A method for preparing Na3V2(PO4)2F3-based sodium ion battery positive electrode material
Through the low-temperature hydrothermal synthesis method, a uniform cube-shaped NVPF is prepared by synergistically using PVP and carbon nanotubes, which solves the irregular morphology and fluorine element loss caused by high-temperature sintering, and realizes a highly efficient and low-cost positive electrode of sodium ion battery The preparation of materials improves the electronic conductivity and cyclic stability of the materials.
Patent Information
- Application Number
- CN202211121308.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-09-15
AI Technical Summary
The high-temperature sintering method of existing Na3V2(PO4)2F3(NVPF) sodium ion battery positive electrode material leads to irregular particles, agglomeration and loss of fluorine elements, increasing energy consumption and impurity phases, making it difficult to meet the needs of green, cheap and efficient synthesis. .
Using the low-temperature hydrothermal synthesis method of synergistic interaction between polyvinylpyrrolidone (PVP) and carbon nanotubes, a cube-shaped NVPF with good crystallization and uniform morphology was prepared in one step through hydrothermal reaction, forming a multi-dimensional conductive network structure, avoiding additional annealing and Fluorine is lost.
The uniformity and structural stability of NVPF particles are achieved, energy consumption and cost are reduced, electronic conductivity and cyclic stability are enhanced, and excellent rate performance and cyclic performance are shown.
Smart Images

Figure CN115425201B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a Na 3 V 2 (PO 4 ) 2 F 3 The invention discloses a method for preparing a positive electrode material for a sodium ion battery, and belongs to the technical field of preparing a positive electrode material for a sodium ion battery. Background Art
[0002] Energy is an important driving force for the development of today's society. With the extensive use of fossil fuels, the increasingly serious energy crisis and environmental pollution problems have forced people to start paying attention to clean and efficient new renewable energy. Considering that new renewable energy sources such as solar energy and wind energy are intermittent and random, and are greatly affected by geographical factors, if they are directly connected to the power grid, the unstable frequency will cause a certain degree of impact on the power grid. Therefore, the development of safe and reliable energy storage systems is the key to their development and utilization. Among the many energy storage technologies, electrochemical battery energy storage is widely used in our daily lives due to its excellent portability.
[0003] As a typical representative of electrochemical batteries, lithium-ion batteries have the advantages of high energy density and long cycle life, and are widely used in various portable electronic products. With the rapid promotion of new energy vehicles driven by lithium-ion batteries, the problem of lithium resource shortage has become increasingly prominent, and lithium-ion batteries cannot meet the growing demand for large-scale energy storage. Sodium and lithium have similar physical and chemical properties, and sodium reserves are abundant (2.83% of the earth's crust abundance, ranking sixth). Sodium-ion batteries, which have resource and price advantages, are considered to be potential substitutes for lithium-ion batteries and have great application prospects in large-scale energy storage.
[0004] In sodium-ion batteries, the cathode material provides active sodium ions and high-potential redox couples, playing a vital role in determining the operating voltage and reversible capacity of the battery. 3 V 2 (PO 4 ) 2 F 3 (NVPF) has a sodium superion conductor (NASICON) structure with good structural stability, a high voltage platform and theoretical specific capacity. The large ion diffusion channel facilitates the rapid escape and embedding of sodium ions. It is a positive electrode material with great application potential.
[0005] According to current reports, solid-phase reaction and sol-gel method are common NVPF synthesis methods. The above methods usually require high-temperature sintering to obtain NVPF with good crystallinity. High temperature will cause NVPF particles to become irregular and uneven, or even agglomerate to form larger clusters, which is not conducive to the transmission of sodium ions. In addition, fluorine may be lost during the calcination process, thereby introducing some impurity phases, such as Na 3 V 2 (PO 4 ) 3 In addition, the long calcination process will undoubtedly greatly increase energy consumption. Therefore, it is urgent to develop a green, cheap and simple NVPF synthesis route. Summary of the invention
[0006] In view of the problems existing in the current preparation process of NVPF sodium ion positive electrode materials, the present invention provides a Na 3 V 2 (PO 4 ) 2 F 3 The invention discloses a method for preparing a positive electrode material for a sodium-ion battery. Under the synergistic effect of polyvinylpyrrolidone (PVP) and carbon nanotubes, a low-temperature hydrothermal synthesis route is adopted to prepare a cubic NVPF with good crystallization and uniform morphology in one step. At the same time, the added carbon nanotubes also form a multi-dimensional conductive network structure on the surface of the NVPF. The method does not require additional annealing treatment, reduces energy consumption, and solves the problems of irregular morphology and agglomeration of NVPF existing in the current high-temperature synthesis process. In addition, the multi-dimensional conductive network on the surface of the NVPF improves the wettability of the electrolyte, reduces the internal diffusion resistance, and provides a fast pathway for electron transfer between NVPF particles, thereby enhancing the poor electronic conductivity of the NVPF. Moreover, the cubic NVPF has good structural stability during the cycle, so that the material has excellent rate performance and cycle stability.
