A low conductivity coolant and preparation method thereof

By using glycol-modified composite metal oxide as an ion capture agent in the coolant, the conductivity of the coolant is reduced, the problems of circuit short circuit and corrosion after coolant leakage are solved, and high stability and low cost are achieved. The preparation of low conductivity coolant is suitable for liquid cooling systems with high safety requirements.

CN115418202BActive Publication Date: 2024-10-08ZHANGJIAGANG TEEC AUTOMOTIVE CHEMICALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211152686.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-21
Publication Date
2024-10-08
Estimated Expiration
2042-09-21

AI Technical Summary

Technical Problem

The high conductivity of the existing coolant causes circuit short circuits and corrosion easily after leakage, affecting the safety of the equipment. Moreover, adding organic corrosion inhibitors has poor stability and high cost, which limits its application.

Method used

Ethylene glycol-modified composite metal oxide is used as an ion trapping agent, and its structural memory effect is used to capture ions in the coolant, reduce the conductivity, and prepare a low-conductivity coolant through a specific preparation method.

Benefits of technology

Significantly reduces the conductivity of the coolant, improves its stability and service life, reduces costs, overcomes the stability and cost problems of organic corrosion inhibitor coolant, and provides efficient anti-corrosion performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003857584490000041
    Figure BDA0003857584490000041
Patent Text Reader

Abstract

The present invention discloses a low-conductivity coolant and a preparation method thereof. The present invention utilizes the structural memory effect of composite metal oxides and the characteristics of simultaneously capturing cations and anions during the conversion process of composite metal oxides into hydrotalcite precursors to effectively reduce the concentration of free cations and anions in the coolant, thereby reducing the conductivity of the coolant and improving its working safety. The mass percentage composition of the coolant is 20-79% ethylene glycol, 20-79% deionized water, and 1-5% ion capture agent. The coolant has the advantages of low conductivity, long service life, simple preparation method, low cost, and easy industrial production, and overcomes the problems of poor stability, short service life, and high cost of coolants with organic corrosion inhibitors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coolants, and in particular to a low-conductivity coolant and a preparation method thereof. Background Art

[0002] Coolant is an indispensable cooling and heat dissipation medium for the cooling system. It has the functions of cooling, anti-corrosion, anti-scaling, and anti-freezing. It is composed of water, antifreeze and various additives (mainly corrosion inhibitors, supplemented by buffers, anti-scaling agents, defoamers and colorants). The study of coolant was born in the 1930s and entered China in the 1970s. The research has a history of 80 years. Commonly used coolants are water, alcohols (ethylene glycol aqueous solution, propylene glycol aqueous solution), polyalphaolefins (PAO), silicates, mineral oils and fluorocarbons. Among them, water is the most common and very efficient cooling medium. It is widely used in industry and life. However, due to its corrosiveness and freezing point, it cannot meet the environmental adaptability requirements of military radars. PAO is a grease, insoluble in water, and can burn when exposed to open flames, so it has poor safety. Ethylene glycol aqueous solution is the most widely used coolant due to its low freezing point, low corrosiveness, high specific heat capacity and good fluidity. However, due to its conductive properties, if the coolant leaks during long-term operation, circuit short circuits, corrosion and other phenomena are likely to occur, posing a safety hazard. Therefore, reducing the conductivity of the coolant is very important to improve the reliability and safety of the coolant.

[0003] In order to reduce the corrosion performance of the coolant, a heterocyclic nitrogen-containing compound corrosion inhibitor is usually added to the coolant. Document CN108102616A discloses a method for preparing a low-conductivity coolant with 8-hydroxyquinoline, uracil, 4-acetaminophen, benzotriazole octadecylamine, N-bromosuccinimide, and inosine as main additives, and the conductivity can reach 0.08μS / cm; Document CN102174313B discloses a method for preparing a low-conductivity coolant with natural alkaloids, heterocyclic alkanes, and azole compounds as main additives, and the conductivity can reach 5μS / cm. The added organic nitrogen-containing compound can form a chelate on the metal surface to prevent further corrosion of the metal to reduce the conductivity of the coolant. Document CN109065912A reports a coolant with a new non-ionic corrosion inhibitor added, which can reduce the conductivity of the coolant, and has a good corrosion inhibition ability for iron and aluminum-based metals, and has a good cooling effect. However, these organic corrosion inhibitors have defects such as complex preparation conditions, high prices, and poor stability, which lead to problems such as poor stability, short service life, and high cost of coolants added with organic corrosion inhibitors, limiting their application in coolants. Therefore, it is urgent to develop new high-stability, low-cost coolant preparation technologies.

