin can be used. The ultraviolet curable resin can be any of an aqueous resin or a non-aqueous (organic solvent-based) resin.

[0093] The first surface protection layer 23 may contain the same inorganic particles as those of the first surface protection layer 13 .

[0094] In addition, similarly to the first surface protection layer 13, as required, for example, one or more additives selected from colorants, matte agents, fillers, ultraviolet absorbers, light stabilizers, heat stabilizers, antioxidants, antistatic agents, lubricants, flame retardants, antibacterial agents, mildewproof agents, friction reducers, and light scattering agents can be added to the first surface protection layer 23. However, the first surface protection layer 23 does not contain a gloss regulator that reduces oleophobicity and makes it easy to attach fingerprints.

[0095] The thickness of the first surface protective layer 23 is preferably set in the range of 1.0 μm or more and 50 μm or less. By setting the thickness of the first surface protective layer 23 in the above range, the design can be protected by protecting the raw material layer 11 and the colored pattern layer 12 to prevent damage. When the thickness of the first surface protective layer 23 is 1.0 μm or more, it can fully have the functions such as wear resistance required as a surface protective layer. In addition, when the thickness of the first surface protective layer 23 is 50 μm or less, the first surface protective layer 23 will not be unnecessarily thickened, thereby having the effect of not excessively increasing the manufacturing cost.

[0096] Although such a decorative sheet 2 does not contain a gloss regulator (matting additive), its glossiness is less than 5.0, thus becoming a decorative sheet with extremely low glossiness. In conventional decorative sheets, when the glossiness of a decorative sheet having a surface protective layer is about 8 or less, the content of the gloss regulator in the surface protective layer is high, and the surface protective layer becomes turbid. Therefore, the color and pattern of the colored pattern layer may not be clearly expressed, or the design of the decorative sheet may be reduced. In addition, in the case of obtaining a decorative sheet with a glossiness close to 0, the content of the gloss regulator in the surface protective layer is further increased, so when forming the surface protective layer, it is difficult to form a surface protective layer with a smooth surface without generating streaks, spots, etc.

[0097] A decorative sheet with a low gloss of 5.0 or less, preferably 2.0 or less, can be obtained while maintaining the same performance of the decorative sheet 2 as a decorative sheet having a gloss of 20±3 or more. Here, "gloss" is a measured value when measured at an incident angle of 60 degrees using a gloss meter gloss measuring device. Therefore, a decorative sheet 2 with high oleophobicity and difficulty in fingerprint adhesion can be obtained while maintaining the performance required as a decorative sheet 2.

[0098] (2.2) Method for manufacturing decorative sheet

[0099] <Method for producing original plate for transfer>

[0100] Reference Figure 8 and Fig. 9 , a method for producing a transfer original plate and a method for producing a decorative sheet using the transfer original plate are described. Figure 8 2 is a cross-sectional process diagram showing a method for manufacturing a transfer original plate according to a second embodiment. Fig. 9 It is a cross-sectional process diagram showing a method for producing a decorative sheet according to the second embodiment.

[0101] like Figure 8 As shown in (A), a resin film is used as a substrate 201, and an ionizing radiation curing resin 203A is applied on the substrate 201. At this time, the application amount of the ionizing radiation curing resin 203A is adjusted to a thickness that can obtain a desired concavo-convex height.

[0102] Then, if Figure 8As shown in (B), the surface coated with the ionizing radiation curing resin 203A is irradiated with a first ionizing radiation having an energy capable of cutting at least one of a carbonyl bond and a carbon-carbon bond to shrink the surface of the ionizing radiation curing resin 203A. The first ionizing radiation may be a single ionizing radiation having a predetermined wavelength, or may be a plurality of ionizing radiations having different wavelengths. As the first ionizing radiation, for example, an excimer laser having high energy may be cited. The medium of the excimer laser may be any medium (discharge gas) used in the past, as long as it has an energy capable of cutting at least one of a carbonyl bond and a carbon-carbon bond. As the discharge gas, a rare gas such as Xe, Ar, Kr, or a mixed gas of a rare gas such as ArBr, ArF, KrCl, XeI, XeCl, XeBr, KrBr, KrF and a halogen gas may be used. The wavelength (center wavelength) of excimer laser varies depending on the medium, for example, it has wavelengths of about 172nm (Xe), about 126nm (Ar), about 146nm (Kr), about 165nm (ArBr), about 193nm (ArF), about 222nm (KrCl), about 253nm (XeI), about 308nm (XeCl), about 283nm (XeBr), about 207nm (KrBr), and about 248nm (KrF).

[0103] By irradiating the ionizing radiation curing resin 203A with high energy ionizing radiation, a concavo-convex shape is formed on the surface of the ionizing radiation curing resin 203A. At this time, the shrinkage rate of the ionizing radiation curing resin 203A is adjusted by adjusting the resin coating amount of the ionizing radiation curing resin 203A and the ionizing radiation irradiation time. Thus, the final gloss of the decorative sheet 2 to which the concavo-convex shape is transferred can be adjusted.

