A method for preparing aluminum ion-doped Co9S8 / MXene heterostructure composite material
Through the preparation of aluminum ion-doped Co9S8/MXene heterostructure composite materials, the problems of low specific capacitance and poor cycle stability of existing CoxSy@MXene electrode materials have been solved, and the electrochemical performance of high-performance supercapacitors has been improved.
Patent Information
- Application Number
- CN202211083941.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-06
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-09-06
AI Technical Summary
Existing CoxSy@MXene electrode materials have low specific capacitance and poor cycle stability in supercapacitor applications.
Using the preparation method of aluminum ion-doped Co9S8/MXene heterostructure composite materials, MXene nanosheets are obtained through etching, and then undergo a one-step solvothermal reaction with metal compounds to generate metal aluminum ion-doped Co9S8/MXene composite materials.
The specific capacitance and cycle stability of the material are improved. The capacitance reaches 1643C g-1 when the current density is 2A g-1, and the capacitance retention rate reaches 70%. It is suitable for high-performance supercapacitors.
Smart Images

Figure CN115411249B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a Co9S8 / MXene heterostructure composite material. Background Art
[0002] With the advancement of science and technology, people's demand for electronic devices is getting higher and higher, and supercapacitors have attracted widespread attention due to their excellent electrochemical properties.
[0003] MXene has been proven to have great potential in the field of energy storage due to its unique layered structure and excellent conductivity. Metal oxide / MXene composites are usually prepared by hydrothermal and solvothermal methods to generate metal oxide / MXene composites on MXene nanosheets. For example, the Chinese patent "Aluminum Ion Battery and Its Cathode Material Cox Sy@MXene" with application number 202011579306.9 discloses an aluminum ion battery and its cathode material CoxSy@MXene, which is made by in-situ growth of micro-nano cobalt sulfide on a MXene matrix material. The micro-nano cobalt sulfide is CoxSy, where x>0, y>0, and the mass of the micro-nano cobalt sulfide accounts for 5% to 95% of the total mass of the cathode material. The dispersibility of nano-micro-nano cobalt sulfide is improved, and the grain size is refined to improve the conductivity, but the material has low specific capacity and poor cycle stability when used in supercapacitors. Summary of the invention
[0004] The present invention is to solve the existing Co x S y In order to solve the technical problems of low specific capacitance and poor cycle stability of @MXene electrode materials, a method for preparing aluminum ion-doped Co9S8 / MXene heterostructure composite materials is provided. MXene nanosheets are first obtained by etching, and then the MXene nanosheets are subjected to a one-step solvothermal reaction with metal compounds to generate metal aluminum ion-doped Co9S8 / MXene composite materials, which provides a new idea for the preparation of high-performance supercapacitors.
[0005] The preparation method of the aluminum ion doped Co9S8 / MXene heterostructure composite material of the present invention is carried out according to the following steps:
[0006] 1. Preparation of MXene nanosheets:
[0007] a. Add 1 g of nickel fluoride to 20 mL of 9 M HCl, mix and stir 9 M HCl and nickel fluoride for 25 to 35 minutes to obtain a mixed solution;
[0008] b. Add titanium aluminum carbide to the mixed solution, heat to 35-45°C and maintain for 85-95 hours;
[0009] c. The product of step b was first washed by centrifugation with 1M HCl, the supernatant was discarded, and the precipitate was then washed by centrifugation with deionized water until the pH value of the supernatant reached 6-8, the supernatant was discarded, and the precipitate was added to deionized water and ultrasonically treated in an ice bath under nitrogen for 50-70 minutes, and finally the mixed solution was centrifuged, the upper suspension was discarded, and the precipitate was freeze-dried to obtain MXene nanosheet powder;
[0010] 2. Preparation of aluminum-doped metal sulfide / MXene Al-Co9S8 / MXene:
[0011] a. Add MXene nanosheet powder to a mixed solution of ethylene glycol and N,N-dimethylformamide, and perform ultrasonic treatment for 20 to 30 minutes; then add cobalt chloride hexahydrate and aluminum chloride hexahydrate and stir for 10 to 20 minutes, and then add thiourea and stir for 25 to 35 minutes to obtain a precursor solution;
[0012] b. Transfer the precursor solution to a Teflon autoclave, heat it to 140-180°C and keep it for 10-14 hours. Take out the product, wash it with ethanol and deionized water by centrifugation, and then freeze-dry it to obtain an aluminum ion-doped Co9S8 / MXene heterostructure composite material.
[0013] Furthermore, the centrifugal separation described in step 1c is performed at a rotation speed of 3000 to 4000 rpm for 5 to 10 minutes.
[0014] Furthermore, in step 2a, the ratio of the mass of the MXene nanosheet powder to the volume of ethylene glycol is 1 g: (95-105) mL.
