Application of organic-inorganic composite wear-resistant and friction-reducing coating in surface protection of polyetheretherketone

By depositing a silicon-oxygen co-doped amorphous carbon coating on the PEEK surface, the wear problem of PEEK materials under dry friction conditions is solved, the anti-friction performance and the application potential of the material are improved, and a stable combination of the coating and the substrate is achieved.

CN115505157BActive Publication Date: 2024-10-18NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211312397.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-25
Publication Date
2024-10-18
Estimated Expiration
2042-10-25

AI Technical Summary

Technical Problem

PEEK material has a high friction coefficient under dry friction conditions and is easy to be worn. The interface between the amorphous carbon coating and the PEEK matrix is ​​poorly matched, resulting in cracking and peeling of the coating, which limits its application and promotion.

Method used

The plasma-enhanced chemical vapor deposition method is used to deposit a silicon-oxygen co-doped amorphous carbon organic-inorganic composite coating on the PEEK surface. By optimizing the doping element content and deposition parameters, the bonding strength and toughness of the coating and the substrate are improved, and the internal stress is reduced. .

Benefits of technology

It significantly improves the anti-friction performance of the PEEK surface and the friction life of the material, enhances the film-based bonding force of the coating, reduces the occurrence of cracks, and improves the application potential of the material and the feasibility of industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115505157B_ABST
    Figure CN115505157B_ABST
Patent Text Reader

Abstract

The present invention discloses a use of an organic-inorganic composite wear-resistant and friction-reducing coating in the surface protection of polyetheretherketone. The organic-inorganic composite wear-resistant and friction-reducing coating is a silicon-oxygen co-doped amorphous carbon organic-inorganic composite coating deposited on the surface of polyetheretherketone, and the atomic percentage content of silicon in the organic-inorganic composite wear-resistant and friction-reducing coating is 3.0-8.0at.%, and the atomic percentage content of oxygen is 2.0-6.5at.%. The present invention modifies the amorphous carbon coating by silicon-oxygen co-doping, which not only improves the bonding force between the coating and the PEEK matrix, but also significantly improves the mechanical properties of the PEEK surface, prolongs the friction life, and enhances the lubricity; in addition, due to the introduction of silicon and oxygen elements into the amorphous carbon coating, the toughness of the coating is improved, and the generation of cracks is reduced, so that it also has great potential in anti-corrosion applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of surface protection, and in particular relates to application of an organic-inorganic composite wear-resistant and friction-reducing coating in the surface protection of polyetheretherketone. Background Art

[0002] Polyetheretherketone (PEEK) is a type of semi-crystalline special polymer material with excellent properties such as good corrosion resistance, self-lubrication, high heat resistance, high mechanical strength, hydrolysis resistance, and flame retardancy. It is widely used in the aerospace field, medical device field (as artificial bone to repair bone defects) and industrial field. In particular, PEEK, as one of the best choices for polymer materials in polymer-metal sliding friction pairs, has been widely used in many key friction systems such as high-pressure plunger pumps, marine hydraulic machinery, artificial joints, and aircraft landing gear pin joints. However, the unmodified PEEK material has a lower mechanical strength and thermal stability than metal materials, and its friction coefficient is as high as 0.4 under dry friction conditions. It is easily worn when rubbing against metal, which is not conducive to the long-term high-reliability and stable operation of the equipment system. Therefore, improving the friction performance of PEEK is the key to extending the service life of friction pairs and improving equipment performance.

[0003] The use of material surface modification technology can significantly improve the mechanical and tribological properties of the matrix without changing the excellent properties of the matrix itself. Amorphous carbon is between diamond and graphite. 2 Hybridization and sp 3 The amorphous coating material composed of hybrid bonds has both anti-wear and wear-reducing properties. At the same time, studies have confirmed that applying a layer of amorphous carbon coating on the surface of PEEK can significantly improve the friction performance and reduce the wear rate of the material.

