Long-cycle graphite negative electrode active materials and their preparation and application in lithium secondary batteries
Through the pretreatment of graphite anode materials and the composite MOF source-hard carbon source roasting process, the problems of fast charge performance and cycle stability of graphite anodes in lithium-ion batteries are solved, and the excellent structural stability and fast charge performance of the material are achieved. Reduces cost and is suitable for lithium-ion battery applications.
Patent Information
- Application Number
- CN202211290997.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-10-21
AI Technical Summary
Graphite anodes have poor fast charging performance, poor cycle stability and safety issues in lithium-ion batteries, mainly due to poor interlayer diffusion kinetics of lithium ions, structural peeling caused by solvent co-intercalation, and lithium dendrite precipitation under fast charging. Battery short circuit or thermal runaway.
The coke powder is pretreated at low temperature in an oxygen-containing atmosphere, and the second stage of pretreatment is carried out in a subcritical fluid, followed by carbonization-graphitization treatment, and combined with the composite MOF source and hard carbon source for roasting to improve particle adaptation. and lithium-ion transmission network to enhance the structural stability and fast charging performance of the material.
It significantly improves the adaptability of lithium ions and the fast charging stability of batteries, improves long-term cycle stability, and reduces material costs, making it suitable for large-scale production.
Smart Images

Figure CN115498168B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium battery electrode materials, and in particular relates to a long-cycle lithium ion battery negative electrode material and a preparation method thereof. Background Art
[0002] Lithium-ion batteries are typical representatives of new green rechargeable battery systems, and are widely used in many fields due to their excellent performance. Graphite has become one of the core raw materials of lithium-ion batteries due to its good conductivity, layered structure suitable for lithium insertion and deinsertion, and good cycle performance.
[0003] In recent years, with the rapid development of lithium-ion new energy vehicles, the rate and cycle characteristics of artificial graphite have become increasingly prominent, and it has become the mainstream raw material for power batteries. While it is widely used commercially, its cost has also attracted widespread attention and become a hot topic of research.
[0004] The essence of the lithium insertion and extraction process of the graphite negative electrode is the insertion and extraction of lithium ions between graphite layers. Graphite negative electrodes have good theoretical capacity when used in lithium-ion batteries. However, there are still some bottleneck problems in the application of graphite: for example, the spacing between graphite layers is small, and the diffusion kinetics of lithium ions between layers are poor, resulting in poor fast charging performance; when lithium ions are embedded in the graphite structure, they are solvated lithium ions, which will lead to the co-embedding of solvent molecules, causing the graphite structure to peel off and fall off under long-term cycling conditions, and the structural stability is poor. In addition, under fast charging conditions, polarization causes lithium precipitation on the graphite surface, and the formed lithium dendrites will cause internal short circuits or thermal runaway in the battery, affecting its safety in use. Summary of the invention
[0005] Based on this, a long-cycle graphite negative electrode active material and a preparation method thereof are provided, aiming to prepare a graphite active material with excellent structural stability and fast charging performance.
[0006] The second purpose of the present invention is to provide an artificial graphite negative electrode material obtained by the preparation method.
[0007] The third purpose of the present invention is to provide the use of the artificial graphite negative electrode material obtained by the preparation method in lithium secondary batteries.
[0008] The fourth object of the present invention is to provide a lithium secondary battery comprising the artificial graphite negative electrode material prepared by the preparation method, and its negative electrode and negative electrode material.
[0009] Coating amorphous carbon materials after carbonization and graphitization of coke raw materials helps to improve various anisotropies and performance. However, the existing means have unsatisfactory compatibility between coke-based graphitized carbon particles, unsatisfactory compatibility between graphitized carbon and the outer amorphous carbon layer, and are easily affected by the cycle process, cracking and peeling, affecting the transmission of lithium ions, the embedding and de-embedding activity of lithium ions, and affecting the fast charging performance and long-range cycle stability. In response to this problem, the present invention provides the following improvement scheme:
[0010] A method for preparing a long-cycle graphite negative electrode active material, comprising:
[0011] Step (1): heating coke powder in an oxygen-containing atmosphere to perform a first pretreatment, and then placing the coke powder in a subcritical fluid to perform a second pretreatment to obtain modified coke;
[0012] The temperature of the first stage pretreatment is 200-400°C;
[0013] Step (2):
[0014] The modified coke is subjected to carbonization and graphitization treatment to obtain coke-based graphitized carbon;
[0015] Step (3)
[0016] The coke-based graphitized carbon, the composite MOF source and the hard carbon source are mixed and then calcined to obtain the long-cycle graphite negative electrode active material;
[0017] The composite MOF source comprises zinc-based MOF and transition metal-based MOF materials.