[0104] When forming a concavoconvex shape, by changing the type of the first ionizing radiation irradiated on the ionizing radiation curing resin 203A, the tactile feel and visual effect of the surface of the decorative sheet 2 on which the concavoconvex shape is transferred can be changed. For example, the ionizing radiation curing resin 203A is irradiated with a first ionizing radiation having a wavelength of about 250nm, and then the first ionizing radiation having a wavelength of about 172nm is irradiated to form a concavoconvex shape, and then the ionizing radiation curing resin 203A is cured. Thus, the tactile feel (hand feel) of the decorative sheet 2 can be adjusted. In addition, for example, the ionizing radiation curing resin 203A can be irradiated with a first ionizing radiation having a wavelength of about 172nm to form a concavoconvex shape, and then the ionizing radiation curing resin 203A is cured. Thus, the surface of the decorative sheet 2 on which the concavoconvex shape is transferred can be smoothed and adjusted to a low gloss, or a glossy matte effect (visual embossing feeling) can be given to the surface of the decorative sheet 2.

[0105] Then, if Figure 8As shown in (C), the ionizing radiation curing resin 203A after the surface shrinkage is irradiated with a second ionizing radiation to cure the ionizing radiation curing resin 203A. Thus, a resin layer 203 having a concave-convex shape 203B on the surface is formed. As the second ionizing radiation, for example, ultraviolet rays with a wavelength of 400nm or less can be cited. The ionizing radiation that cures the ionizing radiation curing resin 203A has a wide band (i.e., a broad spectrum) within a range of 400nm or less.

[0106] Thus, the transfer original plate 200 having the concavo-convex shape 203B on the surface is obtained.

[0107] Here, the concavo-convex shape 203B formed by the contraction of the ionizing radiation curing resin 203A has a different composition from the uncontracted portion of the ionizing radiation curing resin 203A. Specifically, the concavo-convex shape 203B formed by the contraction of the ionizing radiation curing resin 203A has a composition in which the ratio of carbonyl bonds (C=O) and carbon-carbon bonds (double bonds (C=C) and triple bonds (C≡C) of carbon and carbon) contained in the resin is reduced compared to the uncontracted portion of the ionizing radiation curing resin 203A in the deep layer. For example, the ratio of carbonyl bonds and carbon-carbon bonds contained in the resin in the concavo-convex shape 203B is preferably reduced by 10% or more, and more preferably reduced by 20% or more compared to the uncontracted portion of the ionizing radiation curing resin 203A in the deep layer. This is because the polymer chains (carbonyl bonds and carbon-carbon bonds (double bonds, triple bonds)) contained in the resin are broken by irradiating the ionizing radiation curing resin 203A with high energy. In the ionizing radiation curing resin 203A irradiated with high-energy ionizing radiation, new bonds are generated in the broken portions (rebonding, re-crosslinking), so that the surface of the ionizing radiation curing resin 203A shrinks to form the concavo-convex shape 203B. Such a difference in composition between the unshrinked portion of the ionizing radiation curing resin 203A and the concavo-convex shape 203B is a feature when the concavo-convex shape 203B is formed by irradiating ionizing radiation.

[0108] In addition, by irradiating the ionizing radiation curing resin 203A with high energy ionizing radiation, the polymer chains contained in the resin are cut, and rebonded and recrosslinked in a state where hydrogen atoms are abstracted. Therefore, compared with the uncontracted part of the ionizing radiation curing resin 203A in the deep layer, the concavo-convex shape 203B formed by the cutting of the polymer chains and the rebonding and recrosslinking has a high crosslinking density. Therefore, the porosity in the resin constituting the concavo-convex shape 203B as the outermost layer of the transfer original plate 200 is reduced, and the surface hardness of the transfer original plate 200 is improved.

[0109] Such a concavo-convex shape 203B is in a curved shape in the cross-sectional view. The concavo-convex shape 203B is formed by shrinkage due to ablation of the ionizing radiation curing resin 203A after irradiation with ionizing radiation of a specific wavelength. That is, by irradiating the surface of the ionizing radiation curing resin 203A with a strong laser, the ionizing radiation curing resin 203A on the surface that has locally become high temperature evaporates, and atoms, molecules, plasma and their clusters fly away, thereby forming the concavo-convex shape 203B. In this way, the concavo-convex shape 203B in a curved shape in the cross-sectional view has the same characteristics as the concavo-convex shape, i.e., the ridge-shaped portion 23B, which is formed on the surface of the surface protection layer by mechanical processing such as embossing (see Figure 4 ) are of distinctly different shapes.

