A recyclable magnetic mesoporous antimicrobial peptide nanoparticle based on Fe-S bond and its preparation method and application
By using Fe-S bond to fix antibacterial peptides on the surface of magnetic mesoporous nanoparticles, the problems of high production cost and insufficient immobilization stability are solved, and high-efficiency and low-cost antibacterial performance and multiple cycles are achieved. It is suitable for Fight against bacterial resistance.
Patent Information
- Application Number
- CN202211241704.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-11
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-10-11
AI Technical Summary
The existing production methods of antimicrobial peptides are expensive and difficult to achieve industrial production. The immobilization stability and separation operation of antimicrobial peptides are insufficient, making it difficult to effectively solve the problem of bacterial resistance.
By constructing a mesoporous structure on the surface of the magnetic mesoporous nanoparticles Fe3O4@mSiO2, using Fe-S bonds to fix the antimicrobial peptides in the pores, the stability of antimicrobial properties and multiple cycles are achieved, and simple magnetic separation is performed through superparamagnetic Recycle.
It realizes efficient utilization of antimicrobial peptides, reduces application costs, and maintains good antimicrobial performance. It can bactericidal rate of E. coli and Staphylococcus aureus is greater than 99.9%, and the antimicrobial peptides can be circulated more than 9 times.
Smart Images

Figure CN115531516B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of antibacterial technology, in particular to recyclable magnetic mesoporous antibacterial peptide nanoparticles constructed based on Fe-S bonds, and a preparation method and application thereof. Background Art
[0002] Nano-Fe3O4 is a widely used magnetic nanomaterial due to its size surface effect, small size effect and unique superparamagnetism. It has attracted much attention in the field of biomedical materials, especially because of its good biocompatibility. However, due to the large surface energy, magnetic nanoparticles are easily aggregated, thus losing the excellent properties of magnetic nanoparticles. The construction of shell-core structure is a common method to prevent nanoparticle aggregation. Among the many shell structures, the construction of a shell with mesoporous materials has a great promoting effect on the functionalization of materials. Mesoporous materials have the characteristics of extremely high specific surface area, highly ordered pore structure, narrow pore size distribution, and continuously adjustable pore size. Combining mesoporous materials with magnetic materials to construct a magnetic mesoporous composite material not only gives the material the advantages of mesoporous materials, but also can be simply recycled and reused through magnetic separation, providing a new strategy for the efficient and green application of functional materials.
[0003] In recent years, the rapid development of various antimicrobial drugs has enabled the prevention, control and treatment of many diseases caused by bacterial infections. However, while reducing the mortality rate due to bacterial infections, many strains have produced drug-resistant genes through mutation. Therefore, solving the problem of bacterial resistance is a huge threat and challenge faced by people. Peptides have broad-spectrum antibacterial activity and have a strong killing effect on bacteria. Some antimicrobial peptides not only have a killing effect on some viruses, fungi, protozoa and cancer cells, but can even improve immunity and accelerate the wound healing process. However, there are currently three main ways to produce antimicrobial peptides: natural extraction, chemical synthesis and bioengineering fermentation. Natural antimicrobial peptides mainly come from animals and plants, with extremely low content and very complicated extraction process; chemical synthesis methods are costly and not suitable for industrial production, so they cannot be popularized. Immobilization technology provides an effective way to improve the recycling of antimicrobial agents. After searching the prior art, it was found that most of the prior art uses small molecules of antimicrobial peptides or immobilizes them on carriers such as chitosan for enzyme calibration. However, the stability of functional group immobilization and the cheapness of separation operations still face great challenges. Summary of the invention
[0004] In view of the shortcomings of the prior art, the first object of the present invention is to provide a method for preparing recyclable magnetic mesoporous antimicrobial peptide nanoparticles based on Fe-S bonds. By utilizing the mesoporous structure on the surface of magnetic nanomaterials, the antimicrobial peptide is fixed in the pores of the mesoporous material through Fe-S bonds, thereby preparing an antimicrobial peptide with stable antimicrobial properties and capable of being recycled multiple times. At the same time, based on the superparamagnetism of Fe3O4, it can be recovered by a simple magnetic separation method, thereby improving the utilization efficiency of the antimicrobial peptide and reducing its application cost.