[0007] The objectives of the present invention are achieved through the following technical solutions.
[0008] A Na 3 V 2 (PO 4 ) 2 F 3 The method for preparing a positive electrode material for a sodium-ion battery comprises the following steps:
[0009] (1) H 3 PO 4 , H 2 C 2 O 4 NH 4 VO 3, NaF is dissolved in water according to a stoichiometric ratio and stirred evenly, then an aqueous solution of PVP is added and stirred evenly, and then carbon nanotubes are added and dispersed evenly by ultrasonication to obtain a mixed reaction solution;
[0010] (2) The mixed reaction solution is transferred to a reactor for hydrothermal reaction, reacted at 120-250° C. for 8-15 hours, and then cooled naturally. The solid product is then collected and washed and dried to obtain a uniformly distributed cubic NVPF with a surface modified with a carbon nanotube conductive network, namely, Na 3 V 2 (PO 4 ) 2 F 3 Sodium-ion battery cathode materials.
[0011] Furthermore, in step (1), the amount of PVP added is 1 to 30% of the theoretical mass of the target product NVPF.
[0012] Furthermore, in step (1), the amount of carbon nanotubes added is 1 to 20% of the theoretical mass of the target product NVPF.
[0013] More preferably, in step (1), the amount of PVP added is 8-15% of the theoretical mass of the target product NVPF, and the amount of carbon nanotubes added is 8-15% of the theoretical mass of the target product NVPF.
[0014] Furthermore, the carbon nanotubes are single-walled carbon nanotubes, multi-walled carbon nanotubes or element-doped carbon nanotubes (such as nitrogen-doped carbon nanotubes, phosphorus-doped carbon nanotubes, sulfur-doped carbon nanotubes, etc.).
[0015] Furthermore, the concentrations of PVP and carbon nanotubes in the mixed reaction solution are 3.5 mg / mL to 5.4 mg / mL, respectively.
[0016] Beneficial effects:
[0017] (1) From the perspective of grain growth, the addition of carbon nanotubes helps to induce the crystallization and nucleation of NVPF particles, making the size of the in-situ grown NVPF particles more uniform, and at the same time inhibiting the excessive growth of NVPF grains to a certain extent. At the same time, PVP as a surfactant can not only improve the dispersibility of the raw materials but also have an important influence on the morphology of the grains. Under the joint action of PVP and carbon nanotubes, NVPF particles with uniform cubic shape are finally obtained.
[0018] (2) From the cost point of view, the present invention is synthesized in one step by low-temperature hydrothermal reaction, and no additional high-temperature treatment process is required, which greatly reduces energy consumption; and the raw materials for synthesizing NVPF include H 3 PO 4 , H 2 C2 O 4 NH 4 VO 3 and NaF, are very common and have great cost advantages compared to the high prices of organic raw materials such as vanadium acetylacetonate.
[0019] (3) From the perspective of green chemistry, the solvents used in the solvothermal synthesis of NVPF, such as N,N-dimethylformamide, ethanol, acetone, and acid-base coupling extractants (coupled by PC-88A and N1923), are usually toxic and harmful to the environment. The organic high-pressure steam generated during the reaction has high requirements for the reaction vessel, which undoubtedly increases the cost. The present invention uses deionized water as a solvent, which is a green, low-cost synthesis route and is convenient for practical application.
[0020] (4) From the performance point of view, the product prepared by the method of the present invention has good crystallinity. The reduction and crystallization of the material are completed simultaneously in the hydrothermal process, and no additional heat treatment is required, which avoids the loss of fluorine during the calcination process and avoids the Na 3 V 2 (PO 4 ) 3 The appearance of the impure phase; and the generated cubic NVPF is evenly distributed, and the regular morphology helps to ensure the structural integrity of the product during the cycle and inhibits the crushing of the particles. At the same time, the multi-dimensional conductive network formed by carbon nanotubes on the surface of NVPF improves the permeability of the electrolyte, reduces the internal diffusion resistance, and significantly improves the electronic transmission of the composite material, enhances the electronic conductivity of NVPF, and exhibits excellent cycle performance and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a comparison chart of X-ray diffraction (XRD) of the positive electrode materials prepared in Example 1 and Comparative Examples 1 to 3.