[0004] However, due to the large differences in composition and properties between the PEEK matrix and the amorphous carbon coating, the interface matching between PEEK and amorphous carbon is poor. Direct deposition of amorphous carbon on the PEEK surface results in insufficient film-substrate bonding, which easily leads to coating failure behaviors such as cracking and peeling, which seriously restricts the practical application and promotion of amorphous carbon-modified PEEK. Summary of the invention

[0005] The main purpose of the present invention is to provide an organic-inorganic composite wear-resistant and friction-reducing coating for use in the surface protection of polyetheretherketone to overcome the shortcomings of the prior art.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0007] An embodiment of the present invention provides the use of an organic-inorganic composite wear-resistant and friction-reducing coating in the surface protection of polyetheretherketone. The organic-inorganic composite wear-resistant and friction-reducing coating is an organic-inorganic composite coating of silicon-oxygen co-doped amorphous carbon deposited on the surface of polyetheretherketone. The atomic percentage content of silicon in the organic-inorganic composite wear-resistant and friction-reducing coating is 3.0-8.0at.%, and the atomic percentage content of oxygen is 2.0-6.5at.%.

[0008] An embodiment of the present invention also provides an organic-inorganic composite wear-resistant and friction-reducing coating, which is an organic-inorganic composite coating of silicon-oxygen co-doped amorphous carbon deposited on the surface of polyetheretherketone, and the atomic percentage content of silicon in the organic-inorganic composite wear-resistant and friction-reducing coating is 3.0-8.0at.%, and the atomic percentage content of oxygen is 2.0-6.5at.%.

[0009] The embodiment of the present invention also provides a method for preparing the aforementioned organic-inorganic composite wear-resistant and friction-reducing coating, which comprises:

[0010] Cleaning and etching the surface of polyetheretherketone;

[0011] And, using a plasma enhanced chemical vapor deposition method, the polyetheretherketone obtained by etching treatment is placed in a reaction chamber, and carbon source gas and hexamethyldisiloxane are used as working gases, so as to deposit an organic-inorganic composite wear-resistant and friction-reducing coating on the surface of the polyetheretherketone; wherein the pulse negative bias voltage is 400-500V, the duty cycle is 55-65%, the deposition temperature is less than 30°C, the deposition time is 70.0-100.0min, and the gas pressure of the reaction chamber is 10-20mTorr.

[0012] Compared with the prior art, the present invention has the following beneficial effects:

[0013] (1) In the present invention, argon plasma is used to bombard the PEEK surface, which can clean and activate the PEEK surface, and can convert the carbon atoms on the PEEK surface into unsaturated carbon atoms, generating a large number of free radicals, thereby forming chemical bonds with the coating containing organic components, which is beneficial to improving the bonding strength of the coating on the substrate surface;

[0014] (2) The present invention optimizes the content of doping elements and regulates the interface between the coating and the substrate. The appropriate silicon-oxygen content can reduce the internal stress of the amorphous carbon coating and maintain appropriate mechanical properties, thereby improving the film-base bonding strength, reducing the generation of cracks during the friction process of the coating, improving the anti-friction performance of the PEEK surface, and increasing the potential for the material to be applied in other fields.

[0015] (3) The preparation process of the organic-inorganic composite wear-resistant and friction-reducing coating of the present invention is simple and the operating environment is safe: by controlling the flow ratio of acetylene and hexamethyldisiloxane, an amorphous carbon coating with different doping contents is achieved. The operation process is simple and easy to control, and it is easy to uniformly deposit over a large area, which is conducive to industrial production and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0017] Figure 1 The full XPS spectrum of the amorphous carbon coating and the silicon-oxygen co-doped amorphous carbon organic-inorganic composite coating provided in Example 1 of the present invention;

[0018] Figure 2 The bonding strength test diagram of the amorphous carbon coating and the silicon-oxygen co-doped amorphous carbon organic-inorganic composite coating modified PEEK provided in the specific embodiment of the present invention;

[0019] Figure 3 A graph showing the friction coefficient of PEEK modified by an amorphous carbon coating and a silicon-oxygen co-doped amorphous carbon organic-inorganic composite coating provided in a specific embodiment of the present invention;

