A direct quenching bath after high-speed wire laying and quenching method thereof

By designing a quenching bath directly after high-wire spinning, and using a large-flow salt bath circulation and spray pipeline system, the problem of uneven cooling of the wire rod in the high-speed rolling mill was solved, and the stability and uniformity of the wire rod performance were improved.

CN115478150BActive Publication Date: 2024-10-22QINGDAO SPECIAL STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210888934.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-07-27
Publication Date
2024-10-22
Estimated Expiration
2042-07-27

AI Technical Summary

Technical Problem

After wire rod spinning in a high-speed rolling mill, the density varies during transportation on the roller table, resulting in uneven cooling. It is difficult to control the temperature with traditional air cooling. If the salt bath is not properly designed, bainite or proeutectoid structures may appear, affecting product performance. .

Method used

Design a direct quenching bath after high-line spinning, including an upper bath, a lower bath, a conveyor roller, a spray pipe system and a molten salt pump. Through large-flow salt bath circulation and adjustment of the salt outlet and spray pipe frequency, A constant temperature environment is formed to adapt to the cooling speed requirements of areas with different accumulation thicknesses.

Benefits of technology

It effectively improves the stability and uniformity of wire performance, avoids local overheating or overcooling, and improves the uniformity of tissue performance in the same circle.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115478150B_ABST
    Figure CN115478150B_ABST
Patent Text Reader

Abstract

The present invention is specifically a direct quenching bath after high-speed wire spinning and its use method, including an upper bath, a lower bath, a conveying roller, a spray pipe system, and a molten salt pump. The upper bath is arranged above the lower bath, and the conveying roller is laid in the upper bath along the length direction of the upper bath. The molten salt pump is connected to the spray pipe system, and the spray pipe system is arranged above the upper bath. A salt discharge port is arranged at the end of the flow direction of the salt bath in the upper bath. According to the thickness of the processed wire and the salt bath process parameters, the opening size of the salt discharge port and the frequency of the molten salt pump are adjusted so that the upper bath obtains a salt bath with a stable liquid level height, and at the same time, the wire obtains an ideal cooling speed. After the ejected salt bath cools the wire, its own temperature rises, and it flows to the rear end of the upper bath along the forward direction of the wire and enters the lower bath through the salt discharge port. The bath is specially designed according to the stacking mode, travel characteristics and phase change characteristics of the wire after spinning, which greatly improves the performance of the wire and reduces the performance fluctuation in the same circle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel rolling in the metallurgical industry, in particular to a direct quenching bath tank after high-speed wire laying and a quenching method thereof. Background Art

[0002] At present, the density of wire rods in high-speed rolling mills varies at different positions during roller transportation, especially the thickness difference between the two sides of the roller and the middle position is very large, which makes it difficult to control the cooling so that the wire rods can obtain good uniformity of the same circle structure performance. Traditional fan cooling uses a Jialing device to distribute air volume according to the accumulation of wire rods to improve the uniformity of the same circle, but because the thermal conductivity of air is relatively low, it is difficult to control the upper and lower limits of the temperature, and it is very easy to have undesirable structures. Especially for large-sized wire rods, due to the thick accumulation, on the one hand, even if the air volume is increased, the core of the wire rod in the middle position cannot obtain a sufficiently large cooling rate to form a pro-eutectoid structure, and on the other hand, excessively increasing the air volume will cause the surface of the wire rod to cool too fast and form a martensitic structure.

[0003] The use of liquid media such as salt baths and lead baths for quenching can overcome the defects of air cooling, but if the bath is not designed reasonably, new problems will arise. British patent GB2062692A, Multi-purpose apparatus for treating hot rolled steel wire rod, provides a hot rolled wire salt bath treatment tank, which uses two front and rear salt tanks, one for rapid cooling and the other for constant temperature phase change. Since the rapid cooling tank needs to use a lower temperature salt bath to achieve the purpose of rapid cooling of the wire rod, when the wire rod is cooled in this salt temperature, bainite structure often appears at the sub-surface position, which has an adverse effect on the plasticity of the wire rod.