[0022] Figure 2 Scanning electron microscope (SEM) images of the positive electrode material prepared in Example 1 at different magnifications.
[0023] Figure 3 Scanning electron microscope images of the positive electrode material prepared in Comparative Example 1 at different magnifications.
[0024] Figure 4 Scanning electron microscope images of the positive electrode material prepared in Comparative Example 2 at different magnifications.
[0025] Figure 5 Scanning electron microscope images of the positive electrode material prepared in Comparative Example 3 at different magnifications.
[0026] Figure 6It is a comparison chart of the rate performance of sodium ion batteries assembled using the positive electrode materials prepared in Example 1 and Comparative Examples 1 to 3, respectively. DETAILED DESCRIPTION
[0027] The present invention is further described below in conjunction with specific embodiments, wherein the methods are conventional methods unless otherwise specified, and the raw materials can be obtained from public commercial channels unless otherwise specified.
[0028] In the following examples and comparative examples, the assembly steps of the sodium ion battery are as follows: the positive electrode material, conductive carbon black (SuperP) and polyvinylidene fluoride (PVDF) prepared in the example or comparative example are weighed in a mass ratio of 7:2:1, and N-methylpyrrolidone (NMP) is used as a solvent. The slurry is fully ground into a uniform slurry in a mortar, and the slurry is evenly applied on an aluminum foil using a scraper, and dried at 80°C for 12 hours under a vacuum environment. The slice is sliced using a slicer, and the slice is used as the positive electrode; in addition, a metal sodium sheet is used as the negative electrode, a glass fiber (Whatman GF / C) is used as a separator, and the electrolyte is 1 mol / L sodium perchlorate (NaClO 4 ) was dissolved in polycarbonate (PC) and 5 vol% of fluoroethylene carbonate (FEC) was added, and assembled into CR2032 button cells in a glove box filled with argon gas and with water and oxygen values below 0.1 ppm.
[0029] Example 1
[0030] (1) Add 105 μL of 85% H 3 PO 4 , 0.8268 g H 2 C 2 O 4 、0.7090g NH 4 VO 3 and 0.3799 g NaF were dissolved in 20 mL deionized water and stirred for 30 min to mix evenly, then 15 mL of an aqueous solution containing 0.1254 g PVP was added and stirred for 30 min to mix evenly, then 0.1254 g nitrogen-doped carbon nanotubes (NCNTs, Xianfeng Nano nitrogen-doped multi-walled carbon nanotubes XFM63, the same below) were added and ultrasonically dispersed for 30 min to obtain a mixed reaction solution;
[0031] (2) The mixed reaction solution was transferred to a hydrothermal reactor and subjected to a hydrothermal reaction at 180° C. for 12 h. After the hydrothermal reaction was completed, the mixture was naturally cooled to room temperature, and the solid product was collected by centrifugation. The solid product was washed three times with deionized water, and then dried and ground to obtain a uniformly distributed cubic NVPF with a surface modified with a carbon nanotube conductive network, namely, Na 3 V 2 (PO4 ) 2 F 3 Based sodium ion battery positive electrode material, abbreviated as NVPF / PVP / NCNTs positive electrode material.
[0032] Example 2
[0033] (1) Add 105 μL of 85% H 3 PO 4 , 0.8268 g H 2 C 2 O 4 、0.7090g NH 4 VO 3 and 0.3799 g NaF were dissolved in 20 mL deionized water and stirred for 30 min to mix evenly, then 15 mL of an aqueous solution containing 0.2508 g PVP was added and stirred for 30 min to mix evenly, and then 0.2508 g nitrogen-doped carbon nanotubes were added and ultrasonically dispersed for 30 min to obtain a mixed reaction solution;
[0034] (2) The mixed reaction solution was transferred to a hydrothermal reactor and subjected to a hydrothermal reaction at 180° C. for 12 h. After the hydrothermal reaction was completed, the mixture was naturally cooled to room temperature, and the solid product was collected by centrifugation. The solid product was washed three times with deionized water, and then dried and ground to obtain a uniformly distributed cubic NVPF with a surface modified with a carbon nanotube conductive network, namely, Na 3 V 2 (PO 4 ) 2 F 3 Based sodium ion battery positive electrode material, abbreviated as NVPF / PVP / NCNTs positive electrode material.