[0110] Therefore, a smooth concavo-convex shape 203B is formed on the surface of the resin layer 203 due to surface tension. Specifically, the free radicals of the above-mentioned ionizing radiation directly cut the carbonyl bond and the double bond or triple bond between carbon and carbon in the resin constituting the ionizing radiation curing type resin 203A. In addition, by irradiation with high-energy ionizing radiation such as vacuum ultraviolet light, ozone or oxygen free radicals are generated from oxygen molecules, and the free radicals generated in this way may cut the carbonyl bond and the double bond or triple bond between carbon and carbon. In this case, ozone or oxygen free radicals are generated from oxygen molecules whose concentration (for example) is limited to 2000ppm, preferably 1000ppm or less, and more preferably 400ppm or less in a vacuum atmosphere. The cut bonds are re-bonded with adjacent atoms such as carbon, oxygen, nitrogen, or free radicals present in the atmosphere, causing the surface of the ionizing radiation curing type resin 203A to shrink, thereby forming a gentle curve shape. Such gentle shapes of the concavo-convex shapes 203B are also a feature of the transfer original plate 200 on which concavo-convex shapes are formed on the surface by irradiation with ionizing radiation.

[0111] The height of the concavo-convex shape 203B on the surface of such a transfer original plate 200 is, for example, preferably less than 15 μm, more preferably less than 8 μm. In addition, the period p of adjacent concavo-convex shapes 203B (for example, the interval between the vertices of the concavo-convex shapes 203B) is preferably less than 50 μm, preferably less than 10 μm, and more preferably less than 6.5 μm. Compared with the concavo-convex shape formed on the surface of the surface protection layer by mechanical processing such as embossing, the concavo-convex shape 203B on the surface of the transfer original plate 200 formed by irradiating high-energy ionizing radiation to the ionizing radiation curing resin 203A has a fine structure. By using the transfer original plate 200 to transfer such a fine concavo-convex shape 203B on the surface of the first surface protection layer 23, the fingerprint resistance can be improved while maintaining the matte feeling of the surface of the decorative sheet 2.

[0112] The following describes in more detail the mechanism by which the concavo-convex shape 203B is formed by irradiation with the first ionizing radiation.

[0113] Vacuum ultraviolet light (VUV) can use photon energy to cut bond energy that is less than the photon energy. Therefore, by irradiating the surface of the ionizing radiation curing resin 203A with vacuum ultraviolet light, the molecular bonds of the organic matter in the ionizing radiation curing resin 203A can be cut, and the bonding state of the polymer on the surface of the ionizing radiation curing resin 203A changes, thereby modifying (shrinking) the surface.

[0114] When rare gas, halogen gas and mercury are combined as the medium of the first ionizing radiation, a light source close to monochromatic light can be obtained with a wavelength interval of 20nm to 30nm within a range of 100nm to 500nm. As the first ionizing radiation for forming the concave-convex shape 203B, any of these light sources can be used. However, when considering the size of the obtained photon energy, the difference between the wavelength and the bond energy of the organic matter, it is most preferred to use a xenon lamp that emits an excimer laser with a central wavelength of 172nm as the light source. The lower the wavelength and the stronger the energy of the first ionizing radiation, the more it can cut the molecular bonds of the organic matter and thus the easier it is to cause surface shrinkage, so it is preferred. On the other hand, when considering the cost of equipment maintenance, the acquisition of materials, etc., it is most preferred to use a xenon lamp as the light source.

[0115] Here, light with a wavelength of less than 380nm is called ultraviolet light (UV), and light with a wavelength of less than 200nm is called vacuum ultraviolet light (VUV), and the light is absorbed by oxygen in the atmosphere and attenuated. Therefore, by removing the oxygen under the first ionizing radiation irradiation environment, the surface modification effect of the ionizing radiation curing resin 203A can be further improved. In addition, it is preferred that the required reaction gas (for example, nitrogen) is introduced to control the reaction atmosphere, or a chamber system in which the oxygen concentration is suppressed to less than 2000ppm is used to irradiate the ionizing radiation curing resin 203A with ultraviolet light (especially, light less than 250nm). The light energy cuts off the molecular bonds of the organic substance in the ionizing radiation curing resin 203A, hydrogen atoms are extracted, and the molecular composition is easily changed, thereby easily causing the surface modification (contraction) of the ionizing radiation curing resin 203A.

[0116] In order to prevent stains such as hand oil and fingerprints from adhering to the resin surface, it is necessary to have oleophobicity. Therefore, by irradiating the ionizing radiation with the oxygen concentration in the ionizing radiation irradiation atmosphere as low as possible (ideally under the condition of 400 ppm or less), the performance of the decorative sheet for the purpose of this application can be exhibited. By adjusting the oxygen concentration during light irradiation, the desired surface performance can be exhibited.