[0020] Figure 4 1 is a polarization curve diagram of the amorphous carbon coating and the silicon-oxygen co-doped amorphous carbon organic-inorganic composite coating in Example 1 of the present invention. DETAILED DESCRIPTION

[0021] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Specifically, as one aspect of the technical solution of the present invention, the organic-inorganic composite wear-resistant and friction-reducing coating involved is used in the surface protection of polyetheretherketone. The organic-inorganic composite wear-resistant and friction-reducing coating is an organic-inorganic composite coating of silicon-oxygen co-doped amorphous carbon deposited on the surface of polyetheretherketone, and the atomic percentage content of silicon in the organic-inorganic composite wear-resistant and friction-reducing coating is 3.0-8.0at.%, and the atomic percentage content of oxygen is 2.0-6.5at.%.

[0023] In some preferred embodiments, the organic-inorganic composite wear-resistant and friction-reducing coating is prepared on the surface of polyetheretherketone by plasma enhanced chemical vapor deposition.

[0024] In some preferred embodiments, the method for preparing the organic-inorganic composite wear-resistant and friction-reducing coating comprises:

[0025] Cleaning and etching the surface of polyetheretherketone;

[0026] And, using a plasma enhanced chemical vapor deposition method, the polyetheretherketone obtained by etching treatment is placed in a reaction chamber, and carbon source gas and hexamethyldisiloxane are used as working gases, so as to deposit an organic-inorganic composite wear-resistant and friction-reducing coating on the surface of the polyetheretherketone; wherein the pulse negative bias voltage is 400-500V, the duty cycle is 55-65%, the deposition temperature is less than 30°C, the deposition time is 70.0-100.0min, and the gas pressure of the reaction chamber is 10-20mTorr.

[0027] Specifically, the present invention adopts a plasma enhanced chemical vapor deposition system, selects acetylene (C2H2) and hexamethyldisiloxane (HMDSO) as precursors, and forms a silicon-oxygen co-doped amorphous carbon organic-inorganic composite coating on the surface of the polymer matrix PEEK; the present invention adopts a plasma enhanced chemical vapor deposition system and optimizes the deposition process parameters, which can accurately control the content of silicon-oxygen co-doping, thereby ensuring a strong bond between the coating and the PEEK matrix and excellent wear resistance; the present invention modifies the amorphous carbon coating by silicon-oxygen co-doping, which not only improves the bonding force between the coating and the PEEK matrix, but also significantly improves the mechanical properties of the PEEK surface, extends the friction life, and enhances the lubricity; in addition, due to the introduction of silicon and oxygen elements into the amorphous carbon coating, the toughness of the coating is improved, the generation of cracks is reduced, and it also has great potential in corrosion resistance applications.

[0028] Furthermore, the carbon source gas has an inlet flow rate of 40-100 sccm, and the hexamethyldisiloxane has an inlet flow rate of 5-20 sccm.

[0029] Further, the carbon source gas includes acetylene, but is not limited thereto.

[0030] Furthermore, the process parameters of the etching treatment include: Ar flow rate of 50-150sccm, chamber pressure of 15-30mTorr, pulse negative bias voltage of 450-550V, and etching time of 5-15mi.

[0031] Furthermore, the organic-inorganic composite wear-resistant and friction-reducing coating has a thickness of 1.0-2.0 μm.

[0032] Another aspect of an embodiment of the present invention also provides an organic-inorganic composite wear-resistant and friction-reducing coating, which is an organic-inorganic composite coating of silicon-oxygen co-doped amorphous carbon deposited on the surface of polyetheretherketone, and the atomic percentage content of silicon in the organic-inorganic composite wear-resistant and friction-reducing coating is 3.0-8.0at.%, and the atomic percentage content of oxygen is 2.0-6.5at.%.

[0033] In some preferred embodiments, the organic-inorganic composite wear-resistant and friction-reducing coating has a thickness of 1.0-2.0 μm.