[0015] Furthermore, in step 2a, the ratio of the mass of the MXene nanosheet powder to the volume of N,N-dimethylformamide is 1 g: (350-450) mL.
[0016] Furthermore, in step 2a, the mass ratio of MXene nanosheet powder to cobalt chloride hexahydrate is 1:(5-7).
[0017] Furthermore, in step 2a, the molar ratio of cobalt chloride hexahydrate, aluminum chloride hexahydrate and thiourea is 1:(0.1-0.2):(3-3.5).
[0018] Furthermore, in step 2b, when centrifuging ethanol and deionized water, the centrifugal treatment is carried out at a rotation speed of 10,000 to 11,000 rpm for 5 to 20 minutes.
[0019] The present invention uses MXene etched with nickel fluoride as a substrate to prepare an aluminum ion-doped Co9S8 / MXene heterojunction material. The material of the present invention introduces aluminum ions into the metal sulfide lattice to generate lattice defects and thus improve its specific capacitance. The capacitance of the heterojunction material is 2A g -1 1643C g -1 When the current density increases from 2A g -1 Increase to 15A g -1 When the capacitance is maintained at 70%, it can be used in the field of supercapacitors. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is a scanning electron microscope photograph of MXene obtained in step 1 of Example 1;
[0021] Figure 2 This is a scanning electron microscope photograph of the aluminum ion-doped Co9S8 / MXene heterostructure composite material obtained in step 2 of Example 1;
[0022] Figure 3 is the XRD spectrum of the aluminum ion doped Co9S8 / MXene heterostructure composite material Al-Co9S8 / MXene obtained in step 2 of Example 1;
[0023] Figure 4 This is the XPS spectrum of the aluminum ion-doped Co9S8 / MXene heterostructure composite material Al-Co9S8 / MXene obtained in step 2 of Example 1;
[0024] Figure 5 It is a constant current charge and discharge (GCD) curve of the aluminum ion-doped Co9S8 / MXene heterostructure composite material obtained in step 2 of Example 1;
[0025] Figure 6 This is the rate performance diagram of the aluminum ion doped Co9S8 / MXene heterostructure composite material obtained in step 2 of Example 1.
[0026] Figure 7 It is a constant current charge and discharge (GCD) curve of Co9S8 / MXene without aluminum ion doping prepared in comparative example 2;
[0027] Figure 8 This is a rate performance curve of Co9S8 / MXene without aluminum ion doping prepared in comparative example 2. DETAILED DESCRIPTION
[0028] The beneficial effects of the present invention are verified by the following examples.
[0029] Example 1: The preparation method of the aluminum ion-doped Co9S8 / MXene heterostructure composite material of this example is carried out according to the following steps:
[0030] 1. Preparation of MXene nanosheets:
[0031] a. Add 1 g of nickel fluoride to 20 mL of 9 M HCl, mix and stir for 30 minutes to obtain a mixed solution;
[0032] b. Add 1 g of titanium aluminum carbide to the mixed solution, heat to 40°C and keep for 90 hours;
[0033] c. The product of step b was first centrifuged at 3500 rpm with 1M HCl for 6 minutes, the supernatant was discarded, and the precipitate was washed with deionized water at 3500 rpm for 6 minutes, and the supernatant was discarded after repeated centrifugation until the pH value of the supernatant reached 6. The precipitate was added to 30 mL of deionized water, and ultrasonically treated for 60 minutes under nitrogen and at 8°C. Finally, the mixed solution was centrifuged at 3500 rpm for 60 minutes, the upper suspension was discarded, and the precipitate was placed in a freeze dryer at a temperature of -55°C and a vacuum degree of 10 Pa for freeze drying for 2 days to obtain MXene nanosheet powder;
[0034] 2. Preparation of aluminum ion doped Co9S8 / MXene heterostructure composite material Al-Co9S8 / MXene:
[0035] a. Add 60 mg of MXene nanosheet powder to a mixed solution of 6 mL of ethylene glycol and 24 mL of N,N-dimethylformamide, and ultrasonicate for 25 minutes; then add 0.334 g of cobalt chloride hexahydrate and 0.048 g of aluminum chloride hexahydrate and stir for 15 minutes, then add 0.3197 g of thiourea and stir for 30 minutes to obtain a precursor solution;
[0036] b. Transfer the precursor solution to a Teflon autoclave, heat it to 160°C and keep it for 12 hours. Take out the product and centrifuge it with ethanol and deionized water at a speed of 10500 rpm for 3 times, each time for 15 minutes. After centrifugal washing, put it in a freeze dryer at a temperature of -55°C and a vacuum degree of 10Pa for freeze drying for 20 hours to obtain an aluminum ion doped Co9S8 / MXene heterostructure composite material, denoted by Al-Co9S8 / MXene.