[0117] The photons excited by the irradiation of the excimer laser are strongly absorbed into the polymer chains of the ionizing radiation curing resin 203A as the surface protective layer on the surface of the decorative sheet until they reach a depth of about tens to hundreds of nanometers of the ionizing radiation curing resin 203A, generating polymer free radicals. Through the polymer free radicals, the polymer chains of the ionizing radiation curing resin 203A are cut, rebonded, and recrosslinked. As a result, the molecular weight increases on the surface of the ionizing radiation curing resin 203A, and the free volume (void ratio) in the polymer decreases, thereby generating fine concave and convex shapes 203B connected in a wave-like manner like folded folds.

[0118] The period (pitch of concavities and convexities) I of the contracted microstructure generated by irradiating the ionizing radiation-curing resin 203A with an excimer laser can be obtained according to the Polanyi equation represented by the following equation (1) and the Polanyi equation represented by equation (2) focusing on the 0th-order diffracted light and the 1st-order diffracted light.

[0119]

[0120] I·sin[arctan(x / d)]=λ···(2)

[0121] Here, in formula (1), I is the period of the microstructure, is the angle of the diffracted light of the excimer laser, m is an integer greater than 0, and λ is the wavelength of the excimer laser. In addition, in formula (2), x is the distance between the 0th order diffracted light and the 1st order diffracted light on the screen, and d is the distance between the screen on which the diffracted light is projected and the ionizing radiation curing resin 203A as a sample.

[0122] By changing the incident angle θ of the laser irradiated to the ionizing radiation curing resin 203A, the pattern of the contracted microstructure produced in the ionizing radiation curing resin 203A can be controlled. When the incident angle of the excimer laser is close to 0 degrees, the pattern of the microstructure is isotropic relative to the laser irradiation part, and a random microstructure is produced. On the other hand, the larger the incident angle θ of the laser, the greater the anisotropy of the pattern of the microstructure relative to the laser irradiation part. The surface shape of the ionizing radiation curing resin 203A that has shrunk due to the laser with an incident angle of 0 degrees is effective for (for example) improving fingerprint resistance, contamination resistance, and damage resistance. This is because, by isotropically arranged random microstructures, the adhesion, damage, gloss changes, etc. of pollutants become less obvious. The interval (period) I of the microstructure formed by irradiating the laser at an incident angle of 0 degrees is approximately the same as the wavelength λ of the irradiated excimer laser. In addition, when the incident angle θ is changed, the interval I changes while the shape of the microstructure maintains a vertical stripe pattern. The interval I is obtained by the following formula (3) based on the incident angle θ of the laser light.

[0123] I=λ / cosθ···(3)

[0124] <Method for producing decorative sheet>

[0125] like Fig. 9 As shown in (A), a resin film is used as the raw material layer 11, and a desired color ink is printed on the raw material layer 11 to form a coloring layer 12A. Next, a desired color ink is printed in a desired pattern on the coloring layer 12A to form a pattern layer 12B.

[0126] Then, if Fig. 9 As shown in FIG. 2B , an ionizing radiation curing resin 23' is applied to the colored layer 12A (colored pattern layer 12) formed with the pattern layer 12B. At this time, the amount of the ionizing radiation curing resin 23' applied is at least enough to completely cover the colored pattern layer 12, and can be adjusted according to the target gloss and performance, for example, preferably 2.0 g / m 2 Above 20g / m 2 Below left and right.

[0127] Then, if Fig. 9 As shown in (C), the concavo-convex shape 203B is transferred to the ionizing radiation curing resin 23' using the transfer original plate 200. Fig. 9As shown in FIG. 2 , the ionizing radiation curing resin 23′ having the concavo-convex shape 203B of the transfer original plate 200 transferred on its surface is irradiated with a second ionizing radiation to cure the ionizing radiation curing resin 23′. Here, the second ionizing radiation can be the same as the second ionizing radiation used to cure the ionizing radiation curing resin when manufacturing the transfer original plate 200.

[0128] Thus, the decorative sheet 2 including the first surface protection layer 23 having the concavo-convex shape formed by the core 23A and the ridge 23B provided to protrude in a ridge shape from one surface (upper surface) of the core 23A is formed.

[0129] It should be noted that the first surface protection layer 23 formed in this way is formed of a resin material having a substantially uniform composition throughout the first surface protection layer 23 .

[0130] (2.3) Modification of the method for producing decorative sheet

[0131] In the second embodiment, the transfer original plate 200 including the resin layer 203 having the concavo-convex shape 203B on the surface is formed by irradiating the ionizing radiation curing type resin 203A with high energy ionizing radiation to shrink the surface and then cure it, but the present invention is not limited to this configuration.