[0034] The silicon and oxygen contents in the present invention greatly affect the hardness, modulus and internal stress of the silicon-oxygen co-doped amorphous carbon organic-inorganic composite coating. If the silicon-oxygen co-doping content in the amorphous carbon coating is too low, the internal stress of the coating is not significantly reduced, and the bonding effect is weak. If the silicon-oxygen doping content is too high, the hardness and modulus of the coating are too low, the resistance to plastic deformation is weak, and the anti-friction performance is reduced. The appropriate amount of silicon-oxygen content can reduce the internal stress of the amorphous carbon coating and maintain a suitable mechanical property, thereby improving the film-base bonding and toughness, reducing the generation of cracks during the friction process of the coating, and improving the anti-friction and corrosion resistance of the PEEK surface.

[0035] In the present invention, the amorphous carbon coating is composed of sp 2 With sp 3 A type of material composed of hybrid bonds, with high hardness and high elastic modulus, and a friction coefficient as low as 0.03, is one of the preferred materials for precision matching protective coatings. However, when growing an amorphous carbon coating on the surface of a polymer material, the structural mismatch is serious due to the sudden change from the organic carbonaceous structure of the polymer to the inorganic carbonaceous structure of the amorphous carbon, and the internal stress of the amorphous carbon is large, which causes the interface of the two materials to be mismatched, resulting in insufficient bonding strength and failure. When plasma enhanced chemical vapor deposition is used, the organic precursor hexamethyldisiloxane is used to introduce silicon oxygen doping into the amorphous carbon. The silicon element introduced by this preparation method exists in the form of an organic silicon polymer. Before depositing the coating, the PEEK substrate is pretreated with argon plasma. While removing surface attachments, a large number of free radicals are generated on the PEEK surface. These free radicals combine with the chemical bonds in hexamethyldisiloxane, which can slow down the mutation of the interface between the PEEK polymer and the amorphous carbon, and significantly improve the bonding strength between the amorphous carbon coating and the PEEK substrate. Specifically, the silicon-oxygen co-doped amorphous carbon organic-inorganic composite coating is chemically bonded to the free radicals on the surface of PEEK to enhance the bonding strength of the membrane base; the hardness and modulus of the silicon-oxygen co-doped amorphous carbon organic-inorganic composite coating are between PEEK and amorphous carbon, which can achieve a gradient change in the overall mechanical properties of the coating; the silicon-oxygen co-doped amorphous carbon organic-inorganic composite coating has good toughness, which can reduce the generation of cracks in the coating during friction stress, and the coating also exhibits better corrosion resistance.

[0036] Another aspect of the embodiments of the present invention further provides a method for preparing the aforementioned organic-inorganic composite wear-resistant and friction-reducing coating, which comprises:

[0037] Cleaning and etching the surface of polyetheretherketone;

[0038] And, using a plasma enhanced chemical vapor deposition method, the polyetheretherketone obtained by etching treatment is placed in a reaction chamber, and carbon source gas and hexamethyldisiloxane are used as working gases, so as to deposit an organic-inorganic composite wear-resistant and friction-reducing coating on the surface of the polyetheretherketone; wherein the pulse negative bias voltage is 400-500V, the duty cycle is 55-65%, the deposition temperature is less than 30°C, the deposition time is 70.0-100.0min, and the gas pressure of the reaction chamber is 10-20mTorr.

[0039] In some preferred embodiments, the carbon source gas has an inlet flow rate of 40-100 sccm, and the hexamethyldisiloxane has an inlet flow rate of 5-20 sccm.

[0040] In some preferred embodiments, the carbon source gas includes acetylene, but is not limited thereto.

[0041] In some more specific embodiments, the method for preparing the organic-inorganic composite wear-resistant and friction-reducing coating comprises:

[0042] (1) placing a PEEK substrate in a vacuum chamber of a plasma enhanced chemical vapor deposition system, applying a pulsed negative bias voltage to the PEEK substrate, and simultaneously introducing argon gas to pre-treat the surface of the PEEK substrate, so as to generate free radicals on the surface of the PEEK.