[0018] In order to solve the problems faced in preparing graphite negative electrode active materials from coke raw materials, such as unsatisfactory compatibility of particles, layers and lithium ions, unsatisfactory lithium ion storage performance and de-intercalation performance, unsatisfactory fast charging and long-range cycle stability of lithium ion batteries, the present invention innovatively pre-treats the coke powder at low temperature in an oxygen-containing atmosphere, and then pre-treats it under subcritical fluid, and then performs carbonization-graphitization and combined calcination treatment with a composite MOF source-hard carbon source. This can effectively improve the adaptability of the particles, help improve the adaptability of lithium ions, improve the electron-lithium ion transmission network and transmission channels, improve the fast charging stability, and also significantly improve the long-range cycle stability.
[0019] In the present invention, the coke powder is the powder obtained by crushing and shaping the coke raw material;
[0020] Preferably, the obtained coke powder has: D50 of 10 to 20 μm, D10 ≥ 3 μm, D90 ≤ 30 μm, D99 ≤ 50 μm, specific surface area ≤ 1.8 m2 / g, and DN10 ≥ 1 μm;
[0021] More preferably, in the coke powder, D50 is 15-17 μm; D10 ≥ 6 μm; D90 ≤ 25 μm; D99 ≤ 35 μm; and the specific surface area is ≤ 1.5 m2 / g.
[0022] In the present invention, the coke raw material may be petroleum coke, needle coke or other coke raw materials for preparing graphite known in the industry.
[0023] In the present invention, the combination of the first stage pretreatment under oxygen-containing atmosphere and the second stage pretreatment under subcritical fluid is the key to synergistically improving the compatibility between coke particles, improving the adaptability of subsequent lithium ions, and improving the fast charging and long-range cycle stability of lithium-ion batteries.
[0024] Preferably, in step (1), the oxygen-containing atmosphere is at least one of oxygen, air, oxygen-nitrogen composite gas, and oxygen-inert gas composite gas;
[0025] Preferably, in the oxygen-containing atmosphere, the volume content of oxygen is greater than or equal to 5%, preferably 15 to 50 v%;
[0026] Preferably, the first pretreatment time is 0.5 to 4 hours.
[0027] Preferably, in step (1), the medium of the subcritical fluid is water;
[0028] Preferably, the medium of the subcritical fluid is a water-aid aqueous solution, and the aid is at least one of boron oxide, boric acid, borane, and borate. Preferably, the content of the aid in the medium of the subcritical fluid is 0.05-5 g / L. The present invention unexpectedly found that under the combined synergy of the first stage pretreatment and the subcritical fluid under the oxygen-containing atmosphere, further combined with the special control of the composition of the subcritical fluid, the synergy can be further improved, and the adaptability of lithium ions can be unexpectedly further improved, which helps to improve the fast charging and cycle stability of lithium-ion batteries.
[0029] In the present invention, the subcritical fluid can be realized based on existing means, for example, the product after the first stage pretreatment is dispersed in water or a water-auxiliary compound medium, and subjected to heat-pressure treatment to create a subcritical fluid state.
[0030] In the present invention, the system in the subcritical fluid treatment stage is in a subcritical state, and the temperature is, for example, 200 to 350° C. and the pressure is 2 to 20 MPa.
[0031] Preferably, the time of the subcritical fluid treatment is 2 to 8 hours.
[0032] In the present invention, the modified coke obtained in step (1) is subjected to conventional carbonization and graphitization treatment to obtain coke-based graphitized carbon.
[0033] For example, in step (2), the carbonization atmosphere is a protective atmosphere, preferably at least one of nitrogen, inert gas, and hydrogen;
[0034] Preferably, the carbonization temperature is 950-1250°C, preferably 950-1050°C;
[0035] Preferably, the carbonization treatment time is 2 to 6 hours;
[0036] Preferably, the graphitization temperature is 2800-3200°C, preferably 2800-3000°C;
[0037] Preferably, the graphitization time is 18 to 36 hours, preferably 18 to 24 hours.