[0132] For example, the concavo-convex shape 203B formed on the surface of the resin layer 203 may be measured by a three-dimensional shape measuring device, and concavo-convex shape data representing the concavo-convex shape 203B may be obtained, thereby forming a transfer original having a concavo-convex shape formed based on the concavo-convex shape data. In this case, a transfer original having a concavo-convex shape for the original can be formed by forming a concavo-convex shape for the original corresponding to the concavo-convex shape 203B on the surface of a metal material such as a metal plate or a metal roller based on the concavo-convex shape data by laser engraving or the like.

[0133] <Effects of the Second Embodiment>

[0134] In addition to the effects described in the first embodiment, the decorative sheet 2 according to the present embodiment has the following effects.

[0135] (3) The decorative sheet 2 according to the present embodiment includes the first surface protection layer 23 that does not contain a gloss adjuster.

[0136] According to this configuration, when the surface of the decorative sheet 2 is scratched, the particles of the gloss adjuster do not fall off, and gloss changes and scratches are unlikely to occur on the surface of the decorative sheet 2 .

[0137] (4) The decorative sheet 2 according to the present embodiment includes the first surface protection layer 23 that does not contain a gloss adjuster.

[0138] According to this configuration, the content of the additive in the first surface protective layer 23 can be reduced, so that the first surface protective layer 23 can be prevented from becoming cloudy, and the first surface protective layer 23 can be easily formed.

[0139] (5) The method for producing the decorative sheet 2 according to the present embodiment uses a metal material as a transfer original plate, and therefore can improve the productivity of the decorative sheet compared to the case of using a transfer original plate formed of a resin material.

[0140] 3. Third Implementation

[0141] use Figures 10 to 13 A decorative sheet according to a third embodiment of the present disclosure will be described. Hereinafter, as a third embodiment, first to fifth configuration examples of a decorative sheet manufactured by the manufacturing method according to any one of the first to third embodiments will be described. Figures 10 to 13 The drawings are cross-sectional views respectively showing the structures of the decorative sheet 3B described in the second structure example of the decorative sheet involved in the third embodiment of the present disclosure, the decorative sheet 3C described in the third structure example, the decorative sheet 3D described in the fourth structure example, and the decorative sheet 3E described in the fifth structure example.

[0142] Hereinafter, the decorative sheets according to the first to fifth configuration examples will be described in order.

[0143] (3.1) Construction Example 1

[0144] In Configuration Example 1 of the third embodiment, a decorative sheet 3A (not shown) in which the first surface protection layer 13 is formed into multiple layers will be described.

[0145] The decorative sheet 3A has a first surface protective layer 13 formed by laminating a plurality of identical ionizing radiation curing resins or a first surface protective layer 13 formed by laminating a plurality of different ionizing radiation curing resins, and a concavo-convex shape is provided on the outermost surface of the first surface protective layer 13 .

[0146] (3.2) Example 2

[0147] use Fig.10 A decorative sheet 3B according to Configuration Example 2 of the third embodiment of the present disclosure will be described.

[0148] like Fig.10 As shown, the decorative sheet 3B is composed of a multi-layer structure of a raw material layer 11, a colored pattern layer 12, and a first surface protection layer 13 stacked in sequence. That is, the decorative sheet 3B is different from the decorative sheet 1 involved in the first embodiment in that a first film layer 11A and a second film layer 11B are provided instead of a single raw material layer 11.

[0149] The raw material layer 11 of the decorative sheet 3B will be described in detail below. It should be noted that the layers other than the raw material layer 11 (the colored pattern layer 12 and the first surface protection layer 13) have the same structure as the layers of the decorative sheet 1, and thus description thereof will be omitted.

[0150] <Raw material layer>

[0151] The raw material layer 11 is composed of a first film layer 11A and a second film layer 11B stacked together.

[0152] The first film layer 11A and the second film layer 11B can be resin films formed by the same resin material, or can be resin films formed by different resin materials. For example, the first film layer 11A is a polyethylene film and the second film layer 11B is a polypropylene film. In this case, it is preferred that a colored pattern layer 12 is provided on the first film layer 11A, and an adhesive resin layer 14 and a second film layer 11B are laminated on the colored pattern layer 12. In addition, the first surface protection layer 13 is preferably provided on the second film layer 11B. By such a laminated structure, it is possible to prevent the colored pattern layer 12 from being exposed, thereby reducing the wear resistance, damage resistance, stain resistance and weather resistance. When the colored pattern layer 12 is exposed, the weather resistance is particularly easy to reduce. Therefore, in the case where the decorative sheet is required to have high weather resistance, it is preferred that a decorative sheet 3B is obtained by using a film (the first film layer 11A and the second film layer 11B) as the raw material layer and sandwiching the colored pattern layer 12 between the films.

[0153] The first film layer 11A and the second film layer 11B have the function of two layers as raw material layers. The total thickness of the first film layer 11A and the second film layer 11B functioning as raw material layers is preferably in the range of 50 μm to 250 μm, and more preferably in the range of 70 μm to 200 μm. When the total thickness of the first film layer 11A and the second film layer 11B is within the above range, the lamination adaptability can be improved and cracks generated in the bending portion of the sheet can be reduced.