[0005] The specific technical solution of this method is as follows:
[0006] Step (1), preparation of magnetic mesoporous surface nanoparticles Fe3O4@mSiO2
[0007] Hexadecyltrimethylammonium bromide and ferroferric oxide nanoparticles in a mass ratio of 5 to 10:1 are placed in deionized water, ultrasonically mixed, sodium hydroxide solution is added, mechanically stirred at 50 to 60°C, and then a mixed solvent is added to react for 10 to 13 hours; after the reaction, the magnetic substance is separated, washed with deionized water and ethanol, vacuum dried at 40 to 50°C for 10 to 12 hours to remove the solvent, placed in a nitrogen protective atmosphere, and calcined at 300 to 350°C to obtain magnetic mesoporous surface nanoparticles Fe3O4@mSiO2 with a shell-core structure of mesoporous silica-coated magnetic ferroferric oxide;
[0008] The mixed solvent is a mixed solution of ethyl orthosilicate and methanol;
[0009] Step (2), preparation of recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10 based on Fe-S bonds
[0010] The magnetic mesoporous surface nanoparticles Fe3O4@mSiO2 and antimicrobial peptides with a mass ratio of 1 to 1.5:1 were added to PBS buffer and stirred at room temperature for 10 to 15 hours; the magnetic substance was separated and washed with deionized water, and the solvent was removed by freeze drying to obtain recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10 constructed based on Fe-S bonds;
[0011] The antibacterial polypeptide is a CysCHHC10 polypeptide containing a thiol group at the end.
[0012] The structural formula of the CysCHHC10 peptide containing a thiol group at the end is as follows:
[0013]
[0014] Preferably, in step (1), the mass ratio of hexadecyltrimethylammonium bromide to ferrosoferric oxide nanoparticles is 10:1.
[0015] Preferably, the temperature of mechanical stirring in step (1) is 60°C.
[0016] Preferably, the volume ratio of ethyl orthosilicate to methanol in the mixed solvent in step (1) is 1:2-4.
[0017] Preferably, the vacuum drying temperature in step (1) is 50° C. and the vacuum drying time is 12 h.
[0018] Preferably, the calcination temperature in step (1) is 350°C.
[0019] Preferably, in step (2), the mass ratio of Fe3O4@mSiO2 to the antibacterial polypeptide is 1:1.
[0020] The specific surface area of the mesoporous magnetic nanoparticle material prepared in step (1) is 205.3 cm 2 / g, the total void volume is 0.2641cm 3 / g, with an average pore size of 24.22nm; the loading rate of the nanoparticles of recyclable antibacterial polypeptides constructed based on Fe-S bonds prepared in step (2) reaches 44%.
[0021] The second object of the present invention is to provide recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10 based on Fe-S bonds prepared by the above method.
[0022] The third object of the present invention is to provide the use of the above-mentioned recyclable magnetic mesoporous antimicrobial peptide nanoparticles constructed based on Fe-S bonds as antimicrobial agents.
[0023] Preferably, the bacteria targeted by the antibacterial agent include Escherichia coli and Staphylococcus aureus.
[0024] The minimum inhibitory concentration of the magnetic mesoporous antimicrobial peptide nanoparticles to Escherichia coli is 0.05 mg / ml, and the bactericidal rate is greater than 99.9%; the minimum inhibitory concentration to Staphylococcus aureus is 0.068 mg / ml, and the bactericidal rate is greater than 99.9%.
[0025] According to tests, the antibacterial performance of the magnetic mesoporous antimicrobial peptide nanoparticles prepared by the present invention on Escherichia coli and Staphylococcus aureus can be recycled for 9 times, and the sterilization rate is still greater than 99.9%.
[0026] In summary, compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The recyclable magnetic mesoporous antimicrobial peptide nanoparticles provided by the present invention construct a mesoporous structure on the surface of magnetic Fe3O4 nanoparticles, and use the thiol (-SH) functional group contained in the antimicrobial peptide and Fe3O4 in the mesoporous channels to form Fe-S bonds to stably load the antimicrobial peptide on the nanoparticles. Due to the bonding effect of the Fe-S bonds and the protection of the mesoporous channels for the peptide, the clustering of the nanoparticles is effectively prevented, so that the nanoparticles have good antimicrobial properties while increasing the stability of the load, thereby achieving the purpose of multiple recycling and reuse.
[0028] 2. The magnetic nanoparticle material provided by the present invention still has good superparamagnetism before and after loading, so after sterilization, the magnetic mesoporous antimicrobial peptide nanoparticles can be separated and recovered as a whole for recycling through a simple magnetic separation operation.