[0043] (2) Turning off the bias voltage and argon gas, evacuating to the background vacuum, introducing acetylene and hexamethyldisiloxane, applying a pulsed negative bias voltage to the PEEK substrate, and depositing a strongly bonded silicon-oxygen co-doped amorphous carbon organic-inorganic composite wear-resistant and friction-reducing coating on the surface of the PEEK.

[0044] In step (1), the vacuum degree of the vacuum chamber is less than 2*10 -5 Torr.

[0045] In step (1), the pulse negative bias voltage is 450-550V, and the duty cycle is 55-65%.

[0046] In step (1), the argon gas flow rate is 100 sccm and the processing time is 10 min.

[0047] In step (2), the background vacuum is 2*10 -5 Torr.

[0048] In step (2), the gas flow rate of acetylene is 40-100 sccm, and the gas flow rate of hexamethyldisiloxane is 5-20 sccm.

[0049] In step (2), the PEEK substrate is applied with a pulsed negative bias voltage of 400-500 V, a duty cycle of 55-65%, and a deposition time of 70.0-100.0 min.

[0050] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.

[0051] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.

[0052] Example 1

[0053] The present invention provides a PEEK surface organic-inorganic composite wear-resistant and friction-reducing coating and a preparation method thereof, and the specific steps are as follows:

[0054] (1) First, use anhydrous ethanol to clean the PEEK substrate, and then place the cleaned and dried PEEK substrate in a vacuum chamber with a vacuum degree of less than 2*10 -5 In a vacuum chamber of 100 mTorr, first set the chamber pressure to 20 mTorr, and introduce 100 sccm of argon into the vacuum chamber; open the automatic flow control valve, wait for the chamber pressure to reach the set value of 20 mTorr, and then apply a -500 V pulse negative bias to the PEEK substrate with a duty cycle of 61.5% and an etching time of 10 min.

[0055] (2) Turn off the bias voltage and argon gas, and evacuate to 2*10 -5 Torr, introduce 40 sccm acetylene and 10 sccm hexamethyldisiloxane into the chamber at the same time, open the automatic flow control valve, wait for the chamber pressure to reach the set value of 15 mTorr, and then apply a -450 V pulse negative bias to the PEEK substrate with a duty cycle of 61.5% and a deposition time of 77.5 min.

[0056] Through the above steps, a wear-resistant coating with a thickness of 1.5 μm is obtained on the surface of the PEEK substrate. The atomic percentage of carbon in the coating is 86.4 at.%, the atomic percentage of silicon is 7.5 at.%, and the atomic percentage of oxygen is 6.1 at.%. The above coating has a black appearance, and the hardness and modulus are 6.3 GPa and 32.2 GPa respectively. The bonding force between PEEK and the coating is 7.8 N. Under the dry friction conditions of 3 N, 5 Hz, it is not worn out when grinding against a 304 stainless steel ball with a diameter of 6 mm for 30 minutes, and the friction coefficient is 0.13. Through the polarization curve test (such as Figure 4 It was found that the corrosion current density of silicon-oxygen co-doped amorphous carbon coating was two orders of magnitude lower than that of undoped amorphous carbon coating, and the corrosion potentials of the two coatings were close, indicating that silicon-oxygen doping improved the corrosion protection ability of amorphous carbon coating.

[0057] Example 2

[0058] (1) First, use anhydrous ethanol to clean the PEEK substrate, and then place the cleaned and dried PEEK substrate in a vacuum chamber with a vacuum degree of less than 2*10 -5 In a vacuum chamber of 100 mTorr, first set the chamber pressure to 20 mTorr, and introduce 100 sccm of argon into the vacuum chamber; open the automatic flow control valve, wait for the chamber pressure to reach the set value of 20 mTorr, and then apply a -500 V pulse negative bias to the PEEK substrate with a duty cycle of 61.5% and an etching time of 10 min.