[0154] It should be noted that the film layer that functions as the raw material layer may be three or more layers.

[0155] (3.3) Example 3

[0156] use Fig.11 A decorative sheet 3C according to Configuration Example 3 of the third embodiment of the present disclosure will be described.

[0157] In the configuration example 3 of the third embodiment, referring to Fig.11 , a decorative sheet 3C in which the raw material layer 11 ′ is provided in multiple layers will be described.

[0158] like Fig.11As shown, the decorative sheet 3C is composed of a multi-layer structure of a raw material layer 11', a colored pattern layer 12, and a first surface protection layer 13 stacked in sequence. That is, the decorative sheet 3C is different from the decorative sheet 1 involved in the first embodiment in that a raw material layer 11' in which a first paper material 11C, a moisture-proof resin layer 11D, and a second paper material 11E are stacked in sequence is provided instead of a single raw material layer 11.

[0159] The raw material layer 11' of the decorative sheet 3C will be described in detail below. It should be noted that the layers other than the raw material layer 11' (the colored pattern layer 12 and the first surface protection layer 13) have the same structure as the layers of the decorative sheet 1, and thus description thereof will be omitted.

[0160] <Raw material layer>

[0161] The original material layer 11 ′ is constituted by laminating a first paper material 11C, a moisture-proof resin layer 11D, and a second paper material 11E in this order.

[0162] The moisture-proof resin layer 11D is made of, for example, polyethylene resin, etc. In this case, the moisture permeability can be finely adjusted by the type of resin material constituting the moisture-proof resin layer 11D and the thickness of the moisture-proof resin layer 11D, and the effect of suppressing the warping of the moisture-proof resin layer 11D can be obtained.

[0163] The first paper material 11C, the moisture-proof resin layer 11D, and the second paper material 11E function as three layers of raw material layers. The total thickness of the first paper material 11C, the moisture-proof resin layer 11D, and the second paper material 11E, which function as raw material layers, is preferably in the range of 50 μm to 250 μm, and more preferably in the range of 70 μm to 200 μm. When the total thickness of the first paper material 11C and the second paper material 11E is within the above range, the lamination adaptability can be improved and cracks generated in the bent portion of the sheet can be reduced.

[0164] In addition, the paper material functioning as the raw material layer may be a layer of three or more layers laminated via a moisture-proof resin layer.

[0165] (3.4) Example 4

[0166] use Fig.12 A decorative sheet 3D according to Configuration Example 4 of the third embodiment of the present disclosure will be described.

[0167] like Fig.12As shown, the decorative sheet 3D is composed of a raw material layer 11, a colored pattern layer 12, a transparent layer 15, a first surface protection layer 13, and a second surface protection layer 26 stacked in sequence. That is, the decorative sheet 2D is different from the decorative sheet 1 involved in the first embodiment in that a transparent layer 15 is provided between the colored pattern layer 12 and the first surface protection layer 13.

[0168] The transparent layer 15 of the decorative sheet 3D is described in detail below. It should be noted that the layers other than the transparent layer 15 (the raw material layer 11, the colored pattern layer 12, and the first surface protection layer 13) have the same structure as the layers of the decorative sheet 1, and thus description thereof is omitted.

[0169] <Transparency Layer>

[0170] The transparent layer 15 is made of a resin material. The resin material constituting the transparent layer 15 may be, for example, a thermosetting resin, or may be an acrylic resin, a silicone resin, a polyester resin, a urethane resin, an amide resin, or an epoxy resin. In addition, an adhesive resin layer may be provided under the transparent layer 15.

[0171] Alternatively, the raw material layer 11 may be made of a polyolefin film such as a polyethylene film or a polypropylene film.

[0172] Such a decorative sheet 3D prevents the colored pattern layer 12 from being exposed, thereby suppressing the reduction in wear resistance, scratch resistance, stain resistance, and weather resistance.

[0173] (3.5) Example 5

[0174] use Fig.13 A decorative sheet 3E according to Configuration Example 5 of the third embodiment of the present disclosure will be described.

[0175] The decorative sheet 3E includes: a raw material layer 11, a colored pattern layer 12, a first surface protection layer 13, and a second surface protection layer 26. The decorative sheet 3E is composed of the raw material layer 11, the colored pattern layer 12, the first surface protection layer 13, and the second surface protection layer 26 stacked in sequence. That is, the decorative sheet 2 is different from the decorative sheet 1 according to the first embodiment in that the second surface protection layer 26 is provided on the first surface protection layer 13.

[0176] The second surface protection layer 26 will be described below. It should be noted that since each layer (raw material layer 11, colored pattern layer 12, and first surface protection layer 13) other than the second surface protection layer 26 has the same structure as each layer of the decorative sheet 1, description thereof will be omitted.