[0029] 3. The antimicrobial polypeptide provided by the present invention is a broad-spectrum antimicrobial agent that can effectively avoid drug resistance. At the same time, since the ferrosoferric oxide nanoparticles and the antimicrobial polypeptide provided by the present invention have good biocompatibility, it provides the possibility for in vivo detection. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 SEM photos and particle size distribution curves of the magnetic mesoporous surface nanoparticles Fe3O4@mSiO2 and recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10 prepared in Example 1, wherein a) is the magnetic mesoporous surface nanoparticles Fe3O4@mSiO2, b) is the recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10 after loading with antimicrobial peptides, c) is the result after b) is enlarged, and d) is the particle size distribution curve of c).
[0031] Figure 2 TEM images of the magnetic mesoporous surface nanoparticles Fe3O4@mSiO2 and the recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10 prepared in Example 1, wherein a) is the magnetic mesoporous surface nanoparticles Fe3O4@mSiO2, b) is the result after a) is enlarged, c) is the recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10 after loading with antimicrobial peptides, and d) is the result after c) is enlarged.
[0032] Figure 3 IR spectra of Fe3O4, Fe3O4@mSiO2, Fe3O4@mSiO2@CysCHHC10 and CysCHHC10 in Example 1.
[0033] Figure 4These are the XRD spectra of Fe3O4, Fe3O4@mSiO2 and Fe3O4@mSiO2@CysCHHC10 in Example 1.
[0034] Figure 5 VSM spectra and magnet adsorption separation images of Fe3O4, Fe3O4@mSiO2 and Fe3O4@mSiO2@CysCHHC10 in Example 1.
[0035] Figure 6 This is the BET spectrum of the magnetic mesoporous surface nanoparticles Fe3O4@mSiO2 prepared in Example 1.
[0036] Figure 7 This is the XPS energy spectrum of the magnetic mesoporous surface nanoparticles Fe3O4@mSiO2 prepared in Example 1 before and after loading the antibacterial polypeptide.
[0037] Figure 8 This is a locally enlarged XPS spectrum of the magnetic mesoporous surface nanoparticles Fe3O4@mSiO2 and magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10 prepared in Example 1.
[0038] Fig. 9 The minimum inhibitory concentration of the recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10 prepared in Example 1 for Escherichia coli and Staphylococcus aureus.
[0039] Fig.10 The bactericidal cycle performance of the recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10 prepared in Example 1 against Escherichia coli and Staphylococcus aureus. DETAILED DESCRIPTION
[0040] The present invention is further described in detail below in conjunction with specific embodiments. This embodiment is implemented on the premise of the technical solution of the present invention, and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to the following embodiments.
[0041] Example 1
[0042] (1) Preparation of magnetic mesoporous surface nanoparticles Fe3O4@mSiO2
[0043] 500 mg of CTAB (hexadecyltrimethylammonium bromide) was dissolved in 50 mL of deionized water, and then 50 mg of Fe3O4 nanoparticles were added to the mixed solution and ultrasonicated for 30 min.
[0044] 50 mL of 10 mM NaOH and 400 mL of deionized water were added, mechanically stirred at 60° C. for 30 min, and then 2.5 mL of ethyl orthosilicate / methanol (v / v=1:4) was added.
[0045] The synthesized solution was mechanically stirred and heated at 60°C, reacted for 12 hours, separated by a magnet, washed three times with deionized water and ethanol in sequence, vacuum dried at 50°C for 12 hours, and calcined at 350°C for 4 hours to obtain Fe3O4@mSiO2.
[0046] (2) Preparation of recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10
[0047] 15 mg of Fe3O4@mSiO2 was added to 25 mL of PBS buffer containing 15 mg of polypeptide CysCHHC10, stirred at 25°C for 12 h, then washed 6 times with deionized water and freeze-dried to obtain the product.
[0048] The magnetic mesoporous surface nanoparticles Fe3O4@mSiO2 and the recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10 were observed under SEM scanning electron microscope and TEM transmission electron microscope, respectively, and analyzed by IR spectrum, XRD spectrum, VSM, BET method and XPS spectrum. The results are as follows: Figures 1 to 8 shown.
[0049] Using Escherichia coli and Staphylococcus aureus as experimental bacteria, the minimum inhibitory concentration and bactericidal cycle performance of recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10 were tested. Figures 9-10 shown.
[0050] Example 2
[0051] (1) Preparation of magnetic mesoporous surface nanoparticles Fe3O4@mSiO2
[0052] 250 mg of CTAB (hexadecyltrimethylammonium bromide) was dissolved in 50 mL of deionized water, and then 50 mg of Fe3O4 nanoparticles were added to the mixed solution and ultrasonicated for 30 min.
[0053] 50 mL of 10 mM NaOH and 400 mL of deionized water were added, mechanically stirred at 60° C. for 30 min, and then 2.5 mL of ethyl orthosilicate / methanol (v / v=1:4) was added.