[0004] In recent years, hydrotalcite, a type of anionic layered functional inorganic material with a layered structure, has attracted widespread attention due to its adjustable chemical composition, unique structure and properties. Its calcined product, layered bimetallic oxide, or LDO, has a higher specific surface area and a unique "structural memory effect" than the hydrotalcite precursor LDH. When the sample is added to a solution medium containing a certain anion, its structure can be partially restored to a hydrotalcite structure with an ordered layered structure. During the recovery process, it has a very strong active ability to compete for ions, from which it can capture cations to the laminae and anions to the interlayers, thereby forming a trap for capturing ions and effectively reducing the conductivity of the coolant. Therefore, it is of great significance to prepare a low-conductivity coolant based on this research. Summary of the invention

[0005] The present invention aims to provide a low-conductivity coolant and a preparation method thereof. The coolant has low conductivity and still has long-term insulation performance even after accidental leakage, and will not affect the normal operation of the equipment.

[0006] In one aspect, the present invention provides a low-conductivity coolant, which is composed of the following components by mass percentage: 20-79% ethylene glycol, 20-79% deionized water, and 1-5% ion capture agent;

[0007] The general chemical formula of ion capture agent is:

[0008] M 2+ 1-x M 3+ x O 1+x / 2 ·nEG

[0009] Where EG is ethylene glycol, 0.2≤x≤0.33, 0.5≤n≤2; M 2+ Mg 2+ 、Zn 2+ 、Ni 2+ , Ca 2+ , Fe 2+ Cu 2+ Any one or two of M 3+ For Al 3+ 、Co 3+ 、Ti 3+ , Fe 3+ or Cr 3+ Any one of .

[0010] Preferably, M 2+ Mg 2+ 、Zn 2+ or Ca 2+ Any one or two of M 3+ For Al 3+ .

[0011] On the other hand, the present invention provides a method for preparing the low conductivity coolant as described above, the specific steps are as follows:

[0012] A. M 2+ 、M 3+ The soluble salt and urea are dissolved in a mixed solvent to prepare a mixed solution, wherein M 3+ The molar concentration is 0.02~0.5mol / L, M 2+ With M 3+ The molar ratio of urea to M is 2 to 4. 3+ The molar ratio of the hydrotalcite is 6 to 12, and then placed in a reaction kettle, heated to 90 to 150° C., reacted for 2 to 12 hours, after the reaction, the precipitate was filtered and washed to neutrality, and the obtained wet cake was dried at 80 to 120° C. for 6 to 12 hours to obtain a hydrotalcite precursor;

[0013] B. Place the hydrotalcite precursor prepared in step A in a muffle furnace, heat to 450-600°C at a heating rate of 2-10°C / min in an air atmosphere, and keep warm for 2-6 hours to obtain a composite metal oxide M 2+ 1-x M 3+ x O 1+x / 2 , where 0.2≤x≤0.33;

[0014] C. Add the composite metal oxide obtained in step B to ethylene glycol, grind it with a colloid mill for 5 to 20 minutes to obtain a slurry with a solid content of 15 to 30%, and then heat the slurry to 90 to 150° C. and react for 2 to 6 hours to obtain a ethylene glycol-modified composite metal oxide M. 2+ 1-x M 3+ x O 1+x / 2 ·nEG (wherein 0.5≤n≤2) slurry; deionized water and ethylene glycol are added to the slurry, and ground with a colloid mill for 5 to 20 minutes to obtain an ethylene glycol / water type coolant, wherein the mass percentage of ethylene glycol-modified composite metal oxide in the coolant is 1 to 5%, the mass percentage of ethylene glycol is 20 to 79%, and the mass percentage of deionized water is 20 to 79%.

[0015] Preferably, M 2+ The soluble salt is Mg 2+ 、Zn 2+ 、Ni 2+ , Ca 2+ , Fe 2+ , Cu 2+ nitrate, sulfate or chloride; M 3+ The soluble salt is Al 3+、Co 3+ 、Ti 3+ , Fe 3+ Cr 3+ nitrates, sulfates or chlorides.