[0038] In the present invention, the prepared coke-based graphitized carbon, composite MOF and hard carbon source are innovatively composited and then calcined, which can unexpectedly improve the adaptation of lithium ions, improve the embedding and de-embedding of lithium ions, improve the transmission network, and improve fast charging and long-range cycle stability.
[0039] In the present invention, the zinc-based MOF, transition metal-based MOF and hard carbon source are the key to cooperate with the two-stage pretreatment process of step (1) and improve the fast charging performance and long-range cycle stability of the material in lithium secondary batteries.
[0040] Preferably, the zinc-based MOF is a metal-organic framework material constructed of zinc ions and ligands, preferably at least one of Zn-MOF-10, Zn-MOF-74, Zn-MOF-74, Zn-ZIF-62, and ZIF-11;
[0041] Preferably, the transition metal-based MOF is a metal-organic framework material formed by at least one transition metal of iron, nickel, and cobalt and a ligand, preferably at least one of Fe-MOFs, Co-MOFs, Co / Fe-MOFs, Fe / Ni-MOFs, Ni / Co-MOFs, and Co-ZIF;
[0042] Preferably, in the composite MOF source, the weight ratio of zinc-based MOF to transition metal-based MOF is 1:0.5-20; preferably 1:1-10.
[0043] Preferably, the hard carbon source is at least one of phenolic resin, glucose, sucrose, cellulose and lignin.
[0044] Preferably, the weight ratio of the coke-based graphitized carbon, the composite MOF source and the hard carbon source is 100:0.5-5:2-10. Preferably, the weight ratio of the coke-based graphitized carbon, the composite MOF source and the hard carbon source is 100:0.5-5:2-10.
[0045] In the present invention, the pyro-based graphitized carbon, the composite MOF source and the hard carbon source can be prepared based on the existing solid phase or liquid phase composite method.
[0046] Preferably, the calcination atmosphere is at least one of nitrogen, inert gas, and hydrogen;
[0047] Preferably, the calcination temperature is 950-1250°C, preferably 950-1050°C;
[0048] Preferably, the calcination holding time is 2 to 6 hours;
[0049] Preferably, after calcination, the long-cycle graphite negative electrode active material is obtained through purification treatment, washing, drying, depolymerization, demagnetization and screening.
[0050] Preferably, the purification is acid washing; the acid is at least one of hydrochloric acid, nitric acid, HF, and sulfuric acid;
[0051] Preferably, washing is performed until the filtrate is neutral.
[0052] The present invention also provides a long-cycle graphite negative electrode active material prepared by the preparation method, which is based on the combination of the two-stage pretreatment of step (1) and the subsequent composite MOF-hard carbon auxiliary roasting process, which can achieve synergy and give the material special particles and hierarchical adaptation structure and chemical properties. More importantly, the material has excellent fast charging performance and long-range cycle stability.
[0053] The present invention also provides an application of the artificial graphite negative electrode material prepared by the preparation method, which is used as a negative electrode active material of a lithium secondary battery.
[0054] The preferred application is to use it as a negative electrode active material, and to compound it with a conductive agent and a binder to prepare a negative electrode material. The conductive agent and the binder are all materials known in the industry.
[0055] In a further preferred application, the negative electrode material is placed on the surface of the negative electrode current collector to prepare the negative electrode. The negative electrode material of the present invention can be placed on the current collector by conventional methods, such as coating, to form the negative electrode. The current collector can be any material known in the industry.
[0056] In a further preferred application, the negative electrode, the positive electrode, the separator and the electrolyte are assembled into a lithium secondary battery.
[0057] A lithium secondary battery comprises the artificial graphite negative electrode material obtained by the preparation method.
[0058] The lithium secondary battery, the negative electrode plate comprises the graphite negative electrode material.
[0059] Preferably, the lithium secondary battery is a lithium ion battery.
[0060] The beneficial effects of the technical solution of the present invention are:
[0061] (1) The present invention innovatively pre-treats the coke powder at low temperature in an oxygen-containing atmosphere, and then pre-treats it in a subcritical fluid, and then carbonizes and graphitizes it, and then combines it with a composite MOF source-hard carbon source for calcination. This can effectively improve the adaptability of the particles, and help improve the adaptability of lithium ions, improve the electron-lithium ion transmission network and transmission channel, improve fast charging stability, and also significantly improve long-range cycle stability.
[0062] (2) In the present invention, further controlling the subcritical fluid to be a medium containing a boron source can further improve the process synergy effect of step (1) and step (3), help to further improve the material's adaptation effect to lithium ions, help to further improve the storage and de-insertion efficiency of lithium ions, and help to further improve the fast charging performance and long-range cycle stability.