[0059] (2) Turn off the bias voltage and argon gas, and evacuate to 2*10 -5 Torr, introduce 60 sccm acetylene and 10 sccm hexamethyldisiloxane into the chamber at the same time, open the automatic flow control valve, wait for the chamber pressure to reach the set value of 15 mTorr, and then apply a -450 V pulse negative bias to the PEEK substrate with a duty cycle of 61.5% and a deposition time of 84 min.

[0060] Through the above steps, a wear-resistant coating with a thickness of 1.5 μm is obtained on the surface of the PEEK substrate, wherein the atomic percentage of carbon element in the coating is 89.6 at.%, the atomic percentage of silicon element is 5.8 at.%, and the atomic percentage of oxygen element is 4.6 at.%. The above coating has a black appearance, and the hardness and modulus are 7.8 GPa and 35.1 GPa respectively. The bonding force between PEEK and the coating is 8.1 N. Under the dry friction conditions of 3 N and 5 Hz, the coating is not worn through when rubbed against a 304 stainless steel ball with a diameter of 6 mm for 30 minutes, and the friction coefficient is 0.15.

[0061] Example 3

[0062] (1) First, use anhydrous ethanol to clean the PEEK substrate, and then place the cleaned and dried PEEK substrate in a vacuum chamber with a vacuum degree of less than 2*10 -5 In a vacuum chamber of 100 mTorr, first set the chamber pressure to 20 mTorr, and introduce 100 sccm of argon into the vacuum chamber; open the automatic flow control valve, wait for the chamber pressure to reach the set value of 20 mTorr, and then apply a -500 V pulse negative bias to the PEEK substrate with a duty cycle of 61.5% and an etching time of 10 min.

[0063] (2) Turn off the bias voltage and argon gas, and evacuate to 2*10 -5 Torr, introduce 80 sccm acetylene and 10 sccm hexamethyldisiloxane into the chamber at the same time, open the automatic flow control valve, wait for the chamber pressure to reach the set value of 15 mTorr, and then apply a -450 V pulse negative bias to the PEEK substrate with a duty cycle of 61.5% and a deposition time of 88.7 min.

[0064] Through the above steps, a wear-resistant coating with a thickness of 1.5 μm is obtained on the surface of the PEEK substrate, wherein the atomic percentage of carbon element in the coating is 91.1 at.%, the atomic percentage of silicon element is 4.9 at.%, and the atomic percentage of oxygen element is 4.0 at.%. The above coating has a black appearance, and the hardness and modulus are 8.0 GPa and 36.7 GPa respectively. The bonding force between PEEK and the coating is 7.9 N. Under the conditions of 3 N, 5 Hz, and dry friction, the coating is not worn out when ground against a 304 stainless steel ball with a diameter of 6 mm for 30 minutes, and the friction coefficient is 0.14.

[0065] Example 4

[0066] (1) First, use anhydrous ethanol to clean the PEEK substrate, and then place the cleaned and dried PEEK substrate in a vacuum chamber with a vacuum degree of less than 2*10 -5 In a vacuum chamber of 100 mTorr, first set the chamber pressure to 20 mTorr, and introduce 100 sccm of argon into the vacuum chamber; open the automatic flow control valve, wait for the chamber pressure to reach the set value of 20 mTorr, and then apply a -500 V pulse negative bias to the PEEK substrate with a duty cycle of 61.5% and an etching time of 10 min.

[0067] (2) Turn off the bias voltage and argon gas, and evacuate to 2*10 -5 Torr, introduce 100 sccm acetylene and 10 sccm hexamethyldisiloxane into the chamber at the same time, open the automatic flow control valve, wait for the chamber pressure to reach the set value of 15 mTorr, and then apply a -450 V pulse negative bias to the PEEK substrate with a duty cycle of 61.5% and a deposition time of 90.5 min.