[0016] Preferably, M 2+ The soluble salt is Mg 2+ 、Zn 2+ or Ca 2+ Any one or two of M 3+ The soluble salt is Al 3+ nitrates, sulfates or chlorides.

[0017] Preferably, the mixed solvent is a mixture of deionized water and ethanol, ethylene glycol or glycerol.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The present invention uses ethylene glycol modified composite metal oxide M 2+ 1-x M 3+ x O 1+x / 2 nEG is an ion capture agent. With its structural memory effect, it can capture anions and cations in the coolant efficiently while restoring the layered structure of the hydrotalcite precursor, greatly reducing the free anions and cations in the coolant, thereby significantly reducing the conductivity of the coolant, which is 0.1-1μS / cm. The ethylene glycol-modified composite metal oxide has the characteristics of large adsorption capacity, high stability, and convenient synthesis. Therefore, the prepared coolant exhibits the advantages of low conductivity, long service life, simple preparation method, low cost, and easy industrial production, overcoming the problems of poor stability, short service life, and high cost of coolants with organic corrosion inhibitors. DETAILED DESCRIPTION

[0020] In order to enable those skilled in the art to better understand the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments.

[0021] Example 1

[0022] The preparation method of the low conductivity coolant ion capture agent in this embodiment is carried out according to the following steps:

[0023] A. Dissolve 59.5 g Zn(NO3)2·6H2O, 37.5 g Al(NO3)3·9H2O, and 42.0 g urea in 600 mL of a mixed solvent of deionized water and ethylene glycol in a volume ratio of 1:1 to obtain a mixed solution; transfer the solution into a reactor, heat it to 90°C and react at a constant temperature for 8 hours. After the reaction is completed, filter the obtained precipitate, wash it to neutrality, and then place the filter cake in a 90°C oven to dry for 8 hours to obtain a ZnAl hydrotalcite precursor;

[0024] B. placing the obtained ZnAl hydrotalcite precursor in a muffle furnace, heating it to 500° C. at a heating rate of 5° C. / min, keeping the temperature for 3 h, and cooling it to obtain a ZnAl composite metal oxide;

[0025] C. Weigh 5 g of ZnAl composite metal oxide and add it to 20 g of ethylene glycol. Grind it with a colloid mill for 8 min to obtain a slurry. Heat the slurry to 100°C and react for 4 h to obtain a slurry containing ethylene glycol-modified ZnAl composite metal oxide. Then, add 75 g of ethylene glycol and 100 g of deionized water, and grind it with a colloid mill again for 5 min to obtain an ethylene glycol / water type coolant containing ZnAl composite metal oxide. The conductivity of the coolant is 0.81 μS / cm, and the mass percentage of ZnAl composite metal oxide is 2.5%.

[0026] The coolant has excellent corrosion resistance. Brass, copper, aluminum alloy sheets and stainless steel sheets were immersed in the coolant at 80°C for 7 days, and their weight changes were measured. The results are shown in Table 1.

[0027] Example 2

[0028] A. Dissolve 76.9 g Mg(NO3)2·6H2O, 37.5 g Al(NO3)3·9H2O, and 45.0 g urea in 600 mL of a mixed solvent of deionized water and ethylene glycol in a volume ratio of 2:1 to obtain a mixed solution; transfer the solution into a reactor, heat to 120°C and react at a constant temperature for 6 hours. After the reaction is completed, filter the obtained precipitate, wash it to neutrality, and then place the filter cake in an oven at 100°C and dry it for 8 hours to obtain a MgAl hydrotalcite precursor;

[0029] B. placing the obtained MgAl hydrotalcite precursor in a muffle furnace, heating it to 550° C. at a heating rate of 10° C. / min, keeping the temperature for 4 h, and cooling it to obtain a MgAl composite metal oxide;

[0030] C. Weigh 10 g of MgAl composite metal oxide and add it to 30 g of ethylene glycol. Grind it with a colloid mill for 10 min to obtain a slurry. Heat the slurry to 120°C and react for 3 h to obtain a slurry containing ethylene glycol-modified MgAl composite metal oxide. Then, add 170 g of ethylene glycol and 290 g of deionized water, and grind it with a colloid mill again for 6 min to obtain an ethylene glycol / water type coolant containing MgAl composite metal oxide. The conductivity of the coolant is 0.79 μS / cm, and the mass percentage of MgAl composite metal oxide is 2%.