[0037] Comparative Example 2: Compared with Example 1, this comparative example is different in that aluminum ions are not doped. The preparation steps and parameters are different from those of Example 1 in that the operation of step 2a is replaced by the following operation: 60 mg of MXene nanosheet powder is added to a mixed solution of 6 mL of ethylene glycol and 24 mL of N,N-dimethylformamide, and ultrasonically treated for 25 minutes; then 0.334 g of cobalt chloride hexahydrate is added and stirred for 15 minutes, and then 319.7 mg of thiourea is added and stirred for 30 minutes to obtain a precursor solution. The other steps and parameters are the same as those of Example 1, and the material Co9S8 / MXene without aluminum ion doping is obtained.
[0038] The scanning electron microscope photograph of MXene obtained in step 1 of this embodiment 1 is as follows Figure 1 As shown, from Figure 1 It can be seen that MXene has an obvious layered distribution.
[0039] The scanning electron microscope photograph of the aluminum ion doped Co9S8 / MXene heterostructure composite material Al-Co9S8 / MXene obtained in step 2 of this embodiment 1 is as follows Figure 2 As shown, from Figure 2 It can be seen that Al-Co9S8 / MXene is distributed in the form of nanospheres, and the surface of the nanospheres is relatively rough, which proves the successful introduction of aluminum ions.
[0040] The XRD spectrum of the aluminum ion doped Co9S8 / MXene heterostructure composite material Al-Co9S8 / MXene obtained in step 2 of this embodiment 1 is as follows Figure 3 As shown, Figure 3 Several obvious peaks at 38°, 40°, 47°, 51°, and 61° represent the (331), (420), (511), (440), and (533) crystal planes of Co9S8, respectively, indicating the successful synthesis of Al-Co9S8 / MXene.
[0041] The XPS spectrum of the aluminum ion doped Co9S8 / MXene heterostructure composite material Al-Co9S8 / MXene obtained in step 2 of this embodiment 1 is as follows Figure 4 As shown by Figure 4 The peaks of Co, Al, O, C, and S can be seen, further indicating the successful synthesis of Al-Co9S8 / MXene.
[0042] The constant current charge-discharge curve (GCD) of the aluminum ion-doped Co9S8 / MXene heterostructure composite material Al-Co9S8 / MXene obtained in step 2 of this embodiment 1 is shown in the figure Figure 5 As shown by Figure 5It can be seen that Al-Co9S8 / MXene has a clear voltage platform, indicating the existence of pseudocapacitance, and it can be calculated that at a current density of 2A g -1 The capacitance of Al-Co9S8 / MXene is 1643C g -1 .
[0043] The rate performance diagram of the aluminum ion doped Co9S8 / MXene heterostructure composite material Al-Co9S8 / MXene obtained in step 2 of this embodiment 1 is as follows Figure 6 As shown by Figure 6 It can be seen that when the current density reaches 15A g -1 When the capacitance is maintained at 2A g -1 The rate performance of Al-Co9S8 / MXene is about 70%.
[0044] The constant current charge-discharge curve of the comparative material Co9S8 / MXene not doped with aluminum ions prepared in Comparative Example 2 is shown in FIG. Figure 7 As shown by Figure 7 It can be seen that at a current density of 2A g -1 The capacitance of Co9S8 / MXene is 1427C g -1 As a comparison, the rate performance of Co9S8 / MXene, a material not doped with aluminum ions, is shown in the figure below: Figure 8 As shown by Figure 8 It can be seen that when the current density reaches 12A g -1 When the capacitance is only 2A g -1 By comparison, it can be seen that the electrochemical performance of the material Co9S8 / MXene not doped with aluminum ions is far inferior to that of the Al-Co9S8 / MXene composite material prepared in Example 1.
[0045] Comparative Example 3: Compared with Example 1, this comparative example differs in that the amount of aluminum ions doped is too low. The preparation steps and parameters thereof are different from those of Example 1 in that the operation of step 2a is replaced by the following operation: 60 mg of MXene nanosheet powder is added to a mixed solution of 6 mL of ethylene glycol and 24 mL of N,N-dimethylformamide, and ultrasonically treated for 25 minutes; then 0.334 g of cobalt chloride hexahydrate and 0.0274 g of aluminum chloride hexahydrate are added and stirred for 15 minutes, and then 319.7 mg of thiourea is added and stirred for 30 minutes to obtain a precursor solution. The other steps and parameters are the same as those of Example 1, and Co9S8 / MXene doped with aluminum ions having a lower doping level is obtained.
