Passivation agent and application for repairing heavy metal arsenic, lead and cadmium composite pollution
By using the passivating agent prepared by silkworm excrement, modified sepiolite and modified attapulgite, the problem of poor remediation effect of heavy metal contaminated soil in the existing technology is solved, and effective passivation of arsenic, lead and cadmium is achieved. It enhances soil remediation ability and maintains soil stability, avoiding secondary pollution.
Patent Information
- Application Number
- CN202210909680.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-07-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-07-29
AI Technical Summary
Existing remediation passivators for heavy metal contaminated soil are not effective when faced with complex heavy metal arsenic, lead, and cadmium pollution, and may lead to changes in soil properties and secondary pollution.
Using silkworm excrement, modified sepiolite and modified attapulgite as the main raw materials, modified materials are prepared by calcining, acidifying and adding modifiers to form a new passivating agent. The mass ratio of the mixture is silkworm excrement:modified Sepiolite: Ferrous sulfate: modified attapulgite, used to reduce the exchangeable content of heavy metals in the soil, increase the residual content, and maintain the stability of soil properties.
It effectively reduces the exchangeable content of heavy metals in the soil, increases the residual content, improves the passivation effect of metal ions in the soil, enhances soil repair capabilities, avoids secondary pollution, and improves soil fertility.
Smart Images

Figure GDA0004083825390000081 
Figure GDA0004083825390000091 
Figure GDA0004083825390000092
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of soil remediation, and in particular to a passivating agent for remediating the combined pollution of heavy metals arsenic, lead and cadmium, and a preparation method and application thereof. Background Art
[0002] Guangxi is rich in mineral resources and is known as the "hometown of non-ferrous metals". It is home to a large number of manganese, lead-zinc and other non-ferrous metal mines. The development of Guangxi's mineral resources plays a vital role in Guangxi's economic development. However, due to poor management and inappropriate development of mineral resources, heavy metals have caused serious pollution to the soil, water and vegetation around the mining area. Problems in the anti-seepage design or management of tailings ponds are the root causes of heavy metal pollution. For example, a large amount of waste is piled up in the tailings pond after mineral processing, and it migrates and transforms to the surface, underground infiltration and surrounding soil, water and vegetation through precipitation leaching, causing heavy metal pollution. Non-ferrous metal mining areas are mainly seriously affected by As, Cd and Pb.
[0003] Tailings ponds are a man-made debris flow hazard source, with the risk of dam collapse, which can easily cause serious accidents. Many similar accidents have occurred in Guangxi. Mining in the mining area and its surrounding land is also prone to pollution of the land and crop environment in the mining area and surrounding areas. Heavy metal pollution in the soil has seriously affected human life and health, and the remediation of heavy metal-contaminated soil is urgent.
[0004] Common measures for remediation of heavy metal contaminated soil or tailings include chemical passivation, soil leaching and bioremediation. Among them, chemical passivation is widely used because of its convenience. Chemical passivation is a remediation method that uses a fixative to make the biologically effective heavy metals in the soil form a new, less soluble and more stable form, thereby reducing the bioavailability of heavy metals. Chemical passivation uses chemical substances to reduce the mobility and bioavailability of heavy metals in the soil, thereby reducing the absorption and accumulation of heavy metals by crops and reducing the heavy metals that enter the human body through the food chain. Chemical fixation commonly uses inorganic and organic modifiers, which are often used because of their low cost and easy implementation. Passivators for remediating heavy metal contaminated soil can be divided into three types: organic, inorganic and organic-inorganic composite materials. Organic passivators mainly include farmyard manure, fresh plant residues, green manure such as corn stalk powder and organic fertilizers such as peat. Inorganic passivators mainly include fly ash, phosphate rock powder, calcium magnesium phosphate fertilizer, hydroxyapatite, sepiolite, bentonite, etc. Organic-inorganic composite materials are mainly prepared by modifying inorganic passivators with some organic solvents.
[0005] However, due to the complexity of heavy metal substances in soil and the differences in soil space, heavy metal remediation is extremely complicated. For more complex composite heavy metal pollution, the existing passivation agent remediation effect is not ideal.
[0006] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0007] The purpose of the present invention is to provide a passivating agent for repairing the composite pollution of heavy metals arsenic, lead and cadmium, so as to overcome the disadvantage that the passivating agent is not effective in repairing tailings or soil in mining areas.
[0008] Another object of the present invention is to provide a passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium and its application in the pollution control of metal tailings.