[0177] (3.5.1) Basic composition of decorative sheets

[0178] <Second Surface Protective Layer>

[0179] The second surface protection layer 26 is provided on a portion of the concavo-convex shape forming surface of the first surface protection layer 13. The second surface protection layer 26 is a layer that is partially formed on the first surface protection layer 13 to generate a gloss difference with the first surface protection layer 13, thereby visually expressing an embossed feeling through a gloss matte effect.

[0180] The second surface protection layer 26 is formed of a resin material such as an ionizing radiation curing resin or a thermosetting resin, and is preferably formed of an ionizing radiation curing resin.

[0181] As the ionizing radiation curing resin, the same material as that of the first surface protective layer 13 can be used.

[0182] As the thermosetting resin, from the viewpoint of the difference in gloss with the first surface protection layer 13 , for example, a thermosetting resin having a urethane bond such as a two-component curable urethane resin is preferably used.

[0183] As the two-component curable urethane resin, for example, a urethane resin containing polyol as a main component and isocyanate as a crosslinking agent (curing agent) can be used.

[0184] The polyol may be a polyol having two or more hydroxyl groups in the molecule, and for example, polyethylene glycol, polypropylene glycol, acrylic polyol, polyester polyol, polyether polyol, polycarbonate polyol, and polyurethane polyol can be used.

[0185] In addition, as isocyanate, a polyisocyanate having two or more isocyanate groups in the molecule can be used. As a polyisocyanate, for example, aromatic isocyanates such as 2,4-toluene diisocyanate, xylene diisocyanate, and 4,4′-diphenylmethane diisocyanate can be used; or aliphatic (or alicyclic) isocyanates such as 1,6-hexamethylene diisocyanate, isophorone diisocyanate, hydrogenated toluene diisocyanate, and hydrogenated diphenylmethane diisocyanate can be used. In addition, adducts or polymers of the above-mentioned various isocyanates can be used. For example, there are adducts of toluene diisocyanate, toluene diisocyanate trimers, etc. It should be noted that among the above-mentioned isocyanates, aliphatic (or alicyclic) isocyanates are preferred in terms of being able to make weather resistance and heat yellowing resistance good, for example, 1,6-hexamethylene diisocyanate can be used.

[0186] The second surface protection layer 26 is partially formed on the first surface protection layer 13, and the coating area can be adjusted according to the design and target performance. The second surface protection layer 26 is preferably arranged in a manner that covers more than 10% and less than 90% of the surface of the first surface protection layer 13. In the case of showing a glossy matte effect (visual embossing), it is preferably arranged in a manner that covers more than 10% and less than 80% of the surface of the first surface protection layer 13. In addition, in the case where the decorative sheet 2 is required to improve the scratch resistance, stain resistance, and oleophobicity, the second surface protection layer 26 is preferably arranged in a manner that covers more than 10% and less than 80% of the surface of the first surface protection layer 13, and more preferably arranged in a manner that covers more than 10% and less than 30%.

[0187] The raw material layer 11 , the colored pattern layer 12 , and the first surface protection layer 13 of the decorative sheet 2 are formed in the same manner as the decorative sheet 1 .

[0188] The second surface protection layer 26 is formed by applying a resin material on the first surface protection layer 13 by screen printing, offset printing, gravure printing, or the like, and curing the resin material.

[0189] Thus, the decorative sheet 2 is formed.

[0190] The decorative sheet 3E has a second surface protection layer 26 with relatively high glossiness on a part of the concavo-convex shape forming surface of the low-gloss first surface protection layer 13 .

[0191] According to this configuration, in addition to the effects described in the first embodiment, the first surface protection layer 13 and the second surface protection layer 26 are not cloudy and the decorative sheet 2 has a glossy matte effect (visual embossed feeling) can be obtained.

[0192] (3.5.2) Modification

[0193] In the decorative sheet 2, the pattern layer 12B of the colored pattern layer 12 can be synchronized with the gloss matte effect (visual embossed feeling) produced by the gloss difference between the first surface protection layer 13 and the second surface protection layer 26. Compared with the gloss matte effect only produced by the gloss difference between the first surface protection layer 13 and the second surface protection layer 26, the decorative sheet 1 in which the pattern layer 12B is synchronized with the visual embossed feeling can produce a more excellent visual embossed feeling.

[0194] 4. Fourth Implementation

[0195] use Fig.14 A decorative board according to a fourth embodiment of the present disclosure will be described.

[0196] Fig.14 It is a cross-sectional view for explaining a configuration example of a decorative board 30 according to a third embodiment of the present disclosure.

[0197] The decorative board 30 includes a decorative sheet 1 and a base material 31. The decorative board 30 is formed by laminating the base material 31, the raw material layer 11, the colored pattern layer 12, and the first surface protection layer 13 in this order.