[0004] In response to this problem, US Patent US5578150A Heat treatment process for wire rods provides a solution, that is, a salt tank is used, and a salt liquid spray device is arranged at a position where the wire rod inlet end of the salt tank is higher than or immersed in the salt liquid to enhance cooling and achieve the purpose of rapid cooling. Since the sprayed salt liquid is taken from the same salt bath tank, the abnormal bainite structure caused by too low salt temperature is effectively avoided. However, since the output of high-speed wire rods is about 100 tons / hour, the heat brought in is as high as 2.3E-10J / h. A large amount of heat is concentrated at the inlet end of the bath tank instantly, which will cause the salt liquid to heat up rapidly before it can cool down, resulting in the appearance of pro-eutectoid structure, which has an adverse effect on product performance. On the other hand, the natural defect of uneven thickness of wire rods in different areas on the high-speed wire transport roller only relies on the convection heat exchange of the bath liquid, and an overheated area will appear locally in the bath liquid, which will reduce the cooling rate of the wire rod and produce pro-eutectoid structure, and ultimately fail to effectively improve the uniformity of the performance of the same circle structure. Summary of the invention

[0005] The purpose of the present invention is to provide a direct quenching bath for high-speed wire after spinning and a quenching method thereof. The bath is specially designed according to the stacking mode, traveling characteristics and phase change characteristics of the wire after spinning. Compared with traditional air-cooled wire, the wire performance can be greatly improved and the performance fluctuation in the same circle can be reduced.

[0006] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: a high-speed wire laying direct quenching bath comprises an upper bath, a lower bath, a conveying roller, a spray pipe system, and a molten salt pump, wherein the upper bath is arranged above the lower bath, the conveying roller is laid in the upper bath along the length direction of the upper bath, the molten salt pump is connected to the spray pipe system, the spray pipe system is arranged above the upper bath, the molten salt pump is arranged outside the lower bath, and a salt discharge port is arranged at the end of the flow direction of the salt bath liquid in the upper bath.

[0007] Preferably, it also includes a bath liquid cooler, which is arranged in the lower bath tank.

[0008] Preferably, the spray pipe system includes two groups of spray pipes, and the two groups of spray pipes respectively include an inner spray pipe and an outer spray pipe, and the inner spray pipe and the outer spray pipe are respectively connected to a molten salt pump.

[0009] Preferably, the salt discharge port is covered with a baffle, and the position of the baffle is adjusted to control the opening size of the salt discharge port.

[0010] Preferably, the conveying roller comprises a plurality of rollers which penetrate the upper bath transversely and a driving motor which drives the rollers to rotate.

[0011] Preferably, the rotation speed of the roller is 0.1-1.0 m / s, the diameter of the roller is ≥100 mm, and the roller is made of heat-resistant stainless steel.

[0012] The present invention also provides a quenching method:

[0013] (1) According to the chemical composition of the produced wire and the required microstructure and mechanical properties, the salt bath temperature T and salt bath time t are determined by the CCT and TTT curves of the steel;

[0014] (2) Determine the conveying speed μ of the conveyor roller according to the length L of the upper bath and the salt bath time t, μ = L / tm / s;

[0015] (3) According to the wire specification d, rolling speed ν and conveying speed μ of the conveying roller, calculate the accumulation thickness h of the wire on the conveying roller, h = d*v / μπmm;

[0016] (4) According to the wire stacking thickness h, determine the molten salt pump opening frequency χ, 0<χ≤50Hz, and the salt discharge port opening degree λ, 0<λ<1, so that a certain liquid level height h1 is formed in the upper bath tank, satisfying h1>h, h1=(nfχ / 50*λA*Cq) 2 / 2, where the number of molten salt pumps is n, the maximum flow rate of the molten salt pump is f, the maximum opening area of ​​the salt discharge port is A, Cq is the flow coefficient, and Cq is a constant with a value of 0.6-0.65;

[0017] (5) Turn on the molten salt pump to inject the salt bath liquid in the lower bath into the upper bath.

[0018] (6) After the above preparations are completed, the conveyor roller is turned on, the laying machine starts to lay wire, and the wire coil falls on the conveyor roller, is transported by the conveyor roller through the upper bath, and is collected by the coiling station as a finished product after quenching.