[0009] To achieve the above-mentioned purpose, the present invention provides a passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium, which is mainly made of the following raw materials: silkworm feces, modified sepiolite, ferrous sulfate and modified attapulgite; the preparation method of the modified sepiolite is as follows: the sepiolite is crushed, calcined, taken out and cooled to room temperature, phosphoric acid is added to acidify the sepiolite, and then ethylenediaminetetraacetic acid and hexadecyltrimethylammonium bromide are added, stirred to react, filtered and dried, and ground to obtain the modified sepiolite; the preparation method of the modified attapulgite is as follows: the attapulgite is crushed, calcined, taken out and cooled to room temperature, hydrochloric acid is added to acidify the attapulgite, and then ammonium citrate and melamine salt compounds are added, stirred to react, filtered and dried, and ground to obtain the modified attapulgite.
[0010] Preferably, in the above technical solution, the passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium, the silkworm feces, modified sepiolite, ferrous sulfate and modified attapulgite are mixed in a mass ratio of 1-5:1-5:1-5:1-5.
[0011] Preferably, in the above technical solution, the passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium, the silkworm feces, modified sepiolite, ferrous sulfate and modified attapulgite are mixed in a mass ratio of 1:1:1:1.
[0012] Preferably, in the above technical scheme, the preparation method of the modified sepiolite is as follows: crush the sepiolite, calcine it at a temperature of 600-800°C for 5-10h, take it out and cool it to room temperature, add phosphoric acid with a mass concentration of 10-25%, acidify the sepiolite at a temperature of 50-70°C, the solid-liquid ratio of sepiolite to phosphoric acid is 1g:5-15mL, and the acidification reaction time is 1-5h; then add ethylenediaminetetraacetic acid and hexadecyltrimethylammonium bromide, stir the reaction for 3-15h, filter and dry, and grind to obtain the modified sepiolite.
[0013] Preferably, in the above technical solution, in the method for preparing modified sepiolite, the mass ratio of sepiolite, ethylenediaminetetraacetic acid and hexadecyltrimethylammonium bromide is 50-150:0.1-3:0.1-3.
[0014] Preferably, in the above technical scheme, the preparation method of the modified attapulgite is as follows: crush the attapulgite, calcine it at a temperature of 500-600°C for 5-10h, take it out and cool it to room temperature, add hydrochloric acid with a mass concentration of 15-25%, acidify the attapulgite at a temperature of 50-70°C, the solid-liquid ratio of attapulgite to hydrochloric acid is 1g:5-15mL, and the acidification reaction time is 1-5h; then add ammonium citrate and melamine salt compounds, stir the reaction for 1-10h, filter and dry, and grind to obtain modified attapulgite.
[0015] Preferably, in the above technical solution, in the method for preparing attapulgite, the mass ratio of attapulgite, ammonium citrate and melamine salt compound is 50-150:0.1-3:0.1-3.
[0016] Preferably, in the above technical solution, the melamine salt compound includes melamine phosphate, melamine hydrochloride, melamine borate or melamine sulfate.
[0017] The above-mentioned passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium is used in the treatment of metal tailings pollution.
[0018] The method for using the above passivating agent for repairing the combined pollution of heavy metal arsenic, lead and cadmium comprises the following steps: mixing the passivating agent with the pollutants to be repaired, the mixing mass ratio is 0.5-5:100, and the water content of the tailings sand is maintained at 55-75%.
[0019] Compared with the prior art, the present invention has the following beneficial effects: the passivation agent for repairing the composite pollution of heavy metals arsenic, lead and cadmium of the present invention, by adding silkworm feces, modified sepiolite, ferrous sulfate and modified attapulgite to the raw materials, can reduce the exchangeable content of heavy metals in the soil, increase its residual content, and will not cause a significant change in the soil properties. At the same time, it can also increase soil fertility, accelerate soil repair, and make the passivation effect of metal ions in the soil more ideal. And it will not cause secondary pollution. DETAILED DESCRIPTION
[0020] The specific implementation modes of the present invention are described in detail below in conjunction with specific embodiments, but it should be understood that the protection scope of the present invention is not limited by the specific implementation modes.
[0021] Example 1
[0022] A passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium is mainly made of the following raw materials: silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite. The silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite are mixed in a mass ratio of 1:1:1:1.