[0198] It should be noted that the decorative plate 30 may include the decorative sheet 2 instead of the decorative sheet 1. In addition, the decorative plate 30 may include decorative sheets 3A to 3D which are modified examples of the decorative sheet 1 instead of the decorative sheet 1.

[0199] The following describes the substrate 31. It should be noted that the layers other than the substrate 31 (including the raw material layer 11, the colored pattern layer 12, and the layers of the decorative sheet of the first surface protection layer 13) are the same as those described in the first embodiment and the second embodiment, and therefore the description thereof is omitted.

[0200] (4.1) Basic composition of decorative sheets

[0201] <Base material>

[0202] The substrate 31 is, for example, a wood substrate or medium density fiberboard (MDF). It may be a particle board, a metal substrate, a non-combustible substrate, a composite substrate composed of multiple materials, or a bright substrate. In addition, the substrate 31 may be a combination of plywood and MDF.

[0203] In addition, a primer layer, a concealing layer, or the like may be provided on the surface of the base material 31 facing the decorative sheet 1 .

[0204] The scope of the present disclosure is not limited to the exemplary embodiments described in the drawings, but includes all embodiments having equivalent effects to the purpose of the present disclosure. In addition, the scope of the present disclosure is not limited to the combination of features of the invention defined by the claims, but can be defined by all desired combinations of specific features among all disclosed features.

[0205] Explanation of symbols

[0206] 1,2,3A~3E Decorative sheet

[0207] 11,11' Raw material layer

[0208] 11A First film layer

[0209] 11B Second film layer

[0210] 11C First Paper Material

[0211] 11D moisture-proof resin layer

[0212] 11E Second Paper Materials

[0213] 12 Coloring pattern layer

[0214] 12A Coloring layer

[0215] 12B pattern layer

[0216] 13,23 First surface protective layer

[0217] 13' UV curable resin

[0218] 13A Core

[0219] 13B protrusion

[0220] 14 Adhesive resin layer

[0221] 15 Transparent Layer

[0222] 23' Ionizing radiation curing resin

[0223] 23A Core

[0224] 23B Ridge

[0225] 26 Second surface protection layer

[0226] 30 Decorative panels

Claims

1. A decorative sheet comprising: Raw material layer, a colored pattern layer disposed on one surface of the raw material layer, and A first surface protection layer is provided on the surface of the colored pattern layer opposite to the raw material layer and has a concavo-convex shape on the surface; The first surface protection layer includes a core portion as a lower layer region within the layer and a ridge portion as an upper layer region within the layer, The first surface protection layer is composed of an ionizing radiation curable resin. The height of the ridge portion is less than 15 μm, and the period between adjacent ridge portions is less than 50 μm. The concavoconvex shape has a random microstructure arranged isotropically. The ridge-shaped portion is formed using a transfer original plate formed by irradiating a surface of an ionizing radiation curing resin with ionizing radiation of a specific wavelength to shrink the surface of the ionizing radiation curing resin, wherein The surface coated with the ionizing radiation curing resin is irradiated with a first ionizing radiation having energy capable of cutting at least one of a carbonyl bond and a carbon-carbon bond to shrink the surface of the ionizing radiation curing resin, and the ionizing radiation curing resin after the surface shrinkage is irradiated with a second ionizing radiation to cure the ionizing radiation curing resin, thereby obtaining a transfer original plate having a concavo-convex shape on the surface. The first ionizing radiation is an excimer laser, and the incident angle of the excimer laser is 0 degrees. The second ionizing radiation is ultraviolet light having a wavelength of 400 nm or less.

2. The decorative sheet according to claim 1, wherein: The first surface protection layer is formed into the concavo-convex shape by providing convex protrusions or concave grooves on the surface.

3. The decorative sheet according to claim 1 or 2, wherein: The first surface protection layer is formed of a resin material having a uniform composition.

4. The decorative sheet according to claim 1 or 2, wherein: The concavo-convex shape is formed in a curved line shape in a cross-sectional view.

5. The decorative sheet according to claim 1 or 2, A second surface protection layer is provided on a portion of the concavo-convex shape forming surface of the first surface protection layer.

6. The decorative sheet according to claim 5, wherein: The second surface protection layer is provided so as to cover 10% to 80% of the surface of the first surface protection layer.

7. The decorative sheet according to claim 1 or 2, wherein: The first surface protection layer does not contain a gloss regulator, The glossiness of the first surface protection layer is 5.0 or less.

8. The decorative sheet according to claim 1 or 2, wherein: The raw material layer is a resin material or a resin film containing an inorganic material as an additive, and the content of the inorganic material relative to the raw material layer is in a range of 20 mass % to 80 mass %.

9. A decorative panel comprising: The decorative sheet according to any one of claims 1 to 8; and A base material layer is provided on a surface of the raw material layer opposite to the colored pattern layer.