[0019] Preferably, in order to reduce the poor same-turn performance of the wire coil, the frequency of the molten salt pump connected to the outer spray pipe is set to be 5%-25% higher than the frequency of the molten salt pump connected to the inner spray pipe.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] By adopting two box-structured baths and using a large-flow molten salt pump and spray pipes, the salt bath liquid forms a large circulation in the entire bath, avoiding a large temperature difference between the local wire entering the salt bath liquid and the end where the wire exits the salt bath liquid, allowing the wire to complete phase change in a constant temperature environment, thereby improving the stability and uniformity of the wire performance; at the same time, in view of the inherent characteristics of high-speed wires with uneven thickness distribution on the conveyor roller, the local convection is enhanced by adjusting the frequency of the molten salt pump, so that the cooling rate of wires in areas with different stacking thicknesses tends to be consistent, thereby improving the uniformity of the performance of the wires in the same circle. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a front view of the direct quenching bath after high-speed wire laying of the present invention;

[0023] Figure 2 It is a top view of the direct quenching bath after high-speed wire laying of the present invention;

[0024] Figure 3 It is a structural schematic diagram of the spray pipeline system of the quenching bath directly after high-speed wire laying in the present invention.

[0025] In the figure: upper bath 1, lower bath 2, conveying roller 3, spray pipe system 4, inner spray pipe 41, outer spray pipe 42, molten salt pump 5, bath liquid cooler 6, salt discharge port 7, baffle 8, close-packed roller 9, transition roller 10. DETAILED DESCRIPTION

[0026] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] See also Figure 1-3 , This embodiment provides a direct quenching bath after high-speed wire laying, which is used for austempering of high-carbon steel by sorbitization, including an upper bath 1, a lower bath 2, a conveying roller 3, a spray pipe system 4, a molten salt pump 5, and a bath cooler 6. The upper bath 1 is arranged above the lower bath 2, and the conveying roller 3 is laid in the upper bath 1 along the length direction of the upper bath 1. The molten salt pump 5 is connected to the spray pipe system 4, and the spray pipe system 4 is arranged above the upper bath 1. Five sets of spray pipe systems 4 are shown in the figure. The molten salt pump 5 is arranged outside the lower bath 2, and a salt outlet 7 is arranged at the end of the flow direction of the salt bath in the upper bath 1. The salt outlet 7 is covered with a baffle 8, and the position of the baffle 8 is adjusted to control the opening size of the salt outlet 7, and the bath cooler 6 is arranged in the lower bath 2. The salt bath in this embodiment is composed of molten nitrate, and the use temperature is 220-600℃. The upper bath 1 of this embodiment has a length of 15m, a width of 1.2m and a depth of 0.8m; the lower bath 2 has a length of 15m, a width of 3m and a depth of 1.2m. The size of the salt outlet 7 is 1m*1m. The baffle 8 is adjusted electrically, such as by a motor, an electric cylinder or other existing methods.

[0028] The size of the upper bath 1 can be specially designed according to the process requirements, wherein the length is greater than or equal to the phase change characteristics of the quenched wire rod, that is, the product of the phase change completion time and the conveying speed of the conveyor roller, the width is determined by the circle diameter of the spinning machine and its position deviation on the conveyor roller, and the depth depends on the wire rod diameter, the spinning speed and the conveying speed of the conveyor roller The stacking thickness of the wire rod is determined.

[0029] like Figure 3 As shown, as a preferred implementation of this embodiment, the spray pipe system 4 includes two groups of spray pipes, and the two groups of spray pipes include an inner spray pipe 41 and an outer spray pipe 42, respectively, and the inner spray pipe 41 and the outer spray pipe 42 are respectively connected to a molten salt pump 5. The outer spray pipes 42 are placed directly above the wires on both sides of the conveyor roller 3, and the inner spray pipe 41 is placed directly above the wires in the middle of the conveyor roller 3. Each spray pipe has a diameter of 100 mm and a length of 1.5 m, and is placed parallel to the direction of travel of the wires. Figure 2 The layout diagram of each group of spray pipes above the upper bath 1. Each spray pipe is connected to a molten salt pump 5, which is a variable frequency pump with a flow rate of ≥50m 3 / h, head ≥1.5m. When working, turn on the molten salt pump 5, and the salt bath liquid is sprayed on the designated position of the wire coil through the inner spray pipe 41 and the outer spray pipe 42. The spray pipe is made of DN100 stainless steel pipe, in L shape, one end of which is connected to the molten salt pump 5, the other end is blocked, and holes are punched in the interval parallel to the travel direction of the wire coil to form a spray section. After the molten salt pump 5 is turned on, the spray speed of the salt bath liquid is 0-2.5m / s.