[0068] Through the above steps, a wear-resistant coating with a thickness of 1.5 μm was obtained on the surface of the PEEK substrate. The atomic percentage of carbon in the coating was 93.0 at.%, the atomic percentage of silicon was 4.0 at.%, and the atomic percentage of oxygen was 3.0 at.%. From the XPS spectrum of the doped coating, an N peak was observed at a binding energy of 400 eV. The N peak is related to the carbamate group of the organic silicon polymer, which indicates that the coating contains organic components, such as Figure 1 The coating has a black appearance, hardness and modulus are 8.3 GPa and 36.9 GPa respectively, the bonding force between PEEK and the coating is 4.8 N, and it is not worn through when grinding with a 6 mm diameter 304 stainless steel ball under dry friction conditions of 3 N and 5 Hz for 30 minutes, and the friction coefficient is 0.13.

[0069] Comparative Example 1

[0070] (1) First, use anhydrous ethanol to clean the PEEK substrate, and then place the cleaned and dried PEEK substrate in a vacuum chamber with a vacuum degree of less than 2*10 -5 In a vacuum chamber of 100 mTorr, first set the chamber pressure to 20 mTorr, and introduce 100 sccm of argon into the vacuum chamber; open the automatic flow control valve, wait for the chamber pressure to reach the set value of 20 mTorr, and then apply a -500 V pulse negative bias to the PEEK substrate with a duty cycle of 61.5% and an etching time of 10 min.

[0071] (2) Turn off the bias voltage and argon gas, and evacuate to 2*10 -5 Torr, introduce 100 sccm acetylene into the chamber, open the automatic flow control valve, wait for the chamber gas pressure to reach the set value of 15 mTorr, and then apply a -450 V pulse negative bias to the PEEK substrate with a duty cycle of 61.5% and a deposition time of 30 min.

[0072] Through the above steps, a wear-resistant coating with a thickness of 440 nm is obtained on the surface of the PEEK substrate, and the atomic percentage of carbon in the coating is 99.3 at.%, and the atomic percentage of oxygen is 0.7 at.%. The above coating has a black appearance, but the substrate is worn through when rubbing against 304 stainless steel with a diameter of 6 mm under dry friction conditions of 3N, 5 Hz, and 30 min, and the friction coefficient is 0.4. Compared with the thickness in the embodiment, the thickness of the amorphous carbon coating in the comparative example is less than 1 μm, which causes the substrate to be worn through due to insufficient bearing capacity in the friction test; on the other hand, the bonding force between PEEK and the coating in this example is too low, which is also one of the reasons for the premature wear of the substrate.

[0073] Comparative Example 2

[0074] (1) First, use anhydrous ethanol to clean the PEEK substrate, and then place the cleaned and dried PEEK substrate in a vacuum chamber with a vacuum degree of less than 2*10 -5 In a vacuum chamber of 100 mTorr, first set the chamber pressure to 20 mTorr, and introduce 100 sccm of argon into the vacuum chamber; open the automatic flow control valve, wait for the chamber pressure to reach the set value of 20 mTorr, and then apply a -500 V pulse negative bias to the PEEK substrate with a duty cycle of 61.5% and an etching time of 10 min.

[0075] (2) Turn off the bias voltage and argon gas, and evacuate to 2*10 -5 Torr, introduce 20 sccm acetylene and 10 sccm hexamethyldisiloxane into the chamber at the same time, open the automatic flow control valve, wait for the chamber pressure to reach the set value of 15 mTorr, and then apply a -450 V pulse negative bias to the PEEK substrate with a duty cycle of 61.5% and a deposition time of 68 min.

[0076] Through the above steps, a wear-resistant coating with a thickness of 1.5 μm is obtained on the surface of the PEEK substrate, in which the atomic percentage of carbon element is 79.8 at.%, the atomic percentage of silicon element is 10.0 at.%, and the atomic percentage of oxygen element is 10.9 at.%. The above coating has a black appearance and can protect the substrate from being worn through when rubbing against 304 stainless steel with a diameter of 6 mm under dry friction conditions of 3N, 5Hz, and 30min. The friction coefficient is 0.43, the hardness and modulus are 6.2GPa and 29.8GPa respectively, and the bonding force between PEEK and the coating is 6.0N.