[0035] The positive electrode material prepared in Example 2 was subjected to phase analysis. According to the test results, the diffraction peak in the XRD spectrum corresponds to the NVPF peak phase (COD ID: 1521543), and there is no other impurity phase, indicating that a well-crystallized pure phase NVPF was successfully synthesized, and the addition of PVP and NCNTs does not affect the crystal structure of NVPF.
[0036] The positive electrode material prepared in Example 2 was characterized by microscopic morphology. From the characterization results, it can be seen that a relatively evenly distributed cubic micron-sized NVPF with a side length of ~15 μm was obtained, but there was a phenomenon of several particles being piled together locally.
[0037] The positive electrode material prepared in Example 2 was assembled into a sodium ion battery, and tested at the rates of 0.1C, 0.2C, 0.5C, 1C, 2C, and 0.1C in sequence, with a test voltage window of 2.0 to 4.3V and a test temperature of 25°C. The test results showed that the battery had a discharge capacity of 117.35mAh / g, 114.89mAh / g, 92.61mAh / g, 86.32mAh / g, and 73.39mAh / g at current densities of 0.1C, 0.2C, 0.5C, 1C, and 2C, respectively, and when it returned to the current density of 0.1C, it still had a discharge capacity of 110.49mAh / g, equivalent to 94.2% of the initial discharge capacity. The test results of the above rate performance show that under the combined action of PVP and nitrogen-doped carbon nanotubes, the NVPF / PVP / NCNTs positive electrode material synthesized by the hydrothermal method has excellent rate performance and cycle stability.
[0038] Comparative Example 1
[0039] Add 105 μL of 85% HO 3 PO 4 , 0.8268 g H 2 C 2 O 4 、0.7090g NH 4 VO 3 and 0.3799 g NaF were dissolved in 35 mL deionized water and stirred for 30 min to mix evenly, then transferred to a hydrothermal reactor and subjected to hydrothermal reaction at 180 ° C for 12 h. After the hydrothermal reaction was completed, it was naturally cooled to room temperature, and the solid product was collected by centrifugation. The solid product was washed three times with deionized water, and then dried and ground to obtain NVPF positive electrode material.
[0040] Comparative Example 2
[0041] (1) Add 105 μL of 85% H 3 PO 4 , 0.8268 g H 2 C 2 O 4 、0.7090g NH 4 VO 3 and 0.3799 g NaF were dissolved in 20 mL deionized water and stirred for 30 min to mix evenly, and then 15 mL of an aqueous solution containing 0.1254 g PVP was added and stirred for 30 min to mix evenly to obtain a mixed reaction solution;
[0042] (2) The mixed reaction solution was transferred to a hydrothermal reactor and subjected to a hydrothermal reaction at 180° C. for 12 h. After the hydrothermal reaction was completed, the mixture was naturally cooled to room temperature, and the solid product was collected by centrifugation. The solid product was washed three times with deionized water, and then dried and ground to obtain NVPF / PVP positive electrode material.
[0043] Comparative Example 3
[0044] (1) Add 105 μL of 85% H 3 PO 4 , 0.8268 g H 2 C 2 O 4 、0.7090g NH 4 VO 3 and 0.3799 g NaF were dissolved in 35 mL deionized water and stirred for 30 min to mix evenly, and then 0.1254 g nitrogen-doped carbon nanotubes were added and ultrasonically dispersed for 30 min to obtain a mixed reaction solution;
[0045] (2) The mixed reaction solution was transferred to a hydrothermal reactor and subjected to a hydrothermal reaction at 180° C. for 12 h. After the hydrothermal reaction was completed, the mixture was naturally cooled to room temperature, and the solid product was collected by centrifugation. The solid product was washed three times with deionized water, and then dried and ground to obtain NVPF / NCNTs positive electrode material.
[0046] Performance characterization:
[0047] Phase analysis was performed on the positive electrode materials prepared in Example 1 and Comparative Examples 1 to 3. Figure 1 It can be seen from the XRD spectrum that there is no obvious difference in the peak positions of all the diffraction peaks of the above four positive electrode materials, all of which can correspond to the NVPF peak phase (COD ID: 1521543), and are tetragonally symmetrically indexed with the P42 / mnm space group. No other impurity phases were detected, indicating that the hydrothermal method can successfully synthesize well-crystallized pure phase NVPF, and the addition of PVP and NCNTs does not affect the crystal structure of NVPF.