[0030] As a preferred implementation of this embodiment, the conveying roller 3 includes a plurality of rollers that transversely penetrate the upper bath 1 and a driving motor (not shown in the figure) that drives the rollers to rotate. The rollers have a diameter of ≥100 mm, are made of heat-resistant stainless steel, and are driven by a driving motor to rotate. They are used to convey the wire coils in and out of the upper bath 1, and the roller speed is adjustable within a speed range of 0.1-1.0 m / s. The front end of the conveying roller 3 is connected to the closely spaced roller 9 under the high-speed wire laying machine, and the rear end is connected to the transition roller 10 and enters the coiling station.

[0031] According to the thickness of the processed wire and the salt bath process parameters, the opening size of the salt outlet 7 and the frequency of the molten salt pump 5 are adjusted so that the upper bath 1 can obtain a salt bath with a stable liquid level and the wire can obtain an ideal cooling speed. The sprayed salt bath cools the wire and its temperature rises. It flows to the rear end of the upper bath 1 along the forward direction of the wire and enters the lower bath 2 through the salt outlet 7. The high-temperature salt liquid entering the lower bath 2 through the salt outlet 7 passes through the bath cooler 6 under the action of the pump, and after cooling, it is injected into the upper bath 1 again by the pump and the injection pipe for recycling.

[0032] This embodiment also provides a quenching method:

[0033] (1) According to the chemical composition of the produced wire and the required microstructure and mechanical properties, the salt bath temperature T and the salt bath time t are determined from the CCT and TTT curves of the steel by consulting manuals and other literature, measuring with a thermal expansion instrument, or calculating with simulation software such as JMatpro;

[0034] (2) Determine the conveying speed μ of the conveying roller 3 according to the length L of the upper bath 1 and the salt bath time t, μ=L / tm / s;

[0035] (3) According to the specification d of the wire, the rolling speed ν and the conveying speed μ of the conveying roller 3, the accumulation thickness h of the wire on the conveying roller 3 is calculated, h=d*v / μπmm;

[0036] (4) According to the wire stacking thickness h, the opening frequency x of the molten salt pump 5 is determined, 0<x≤50Hz, and the opening degree λ of the salt discharge port 7 is determined, 0<λ<1, so that a certain liquid level height h1 is formed in the upper bath 1, satisfying h1>h, h1=(nfχ / 50*λA*Cq) 2 / 2, where the number of molten salt pumps 5 is n, the maximum flow rate of the molten salt pump 5 is f, the maximum opening area of ​​the salt discharge port 7 is A, Cq is the flow coefficient, and Cq is a constant with a value of 0.6-0.65;

[0037] (5) Turn on the molten salt pump 5 to inject the salt bath liquid in the lower bath 2 into the upper bath 1. In order to reduce the poor same-turn performance of the wire coil, the frequency of the molten salt pump 5 connected to the outer spray pipe 42 is set to be 5%-25% higher than the frequency of the molten salt pump 5 connected to the inner spray pipe 41;

[0038] (6) After the above preparations are completed, the conveyor roller 3 is turned on, the spinning machine starts spinning, and the wire coil falls on the conveyor roller 3, is transported by the conveyor roller 3 through the upper bath 1, and is collected by the coiling station as a finished product after quenching.