[0063] (3) The main raw materials and materials of the present invention are widely available and low in cost. The process used is simple and easy to control, and it is easy to achieve large-scale production, with good prospects for practical application. BRIEF DESCRIPTION OF THE DRAWINGS
[0064] Attached Figure 1 This is the SEM image of the material obtained in Example 1.
[0065] Attached Figure 2 This is the TEM image of the material obtained in Example 1. DETAILED DESCRIPTION
[0066] The specific steps of the present invention are described below by way of examples. It should be understood that these examples are only for illustrating the present invention and are not intended to limit the scope of the present invention in any way. Various processes and methods not described in detail in the present invention are conventional methods known in the art.
[0067] Example 1
[0068] Step (1): Place the coke powder in a jet mill for crushing, and obtain a product with a D50 of 16 μm, a D10 of 8 μm, a D90 of 22 μm, a D99 of 30 μm, and a specific gravity of 1.2 μm. 2 / g; DN10 is 2μm.
[0069] Step (2): Preprocessing:
[0070] (2-1): The first stage of preprocessing:
[0071] The coke powder obtained in the previous step was placed in an atmosphere furnace, air was introduced, and the temperature was raised to 300°C (marked as T1) at a rate of 5°C / min, maintained for 3h, and naturally cooled to room temperature;
[0072] (2-2): Second stage preprocessing:
[0073] The first stage pretreatment product is then dispersed in water to form a 200 g / L dispersion, and the resulting mixed solution is placed in a closed reactor, heated to a subcritical state (temperature of 250°C, pressure of 5 MPa), maintained for 3 hours, and naturally cooled to room temperature after pressure relief. The modified material is obtained after solid-liquid separation and drying.
[0074] Step (3): The modified material is heated to 1050°C (marked as T2) at 5°C / min under argon, kept warm for 2 hours, and naturally cooled to room temperature to obtain a pretreated material, which is then placed in an Acheson crucible furnace for graphitization at a graphitization temperature of 3000°C (marked as T3) for 20 hours.
[0075] Step (4):
[0076] The graphitized material of step (3), the composite MOF and the phenolic resin are mixed in a mixed solution of water and ethanol at a weight ratio of 100:5:5, dispersed uniformly by ultrasonication, and then spray-dried to obtain a precursor;
[0077] The composite MOF includes Zn-MOF (such as Zn-MOF-10) and Fe-MOF (Fe-MIL-100) in a weight ratio of 1:10;
[0078] Step (5): Place the mixed powder from the previous step in an atmosphere furnace, and under the protection of a nitrogen atmosphere, heat it to 1050°C (marked as T4) at a rate of 5°C / min, keep it at that temperature for 4 hours, and cool it naturally to room temperature.
[0079] The obtained material is placed in a 2M hydrochloric acid solution, stirred at room temperature for 4 hours, filtered, washed, dried, and then subjected to conventional depolymerization, demagnetization, and screening to obtain the artificial graphite negative electrode material.
[0080] According to GB / T 24533-2009, CR2025 button cells were assembled in a dry glove box filled with argon with the graphite electrode as the working electrode, metallic lithium as the negative electrode, 1 mol / L LiPF6 EC / DEC / DMC (volume ratio 1:1:1) as the electrolyte, and a PE-PP composite film as the separator, and the electrochemical performance was tested at a temperature of 25° C. and a voltage range of 0.001 V to 1.5 V.
[0081] Example 2
[0082] Compared with Example 1, the only difference is that in step (2), the atmosphere of the first pretreatment stage is air and the temperature T1 is 400° C. Other operations and parameters are the same as in Example 1.
[0083] Example 3
[0084] Compared with Example 1, the only difference is that in step (2), the atmosphere of the first pretreatment stage is oxygen-Ar composite gas, wherein the oxygen content is 50v%, and the T1 temperature is 250° C. Other operations and parameters are the same as in Example 1.
[0085] Example 4
[0086] Compared with Example 1, the only difference is that in step (2), in the second pretreatment stage, the subcritical medium is an aqueous solution added with a boron source, and the second pretreatment process of the different step (2) is:
[0087] The first stage pretreatment product was dispersed in water to form a 200 g / L dispersion, 1 g / L of borane was added, the resulting mixture was placed in a closed reactor, heated to a subcritical state (temperature of 250° C., pressure of 5 MPa), maintained for 3 h, naturally cooled to room temperature after pressure relief, solid-liquid separation, and drying to obtain a modified material. Other operations and parameters were the same as in Example 1.