[0023] A method for preparing a passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium comprises the following steps:
[0024] (1) Preparation of modified sepiolite
[0025] The sepiolite was crushed, calcined at 750°C for 7h, taken out and cooled to room temperature, and then phosphoric acid with a mass concentration of 18% was added to acidify the sepiolite at 60°C. The solid-liquid ratio of sepiolite to phosphoric acid was 1g:8mL, and the acidification reaction time was 3h. Then ethylenediaminetetraacetic acid and hexadecyltrimethylammonium bromide were added, stirred for reaction for 6h, filtered and dried, and ground to obtain modified sepiolite. Among them, the mass ratio of sepiolite, ethylenediaminetetraacetic acid and hexadecyltrimethylammonium bromide was 100:1:1.
[0026] (2) Preparation of modified attapulgite
[0027] The attapulgite is crushed, calcined at 550°C for 7h, taken out and cooled to room temperature, and then hydrochloric acid with a mass concentration of 17% is added to acidify the attapulgite at 60°C. The solid-liquid ratio of attapulgite to hydrochloric acid is 1g:7mL, and the acidification reaction time is 3h. Then, ammonium citrate and melamine salt compounds are added, stirred for reaction for 3h, filtered and dried, and ground to obtain modified attapulgite.
[0028] The mass ratio of attapulgite, ammonium citrate and melamine salt compound is 100:1.5:1. The melamine salt compound is melamine phosphate.
[0029] (3) Silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite are mixed uniformly according to a certain proportion to obtain a passivating agent 1.
[0030] Example 2
[0031] A passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium is mainly made of the following raw materials: silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite. The silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite are mixed in a mass ratio of 1:5:5:1.
[0032] A method for preparing a passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium comprises the following steps:
[0033] (1) Preparation of modified sepiolite
[0034] The sepiolite was crushed, calcined at 600°C for 10 hours, taken out and cooled to room temperature, and then phosphoric acid with a mass concentration of 25% was added to acidify the sepiolite at 50°C. The solid-liquid ratio of sepiolite to phosphoric acid was 1g:5mL, and the acidification reaction time was 1h. Then ethylenediaminetetraacetic acid and hexadecyltrimethylammonium bromide were added, stirred for reaction for 8 hours, filtered and dried, and ground to obtain modified sepiolite. Among them, the mass ratio of sepiolite, ethylenediaminetetraacetic acid and hexadecyltrimethylammonium bromide was 50:0.1:0.3.
[0035] (2) Preparation of modified attapulgite
[0036] The attapulgite is crushed, calcined at 500°C for 10 hours, taken out and cooled to room temperature, and then hydrochloric acid with a mass concentration of 25% is added to acidify the attapulgite at 70°C. The solid-liquid ratio of attapulgite to hydrochloric acid is 1g:5mL, and the acidification reaction time is 1 hour. Then, ammonium citrate and melamine salt compounds are added, stirred for reaction for 6 hours, filtered and dried, and ground to obtain modified attapulgite.
[0037] The mass ratio of attapulgite, ammonium citrate and melamine salt compound is 50:0.2:0.1. The melamine salt compound is melamine hydrochloride.
[0038] (3) Silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite are mixed uniformly according to a certain proportion to obtain passivating agent 2.
[0039] Example 3
[0040] A passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium is mainly made of the following raw materials: silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite. The mass ratio of the silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite is 5:1:1:5.
[0041] A method for preparing a passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium comprises the following steps:
[0042] (1) Preparation of modified sepiolite
[0043] The sepiolite was crushed, calcined at 800°C for 5h, taken out and cooled to room temperature, and then phosphoric acid with a mass concentration of 10% was added to acidify the sepiolite at 70°C. The solid-liquid ratio of sepiolite to phosphoric acid was 1g:15mL, and the acidification reaction time was 5h. Then ethylenediaminetetraacetic acid and hexadecyltrimethylammonium bromide were added, stirred for reaction for 3h, filtered and dried, and ground to obtain modified sepiolite. Among them, the mass ratio of sepiolite, ethylenediaminetetraacetic acid and hexadecyltrimethylammonium bromide was 150:2:0.7.
[0044] (2) Preparation of modified attapulgite
[0045] The attapulgite is crushed, calcined at 600°C for 5h, taken out and cooled to room temperature, and then hydrochloric acid with a mass concentration of 15% is added to acidify the attapulgite at 50°C. The solid-liquid ratio of attapulgite to hydrochloric acid is 1g:15mL, and the acidification reaction time is 5h. Then, ammonium citrate and melamine salt compounds are added, stirred for reaction for 3h, filtered and dried, and ground to obtain modified attapulgite.
[0046] The mass ratio of attapulgite, ammonium citrate and melamine salt compound is 150:2.1:0.9. The melamine salt compound is melamine borate.