[0048] The positive electrode materials prepared in Example 1 and Comparative Examples 1 to 3 were characterized by microscopic morphology. The test results are as follows: Figures 2 to 5 shown. Figure 2 The SEM image shows that, under the combined action of PVP and nitrogen-doped carbon nanotubes, Example 1 forms evenly distributed cubic micron-sized NVPFs with a side length of about 20 μm. Figure 3 The SEM showed that the NVPF particles were severely stacked. Figure 4 The SEM showed that the dispersion of NVPF / PVP particles was improved, but the particle size was uneven and the morphology was irregular. Figure 5The SEM shows that the NVPF / NCNTs particles are relatively uniform in size, but the morphology is not a regular cubic structure, and the dispersion of carbon nanotubes is poor. The above SEM characterization results show that the addition of PVP and nitrogen-doped carbon nanotubes effectively improves the dispersion of NVPF, avoids the agglomeration of NVPF particles, and regulates the morphology of NVPF particles, forming a regular and uniformly distributed cubic structure.
[0049] The positive electrode materials prepared in Example 1 and Comparative Examples 1 to 3 were assembled into sodium ion batteries, and tested at 0.1C, 0.2C, 0.5C, 1C, 2C, and 0.1C rates, with a test voltage window of 2.0 to 4.3V and a test temperature of 25°C. The test results are as follows: Figure 6 As shown. Relative to the NVPF prepared in Comparative Example 1, the rate performance of the NVPF / PVP prepared in Comparative Example 2, the NVPF / NCNTs prepared in Comparative Example 3 and the NVPF / PVP / NCNTs prepared in Example 1 are all improved. Under the synergistic effect of PVP and NCNTs, the NVPF / PVP / NCNTs prepared in Example 1 exhibits the best rate performance, and the corresponding discharge specific capacities at current densities of 0.1C, 0.2C, 0.5C, 1C and 2C can reach 120.1mAh / g, 115.1mAh / g, 103.8mAh / g, 91.3mAh / g and 74.1mAh / g, respectively, and when returning to the current density of 0.1C, there is still a discharge specific capacity of 116.9mAh / g, which is equivalent to 97.3% of the initial discharge capacity. The test results of the above rate performance show that under the joint action of PVP and nitrogen-doped carbon nanotubes, the NVPF / PVP / NCNTs positive electrode material synthesized by hydrothermal method has excellent rate performance and cycle stability, and is a potential application material for high-performance sodium-ion batteries.
[0050] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a Na3V2(PO4)2F3-based sodium ion battery positive electrode material, characterized in that: The specific steps include: (1) H3PO4, H2C2O4, NH4VO3, and NaF are dissolved in water according to a stoichiometric ratio and stirred evenly, then an aqueous solution of PVP is added and stirred evenly, and then carbon nanotubes are added and dispersed evenly by ultrasonication to obtain a mixed reaction solution; (2) The mixed reaction solution is transferred to a reactor for a hydrothermal reaction. After reacting at 120-250° C. for 8-15 hours, the mixture is naturally cooled. The solid product is then collected, washed, and dried to obtain a uniformly distributed cubic NVPF with a surface modified with a carbon nanotube conductive network, i.e., a Na3V2(PO4)2F3-based sodium ion battery positive electrode material.
2. The method for preparing a Na3V2(PO4)2F3-based sodium ion battery positive electrode material according to claim 1, characterized in that: In step (1), the amount of PVP added is 1 to 30% of the theoretical mass of the target product NVPF.
3. The method for preparing a Na3V2(PO4)2F3-based sodium ion battery positive electrode material according to claim 1, characterized in that: In step (1), the amount of carbon nanotubes added is 1 to 20% of the theoretical mass of the target product NVPF.
4. The method for preparing a Na3V2(PO4)2F3-based sodium ion battery positive electrode material according to claim 1, characterized in that: In step (1), the amount of PVP added is 8-15% of the theoretical mass of the target product NVPF, and the amount of carbon nanotubes added is 8-15% of the theoretical mass of the target product NVPF.
5. A method for preparing a Na3V2(PO4)2F3-based sodium ion battery positive electrode material according to any one of claims 1 to 4, characterized in that: The carbon nanotubes are single-walled carbon nanotubes, multi-walled carbon nanotubes or element-doped carbon nanotubes.
6. A method for preparing a Na3V2(PO4)2F3-based sodium ion battery positive electrode material according to any one of claims 1 to 4, characterized in that: The concentrations of PVP and carbon nanotubes in the mixed reaction solution are 3.5 mg / mL to 5.4 mg / mL, respectively.
Citation Information
Patent Citations
Composite cathode material of sodium-ion battery and preparation method of composite cathode material
CN106058212A
KR20210099501A