[0077] The coating prepared in this comparative example was quickly worn through in the friction test and could not provide good protection for the substrate. This is mainly because the mechanical properties of the coating are inversely proportional to the doping content. When the doping content is too high, the mechanical properties of the coating are too low, making it easy to wear.

[0078] Comparative Example 3

[0079] (1) First, use anhydrous ethanol to clean the PEEK substrate, and then place the cleaned and dried PEEK substrate in a vacuum chamber with a vacuum degree of less than 2*10 -5 Torr's vacuum chamber.

[0080] (2) 40 sccm acetylene and 10 sccm hexamethyldisiloxane were introduced into the chamber at the same time, the automatic flow control valve was opened, and the chamber pressure was waited to reach the set value of 15 mTorr. Then, a -450 V pulse negative bias was applied to the PEEK substrate with a duty cycle of 61.5% and a deposition time of 77.5 min.

[0081] Through the above steps, a silicon-oxygen co-doped amorphous carbon coating with a thickness of 1.5 μm is obtained on the surface of the PEEK substrate, and the atomic percentage of carbon element in the coating is 86.4 at.%, the atomic percentage of silicon element is 7.5 at.%, and the atomic percentage of oxygen element is 6.1 at.%. The above coating has a black appearance, and the hardness and modulus are 6.3 GPa and 32.2 GPa respectively. The bonding force between PEEK and the coating is only 3.8N, which is more than twice lower than the sample in which silicon-oxygen co-doped amorphous carbon is deposited after etching the substrate surface. The main reason for the reduction in bonding force is that the PEEK substrate has not been treated with argon plasma etching, and its surface has not formed hanging bonds. The substrate and the coating are mainly bonded in the form of physical bonds, indicating that pretreatment of substrate etching is very important for improving the bonding force of the membrane substrate.

[0082] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0083] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.

Claims

1. Use of organic-inorganic composite wear-resistant and friction-reducing coating in polyetheretherketone surface protection, characterized by: The organic-inorganic composite wear-resistant and friction-reducing coating is an organic-inorganic composite coating of silicon-oxygen co-doped amorphous carbon deposited on the surface of polyetheretherketone, wherein the atomic percentage content of silicon in the organic-inorganic composite wear-resistant and friction-reducing coating is 4.9-8.0 at.%, and the atomic percentage content of oxygen is 4.6-6.5 at.%; the thickness of the organic-inorganic composite wear-resistant and friction-reducing coating is 1.0-2.0 μm; The preparation method of the organic-inorganic composite wear-resistant and friction-reducing coating comprises: The surface of the polyetheretherketone is cleaned and etched; wherein the etching process can convert carbon atoms on the surface of the polyetheretherketone into unsaturated carbon atoms and generate a large number of free radicals; the process parameters of the etching process include: Ar flow rate of 50-150sccm, chamber pressure of 15-30 mTorr, pulse negative bias of 450-550 V, and etching time of 5-15 min; In addition, a plasma enhanced chemical vapor deposition method is used to place the polyetheretherketone obtained by etching treatment in a reaction chamber, and carbon source gas and hexamethyldisiloxane are used as working gases, so as to deposit an organic-inorganic composite wear-resistant and friction-reducing coating on the surface of the polyetheretherketone; wherein the pulse negative bias voltage is 400-500V, the duty cycle is 55-65%, the deposition temperature is less than 30°C, the deposition time is 70.0-100.0 min, and the gas pressure of the reaction chamber is 10-20 mTorr.

2. The use according to claim 1, characterized in that: The carbon source gas has an inlet flow rate of 40-100 sccm, and the hexamethyldisiloxane has an inlet flow rate of 5-20 sccm.

3. The use according to claim 1, characterized in that: The flow ratio of hexamethyldisiloxane to carbon source gas is 1:10-1:

4.

4. The use according to claim 1, characterized in that: The carbon source gas is selected from acetylene.

Citation Information

Patent Citations

  • Amorphous-carbon-based thin film for polyether-ether-ketone surface protection as well as preparation method and application thereof

    CN111172512A

  • Aluminum alloy surface wear-resisting coating and preparation method and application thereof

    CN111286709A