[0047] (3) Silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite are mixed uniformly according to a certain proportion to obtain passivating agent 3.
[0048] Example 4
[0049] The preparation method of the passivator in this embodiment is basically the same as that in embodiment 1, except that the passivator is mainly made of the following raw materials: silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite mixed in a mass ratio of 1:2:3:2. It is recorded as passivator 4.
[0050] Example 5
[0051] The preparation method of the passivator in this embodiment is basically the same as that in embodiment 1, except that the passivator is mainly made of the following raw materials: silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite mixed in a mass ratio of 3:2:1:3. It is recorded as passivator 5.
[0052] Pot test 1
[0053] 1. Test materials: tailings 1 (Yangshuo County, Guilin City); tailings 2 (Nandan County, Hechi City).
[0054] 2. Additives: control (CK); passivator.
[0055] 3. Experimental design: Accurately weigh 600g of pre-treated tailings and soil and place them in plastic basins with a diameter of 13cm at the mouth, a diameter of 10cm at the bottom and a height of 12cm. Add the following different treatments and their proportions to the test tailings. There are 18 treatments in total, each of which is repeated 3 times. The average values are taken for comparison, as shown in Table 1.
[0056] The silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite in the passivator are represented by A, B, C and D respectively. Except for passivator 2 and passivator 3, the passivator modified sepiolite and modified attapulgite mentioned in other treatments are prepared by the method of Example 1. B1 is unmodified sepiolite, and D1 is unmodified sepiolite.
[0057] 4. Operation method: Put the test tailings into small plastic buckets according to 600g each. Mix the compound passivator and test materials for each treatment with a small wooden shovel, add deionized water to the tailings by weighing method every other day to maintain a constant moisture content (60% of the saturated moisture content of the tailings), seal with plastic wrap and place in a greenhouse for cultivation. After adding the passivator, take samples and analyze them on the 14th day (0d, 7d, 14d, 30d and 60d) to test the pH value, effective Pb, effective Cd, and effective As. The test results are shown in Table 2, Table 3, Table 4, Table 5, Table 6 Table 1 Potted test 1 Passivation agent design
[0058]
[0059]
[0060] Table 2 Results of the influence of Guilin Yangshuo tailings 1 potted experiment on the pH value of tailings
[0061]
[0062]
[0063] Table 3 Results of the influence of Nandan tailings 2 pot experiment on tailings pH value
[0064]
[0065]
[0066] Table 4 Guilin tailings 1 passivation 14 days test results
[0067]
[0068]
[0069] Table 5 Nandan tailings 2 passivation 14 days test results
[0070]
[0071]
[0072] Pot test 2
[0073] 1. Test materials: Contaminated soil around tailings 1 (Yangshuo County, Guilin City); contaminated soil around tailings 2 (Nandan County, Hechi City).
[0074] 2. Additives: control (CK); passivator.
[0075] 3. Experimental design: 600 g of pre-treated soil was accurately weighed and placed in plastic pots with a diameter of 13 cm at the mouth, a diameter of 10 cm at the bottom and a height of 12 cm. The soil was mixed into the test tailings according to the following different treatments and their proportions. There were 16 treatments in total, each of which was repeated 3 times. The average values were taken for comparison, as shown in Table 6.
[0076] The silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite in the passivator are represented by A, B, C and D respectively. Except for passivator 2 and passivator 3, the passivator modified sepiolite and modified attapulgite mentioned in other treatments are prepared by the method of Example 1. B1 is unmodified sepiolite, and D1 is unmodified sepiolite.
[0077] 4. Operation method: Put the test tailings into a small plastic bucket according to 600g each. Mix the compound passivator and the test material for each treatment with a small wooden shovel, add deionized water to the tailings by weighing method every other day to maintain a constant moisture content (60% of the saturated moisture content of the tailings), seal with plastic wrap and place in a greenhouse for cultivation. After adding the passivator, sample and analyze the pH value, effective Pb, effective Cd, and effective As on the 14th day (0d, 7d, 14d, 30d, and 60d). The test results are shown in Table 7, Table 8, Table 9, Table 10, and Table 11.