[0088] Example 5
[0089] Compared with Example 1, the only difference is that in step (2), the temperature and pressure of the subcritical state are changed to 300° C. and 15 MPa, respectively.
[0090] Example 6
[0091] Compared with Example 1, the only difference is that the composite MOF is changed to a mixture of Zn-MOF-10 and MIL-100 (Fe / Co, Fe / Co molar ratio is 1:1) in a mass ratio of 1:1.
[0092] Example 7
[0093] Compared with Example 1, the only difference is that the carbonization temperature T2 is changed to 950° C., the graphitization temperature T3 is changed to 2800° C. The weight ratio of the coke-based graphitized carbon, the composite MOF source and the hard carbon source is 100:0.5:2, and the subsequent calcination temperature T4 is 950° C.
[0094] Comparative Example 1:
[0095] Compared with Example 1, the only difference is that the first pretreatment stage is not performed, and other operations and parameters are the same as Example 1.
[0096] Comparative Example 2:
[0097] Compared with Example 1, the only difference is that in the first pretreatment stage, the oxygen-containing atmosphere is replaced by nitrogen, and the other operations and parameters are the same as Example 1.
[0098] Comparative Example 3:
[0099] Compared with Example 1, the only difference is that the second stage pretreatment is not performed.
[0100] Comparative Example 4:
[0101] Compared with Example 1, the only difference is that the first stage pretreatment is not performed, and in the second stage pretreatment stage, it reaches supercritical conditions (the temperature of the autoclave is 400° C. and the pressure is 25 MPa).
[0102] Comparative Example 5:
[0103] Compared with Example 1, the only difference is that the second pretreatment stage reaches supercritical conditions (the temperature of the autoclave is 400° C. and the pressure is 25 MPa).
[0104] Comparative Example 6:
[0105] Compared with Example 1, the only difference is that the composite MOF material lacks Zn-MOF-10, and the total MOF dosage remains unchanged. Other operations and parameters are the same as Example 1.
[0106] Comparative Example 7:
[0107] Compared with Example 1, the only difference is that Fe-MOF is missing in the MOF material, and the total MOF dosage remains unchanged. Other operations and parameters are the same as Example 1.
[0108] Comparative Example 8
[0109] Compared with Example 1, the only difference is that Cu-MOF is used to replace the zinc-MOF in the composite MOF, and other operations and parameters are the same as Example 1.
[0110] Comparative Example 9:
[0111] Compared with Example 1, the only difference is that phenolic resin is missing and its missing weight is supplemented by composite MOF (that is, in step (4), the weight ratio of the graphitized material in step (3) to the composite MOF is 100:10). Other operations and parameters are the same as in Example 1.
[0112] The test results of the materials obtained in the above examples and comparative examples are as follows
[0113]
[0114]
[0115] In summary, the present invention innovatively pre-treats the coke powder at a low temperature in an oxygen-containing atmosphere, and then pre-treats it under a subcritical fluid, and then carbonizes and graphitizes it, and then conducts a combined calcination treatment of a composite MOF source-hard carbon source. This can effectively improve the adaptability of the particles, and help improve the adaptability of lithium ions, improve the electron-lithium ion transmission network and transmission channels, improve fast charging stability, and in addition, can also significantly improve long-range cycle stability.
Claims
1. A method for preparing a long-cycle graphite negative electrode active material, characterized in that the steps include: Step (1): heating the coke powder in an oxygen-containing atmosphere to perform a first pretreatment, and then placing the coke powder in a subcritical fluid to perform a second pretreatment to obtain modified coke; The medium of the subcritical fluid is water, or a water-aid aqueous solution, wherein the aid is at least one of boron oxide, boric acid, borane, and borate; The temperature of the first stage pretreatment is 200~400℃; Step (2): The modified coke is subjected to carbonization and graphitization treatment to obtain coke-based graphitized carbon; Step (3) The coke-based graphitized carbon, the composite MOF source and the hard carbon source are mixed and then calcined to obtain the long-cycle graphite negative electrode active material; The composite MOF source comprises zinc-based MOF and transition metal-based MOF materials.
2. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: The coke powder is the powder obtained by crushing and shaping the coke raw material.