[0031] The coolant has excellent corrosion resistance. Brass, copper, aluminum alloy sheets and stainless steel sheets were immersed in the coolant at 80°C for 7 days, and their weight changes were measured. The results are shown in Table 1.

[0032] Comparative Example:

[0033] The metal corrosion test was conducted with commercially available ethylene glycol / water type coolant as a comparative sample. Brass, copper, aluminum alloy sheets, and stainless steel sheets were immersed in the commercially available coolant at 80°C for 7 days, and their weight changes were measured. The results are shown in Table 1.

[0034] Table 1 Coolant test results of Examples 1, 2 and Comparative Examples

[0035]

[0036] It can be concluded from Table 1 that the coolant provided by the embodiment of the present invention has an electrical conductivity of about 0.8 μS / cm, which is much less than 5 μS / cm, and can be used in liquid cooling systems with relatively high electrical conductivity requirements. The coolant of the present invention can effectively alleviate metal corrosion, extend the use time of the coolant, and ensure safe operation of the machine.

[0037] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A method for preparing a low-conductivity coolant, characterized in that: The specific steps are as follows: A. M 2+ 、M 3+ The soluble salt and urea are dissolved in a mixed solvent to prepare a mixed solution, wherein M 3+ The molar concentration is 0.02~0.5mol / L, M 2+ With M 3+ The molar ratio of urea to M is 2 to 4. 3+ The molar ratio of is 6 to 12, and then placed in a reaction kettle, heated to 90 to 150 ° C, reacted for 2 to 12 hours, after the reaction, the precipitate is filtered and washed to neutrality, and the obtained wet cake is dried at 80 to 120 ° C for 6 to 12 hours to obtain a hydrotalcite precursor, wherein M 2+ Mg 2+ 、Zn 2+ 、Ni 2+ , Ca 2+ , Fe 2+ Cu 2+ Any one or two of M 3+ For Al 3+ 、Co 3+ 、Ti 3+ , Fe 3+ or Cr 3+ Any of the following: B. Place the hydrotalcite precursor prepared in step A in a muffle furnace, heat to 450-600°C at a heating rate of 2-10°C / min in an air atmosphere, and keep warm for 2-6 hours to obtain a composite metal oxide M 2+ 1-x M 3+ x O 1+x / 2 , where 0.2≤x≤0.33; C. Add the composite metal oxide obtained in step B to ethylene glycol, grind it with a colloid mill for 5 to 20 minutes to obtain a slurry with a solid content of 15 to 30%, and then heat the slurry to 90 to 150° C. and react for 2 to 6 hours to obtain a ethylene glycol-modified composite metal oxide M. 2+ 1-x M 3+ x O 1+x / 2 ·nEG (wherein 0.5≤n≤2) slurry; deionized water and ethylene glycol are added to the slurry, and ground with a colloid mill for 5 to 20 minutes to obtain an ethylene glycol / water type coolant, wherein the mass percentage of ethylene glycol-modified composite metal oxide in the coolant is 1 to 5%, the mass percentage of ethylene glycol is 20 to 79%, and the mass percentage of deionized water is 20 to 79%.

2. The method for preparing a low-conductivity coolant according to claim 1, characterized in that: The M 2+ The soluble salt is Mg 2+ 、Zn 2+ 、Ni 2+ , Ca 2+ , Fe 2+ , Cu 2+ nitrate, sulfate or chloride; said M 3+ The soluble salt is Al 3+ 、Co 3 + 、Ti 3+ , Fe 3+ Cr 3+ nitrates, sulfates or chlorides.

3. The method for preparing a low-conductivity coolant according to claim 2, characterized in that: The M 2+ The soluble salt is Mg 2+ 、Zn 2+ or Ca 2+ Any one or two of the M 3+ The soluble salt is Al 3+ Nitrates, sulfates and chlorides.

4. The method for preparing a low-conductivity coolant according to claim 1, characterized in that: The mixed solvent is a mixture of deionized water and ethanol, ethylene glycol or glycerol.