[0078] Table 6 Passivation agent design for pot experiment 2
[0079]
[0080]
[0081] Table 7 Results of the influence of Guilin Yangshuo soil 1 potted plant experiment on soil pH
[0082]
[0083]
[0084] Table 8 Results of the Nandan soil 2 pot experiment on soil pH
[0085]
[0086]
[0087] Table 9 Guilin soil 1 passivation 14 days test results
[0088]
[0089]
[0090] Table 10 Nandan soil 2 passivation 14 days test results
[0091]
[0092]
[0093] The foregoing description of specific exemplary embodiments of the present invention is for the purpose of illustration and demonstration. These descriptions are not intended to limit the present invention to the precise form disclosed, and it is clear that many changes and variations can be made based on the above teachings. The purpose of selecting and describing the exemplary embodiments is to explain the specific principles of the present invention and its practical application, so that those skilled in the art can realize and utilize various different exemplary embodiments of the present invention and various different selections and changes. The scope of the present invention is intended to be limited by the claims and their equivalents.
Claims
1. A passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium, characterized in that: It is mainly made of the following raw materials: silkworm feces, modified sepiolite, ferrous sulfate and modified attapulgite; The preparation method of the modified sepiolite is as follows: crushing the sepiolite, calcining it, taking it out and cooling it to room temperature, adding phosphoric acid to acidify the sepiolite, then adding ethylenediaminetetraacetic acid and hexadecyltrimethylammonium bromide, stirring to react, filtering and drying, and grinding to obtain the modified sepiolite; The preparation method of the modified attapulgite is as follows: crushing the attapulgite, calcining it, taking it out and cooling it to room temperature, adding hydrochloric acid to acidify the attapulgite, then adding ammonium citrate and melamine salt compounds, stirring to react, filtering and drying, and grinding to obtain the modified attapulgite; The mass ratio of the silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite is 1-5:1-5:1-5:1-5.
2. The passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium according to claim 1, characterized in that: The mass ratio of the silkworm excrement, modified sepiolite, ferrous sulfate and modified attapulgite is 1:1:1:
1.
3. The passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium according to claim 1, characterized in that: The preparation method of the modified sepiolite is as follows: crushing the sepiolite, calcining it at a temperature of 600-800°C for 5-10h, taking it out and cooling it to room temperature, adding phosphoric acid with a mass concentration of 10-25%, acidifying the sepiolite at a temperature of 50-70°C, the solid-liquid ratio of sepiolite to phosphoric acid is 1g:5-15mL, and the acidification reaction time is 1-5h; then adding ethylenediaminetetraacetic acid and hexadecyltrimethylammonium bromide, stirring and reacting for 3-15h, filtering and drying, and grinding to obtain the modified sepiolite.
4. The passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium according to claim 1, characterized in that: In the method for preparing modified sepiolite, the mass ratio of sepiolite, ethylenediaminetetraacetic acid and hexadecyltrimethylammonium bromide is 50-150:0.1-3:0.1-3.
5. The passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium according to claim 1, characterized in that: The preparation method of the modified attapulgite is as follows: crushing the attapulgite, calcining it at a temperature of 500-600°C for 5-10h, taking it out and cooling it to room temperature, adding hydrochloric acid with a mass concentration of 15-25%, acidifying the attapulgite at a temperature of 50-70°C, the solid-liquid ratio of the attapulgite to the hydrochloric acid is 1g:5-15mL, and the acidification reaction time is 1-5h; then adding ammonium citrate and melamine salt compounds, stirring and reacting for 1-10h, filtering and drying, and grinding to obtain the modified attapulgite.
6. The passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium according to claim 1, characterized in that: In the method for preparing attapulgite, the mass ratio of attapulgite, ammonium citrate and melamine salt compound is 50-150:0.1-3:0.1-3.
7. The passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium according to claim 1, wherein the melamine salt compound comprises melamine phosphate, melamine hydrochloride, melamine borate or melamine sulfate.
8. Use of a passivating agent for repairing the combined pollution of heavy metals arsenic, lead and cadmium as claimed in any one of claims 1 to 7 in the treatment of metal tailings pollution.
9. A method for using a passivating agent for repairing heavy metal arsenic, lead and cadmium composite pollution as claimed in any one of claims 1 to 7, characterized in that: The method comprises the following steps: mixing the passivating agent with the pollutants to be repaired, with the mixing mass ratio being 0.5-5:100, and maintaining the water content of the tailings sand at 55-75%.
Citation Information
Patent Citations
Preparation and application method of soil heavy metal composite passivating agent
CN102719255A
Method for improving farmland soil environment capacity
CN103814649A
Sludge treatment method for heavy metal stabilization
CN104230130A
Water body eutrophication ion attapulgite adsorbent
CN106040164A
Passivating agent used for treating lead-cadmium compound contaminated soil as well as preparation method thereof and using method thereof
CN106753392A