3. The method for preparing a long-cycle graphite negative electrode active material according to claim 2, characterized in that: The obtained coke powder has the following characteristics: D50 is 10~20μm, D10≥3μm, D90≤30μm, D99≤50μm, and specific surface area≤1.8m 2 / g, DN10≥1μm.
4. The method for preparing a long-cycle graphite negative electrode active material according to claim 2, characterized in that: The obtained coke powder has a D50 of 15-17 μm, a D10 of ≥ 6 μm, a D90 of ≤ 25 μm, a D99 of ≤ 35 μm, and a specific surface area of ≤ 1.5 m 2 / g.
5. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: In step (1), the oxygen-containing atmosphere is at least one of oxygen, air, oxygen-nitrogen composite gas, and oxygen-inert gas composite gas.
6. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: In the oxygen-containing atmosphere, the volume content of oxygen is greater than or equal to 5%.
7. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: The first pretreatment time is 0.5~4h.
8. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: In step (1), the content of the auxiliary agent in the subcritical fluid medium is 0.05-5 g / L.
9. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: The subcritical fluid treatment time is 2~8h.
10. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: In step (2), the carbonization atmosphere is a protective atmosphere.
11. The method for preparing a long-cycle graphite negative electrode active material according to claim 10, characterized in that: In step (2), the protective atmosphere is at least one of nitrogen, inert gas and hydrogen.
12. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: In step (2), the carbonization temperature is 950-1250°C.
13. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: In step (2), the carbonization treatment time is 2 to 6 hours.
14. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: In step (2), the graphitization temperature is 2800~3200℃.
15. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: In step (2), the graphitization time is 18 to 32 hours.
16. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: In the composite MOF source, the zinc-based MOF is a metal-organic framework material constructed of zinc ions and ligands.
17. The method for preparing a long-cycle graphite negative electrode active material according to claim 16, characterized in that: The zinc-based MOF is at least one of Zn-MOF-10, Zn-MOF-74, Zn-MOF-74, Zn-ZIF-62, and ZIF-11.
18. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: The transition metal-based MOF is a metal-organic framework material formed by at least one transition metal among iron, nickel and cobalt and a ligand.
19. The method for preparing a long-cycle graphite negative electrode active material according to claim 18, characterized in that: The transition metal-based MOF is at least one of Co / Fe-MOFs, Fe / Ni-MOFs, Ni / Co-MOFs, and Co-ZIF.
20. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: In the composite MOF source, the weight ratio of zinc-based MOF to transition metal-based MOF is 1:0.5~20.
21. The method for preparing a long-cycle graphite negative electrode active material according to claim 20, characterized in that: In the composite MOF source, the weight ratio of zinc-based MOF and transition metal-based MOF is 1:1~10.
22. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: The hard carbon source is at least one of phenolic resin, glucose, sucrose, cellulose and lignin.
23. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: The weight ratio of the pyro-based graphitized carbon, the composite MOF source and the hard carbon source is 100:0.5~5:2~10.
24. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: The calcination atmosphere is at least one of nitrogen, inert gas and hydrogen.
25. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: The calcination temperature is 950~1250℃.
26. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: The roasting and holding time is 2~6h.
27. The method for preparing a long-cycle graphite negative electrode active material according to claim 1, characterized in that: After calcination, the long-cycle graphite negative electrode active material is obtained through purification, washing, drying, depolymerization, demagnetization and screening.
28. The method for preparing a long-cycle graphite negative electrode active material according to claim 27, characterized in that: The purification is acid washing; the acid is at least one of hydrochloric acid, nitric acid, HF and sulfuric acid.
29. The method for preparing a long-cycle graphite negative electrode active material according to claim 28, characterized in that: Wash until the filtrate is neutral.
30. A long-cycle graphite negative electrode active material prepared by the preparation method according to any one of claims 1 to 29.
31. An application of the long-cycle graphite negative electrode active material according to claim 30, characterized in that: It is used as negative electrode active material to prepare lithium secondary batteries.
32. A negative electrode for a lithium secondary battery, comprising a current collector and a negative electrode material composited on the current collector, characterized in that: The negative electrode material comprises the long-cycle graphite negative electrode active material as described in claim 30.
33. The negative electrode of the lithium secondary battery according to claim 32, characterized in that: In the negative electrode material, the content of long-cycle graphite negative electrode active material is greater than or equal to 70wt%.
34. A lithium secondary battery, characterized in that: Comprising the negative electrode according to claim 32 or 33.