[0039] The quenching method of this embodiment is further described in detail below with an example:

[0040] The direct quenching method after high-carbon steel wire rod YL82B high-wire spinning adopts the quenching tank and the quenching method described in this embodiment. The salt bath temperature required for the YL82B wire rod is 500-520°C, and it only takes 20 seconds to complete the troostite transformation. However, considering the influence of component segregation and radial temperature gradient of the wire rod, the conveying speed of the conveyor roller is set to 0.2m / s, that is, the salt bath isothermal quenching time is 75s to ensure that the core structure is completely transformed. The diameter of the YL82B wire rod is 12.5mm, the rolling speed is 35m / s, and the maximum accumulation thickness is about 150mm when the conveying speed of the conveyor roller is 0.2m / s. The frequency of the molten salt pump connected to the outer spray pipe is set to 40HZ, the frequency of the molten salt pump connected to the inner spray pipe is set to 32HZ, and the liquid level height of the upper bath is 400mm. Although all other high-speed wire production parameters are the same as those used in traditional air-cooled wire production, the average tensile strength of the YL82B wire rod in this embodiment after spinning and isothermal quenching in a salt bath is 1230MPa, and the strength difference in the same circle is ≤25MPa; while the average tensile strength of traditional air-cooled materials is 1180MPa, and the strength difference in the same circle is ≤60MPa.

[0041] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A quenching method using a quenching bath directly after high-speed wire laying, characterized in that: The bath comprises an upper bath, a lower bath, a conveying roller, a spray pipe system, and a molten salt pump. The upper bath is arranged above the lower bath, the conveying roller is laid in the upper bath along the length direction of the upper bath, the molten salt pump is connected to the spray pipe system, the spray pipe system is arranged above the upper bath, the molten salt pump is arranged outside the lower bath, and a salt discharge port is arranged at the end of the flow direction of the salt bath liquid in the upper bath. The quenching method using the bath is: (1) According to the chemical composition of the produced wire and the required microstructure and mechanical properties, the salt bath temperature T and salt bath time t are determined by the CCT and TTT curves of the steel; (2) Determine the conveying speed μ of the conveyor roller according to the length L of the upper bath and the salt bath time t, μ=L / tm / s; (3) According to the wire specification d, rolling speed ν and conveying speed μ of the conveyor roller, calculate the accumulation thickness h of the wire on the conveyor roller, h=d*v / μπ mm; (4) According to the wire stacking thickness h, determine the molten salt pump opening frequency χ, 0<χ≤50 Hz, and the salt discharge port opening degree λ, 0<λ<1, so that a certain liquid level height h1 is formed in the upper bath tank, satisfying h1>h, h1= (nfχ / 50*λA*Cq) 2 / 2, where the number of molten salt pumps is n, the maximum flow rate of the molten salt pump is f, the maximum opening area of ​​the salt discharge port is A, Cq is the flow coefficient, and Cq is a constant with a value of 0.6-0.65; (5) Turn on the molten salt pump to inject the salt bath liquid in the lower bath into the upper bath. (6) After the above preparations are completed, the conveyor roller is turned on, the laying machine starts to lay wire, and the wire coil falls on the conveyor roller, and is transported by the conveyor roller through the upper bath. After the quenching treatment is completed, it is collected by the coiling station as a finished product.

2. The quenching method according to claim 1, characterized in that: The spray pipe system includes two groups of spray pipes, and the two groups of spray pipes include an inner spray pipe and an outer spray pipe respectively. The inner spray pipe and the outer spray pipe are respectively connected to a molten salt pump. In order to reduce the same-turn performance difference of the wire coiling, the frequency of the molten salt pump connected to the outer spray pipe is set to be 5%-25% higher than the frequency of the molten salt pump connected to the inner spray pipe.

3. The quenching method according to claim 1, characterized in that: The bath tank further comprises a bath liquid cooler, and the bath liquid cooler is arranged in the lower bath tank.

4. The quenching method according to claim 1, characterized in that: The salt discharge port is covered with a baffle, and the position of the baffle is adjusted to control the opening size of the salt discharge port.

5. The quenching method according to claim 1, characterized in that: The conveying roller table comprises a plurality of rollers which penetrate the upper bath tank transversely and a driving motor which drives the rollers to rotate.

6. The quenching method according to claim 5, characterized in that: The rotation speed of the roller is 0.1-1.0 m / s, the diameter of the roller is ≥100 mm, and the roller is made of heat-resistant stainless steel.