[0046] Comparative Example 4: Compared with Example 1, the difference in this comparative example is that the amount of aluminum ions doped is too high. The preparation steps and parameters are different from those in Example 1. The operation of step 2a is replaced by the following operation: 60 mg of MXene nanosheet powder is added to a mixed solution of 6 mL of ethylene glycol and 24 mL of N, N-dimethylformamide, and ultrasonically treated for 25 minutes; then 0.334 g of cobalt chloride hexahydrate and 0.0154 g of aluminum chloride hexahydrate are added and stirred for 15 minutes, and then 319.7 mg of thiourea is added and stirred for 30 minutes to obtain a precursor solution. The other steps and parameters are the same as those in Example 1, and Co9S8 / MXene doped with aluminum ions having a higher doping level is obtained.
[0047] By comparing the constant current charge and discharge curves, the materials prepared in Comparative Example 3 and Comparative Example 4 have a current density of 2A g -1 The capacitance is 1308C g -1 and 1245C g -1 , which are lower than the Al-Co9S8 / MXene prepared in implementation 1. This is because the addition of an appropriate amount of aluminum ions is beneficial to improving the electrochemical performance, but when the doping amount is too small, it cannot induce the generation of defects. If the doping amount is too large, it will change the structure of the material itself, slow down the ion transmission speed, and lead to slower reaction kinetics, which will lead to reduced electrochemical performance.
Claims
1. A method for preparing an aluminum ion-doped Co9S8 / MXene heterostructure composite material, characterized in that The method proceeds as follows:
1. Preparation of MXene nanosheets: a. Add 1 g of nickel fluoride to 20 mL of 9 M HCl, mix and stir 9 M HCl and nickel fluoride for 25 to 35 minutes to obtain a mixed solution; b. Add titanium aluminum carbide to the mixed solution, heat to 35-45°C and maintain for 85-95 hours; c. The product of step b was first washed by centrifugation with 1M HCl, the supernatant was discarded, and the precipitate was then washed by centrifugation with deionized water until the pH value of the supernatant reached 6-8, the supernatant was discarded, and the precipitate was added to deionized water and ultrasonically treated in an ice bath under nitrogen for 50-70 minutes, and finally the mixed solution was centrifuged, the upper suspension was discarded, and the precipitate was freeze-dried to obtain MXene nanosheet powder; 2. Preparation of aluminum-doped metal sulfide / MXene Al-Co9S8 / MXene: a. Add MXene nanosheet powder to a mixed solution of ethylene glycol and N,N-dimethylformamide, and perform ultrasonic treatment for 20 to 30 minutes; then add cobalt chloride hexahydrate and aluminum chloride hexahydrate and stir for 10 to 20 minutes, and then add thiourea and stir for 25 to 35 minutes to obtain a precursor solution; b. Transfer the precursor solution to a Teflon autoclave, heat it to 140-180°C and keep it for 10-14 hours. Take out the product, wash it with ethanol and deionized water by centrifugation, and then freeze-dry it to obtain an aluminum ion-doped Co9S8 / MXene heterostructure composite material.
2. The method for preparing an aluminum ion-doped Co9S8 / MXene heterostructure composite material according to claim 1, characterized in that The centrifugal separation in step 1c is carried out at a rotation speed of 3000 to 4000 rpm for 5 to 10 minutes.
3. The method for preparing an aluminum ion-doped Co9S8 / MXene heterostructure composite material according to claim 1 or 2, characterized in that In step 2a, the ratio of the mass of MXene nanosheet powder to the volume of ethylene glycol is 1 g: (95-105) mL.
4. The method for preparing an aluminum ion-doped Co9S8 / MXene heterostructure composite material according to claim 1 or 2, characterized in that In step 2a, the ratio of the mass of the MXene nanosheet powder to the volume of N,N-dimethylformamide is 1 g: (350-450) mL.
5. The method for preparing an aluminum ion-doped Co9S8 / MXene heterostructure composite material according to claim 1 or 2, characterized in that In step 2a, the mass ratio of MXene nanosheet powder to cobalt chloride hexahydrate is 1:(5-7).
6. The method for preparing an aluminum ion-doped Co9S8 / MXene heterostructure composite material according to claim 1 or 2, characterized in that In step 2a, the molar ratio of cobalt chloride hexahydrate, aluminum chloride hexahydrate and thiourea is 1:(0.1-0.2):(3-3.5).
7. The method for preparing an aluminum ion-doped Co9S8 / MXene heterostructure composite material according to claim 1 or 2, characterized in that In step 2b, when ethanol and deionized water are centrifuged, the centrifugation is performed at a rotation speed of 10,000 to 11,000 rpm for 5 to 20 minutes.
Citation Information
Patent Citations
Aluminum ion battery and positive electrode material CoxSy@MXene thereof
CN112599769A
MXene / ZnMnNi LDH Van der Waals heterostructure, preparation method and application thereof
CN111599603A
Preparation method, product and application of nitrogen-doped MXene loaded molybdenum disulfide composite material
CN114512653A
Preparation method of metal-sulfur in-situ co-doped MXene electrode material
CN114843510A
Method for preparing sulfur-doped rese 2 / mxene composite material
WO2022032747A1