[0054] The synthesized solution was mechanically stirred and heated at 60°C, reacted for 12 hours, separated by a magnet, washed three times with deionized water and ethanol in sequence, vacuum dried at 50°C for 12 hours, and calcined at 350°C for 4 hours to obtain Fe3O4@mSiO2.
[0055] (2) Preparation of recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10
[0056] 15 mg of Fe3O4@mSiO2 was added to 25 mL of PBS buffer containing 15 mg of polypeptide CysCHHC10, stirred at 25°C for 12 h, then washed 6 times with deionized water and freeze-dried to obtain the product.
[0057] Example 3
[0058] (1) Preparation of magnetic mesoporous surface nanoparticles Fe3O4@mSiO2
[0059] 500 mg of CTAB (hexadecyltrimethylammonium bromide) was dissolved in 50 mL of deionized water, and then 50 mg of Fe3O4 nanoparticles were added to the mixed solution and ultrasonicated for 30 min.
[0060] 50 mL of 10 mM NaOH and 400 mL of deionized water were added, mechanically stirred at 50° C. for 30 min, and then 2.5 mL of ethyl orthosilicate / methanol (v / v=1:4) was added.
[0061] The synthesized solution was mechanically stirred and heated at 60°C, reacted for 12 hours, separated by a magnet, washed three times with deionized water and ethanol in sequence, vacuum dried at 50°C for 12 hours, and calcined at 350°C for 4 hours to obtain Fe3O4@mSiO2.
[0062] (2) Preparation of recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10
[0063] 15 mg of Fe3O4@mSiO2 was added to 25 mL of PBS buffer containing 15 mg of polypeptide CysCHHC10, stirred at 25°C for 12 h, then washed 6 times with deionized water and freeze-dried to obtain the product.
[0064] Example 4
[0065] (1) Preparation of magnetic mesoporous surface nanoparticles Fe3O4@mSiO2
[0066] 500 mg of CTAB (hexadecyltrimethylammonium bromide) was dissolved in 50 mL of deionized water, and then 50 mg of Fe3O4 nanoparticles were added to the mixed solution and ultrasonicated for 30 min.
[0067] 50 mL of 10 mM NaOH and 400 mL of deionized water were added, mechanically stirred at 60° C. for 30 min, and then 2.5 mL of ethyl orthosilicate / methanol (v / v=1:2) was added.
[0068] The synthesized solution was mechanically stirred and heated at 60°C, reacted for 12 hours, separated by a magnet, washed three times with deionized water and ethanol in sequence, vacuum dried at 50°C for 12 hours, and calcined at 350°C for 4 hours to obtain Fe3O4@mSiO2.
[0069] (2) Preparation of recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10
[0070] 15 mg of Fe3O4@mSiO2 was added to 25 mL of PBS buffer containing 15 mg of polypeptide CysCHHC10, stirred at 25°C for 12 h, then washed 6 times with deionized water and freeze-dried to obtain the product.
[0071] Example 5
[0072] (1) Preparation of magnetic mesoporous surface nanoparticles Fe3O4@mSiO2
[0073] 500 mg of CTAB (hexadecyltrimethylammonium bromide) was dissolved in 50 mL of deionized water, and then 50 mg of Fe3O4 nanoparticles were added to the mixed solution and ultrasonicated for 30 min.
[0074] 50 mL of 10 mM NaOH and 400 mL of deionized water were added, mechanically stirred at 60° C. for 30 min, and then 2.5 mL of ethyl orthosilicate / methanol (v / v=1:4) was added.
[0075] The synthesized solution was mechanically stirred and heated at 60°C, reacted for 12 hours, separated by a magnet, washed three times with deionized water and ethanol in sequence, vacuum dried at 40°C for 10 hours, and calcined at 350°C for 4 hours to obtain Fe3O4@mSiO2.
[0076] (2) Preparation of recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10
[0077] 15 mg of Fe3O4@mSiO2 was added to 25 mL of PBS buffer containing 15 mg of polypeptide CysCHHC10, stirred at 25°C for 12 h, then washed 6 times with deionized water and freeze-dried to obtain the product.
[0078] Example 6
[0079] (1) Preparation of magnetic mesoporous surface nanoparticles Fe3O4@mSiO2
[0080] 500 mg of CTAB (hexadecyltrimethylammonium bromide) was dissolved in 50 mL of deionized water, and then 50 mg of Fe3O4 nanoparticles were added to the mixed solution and ultrasonicated for 30 min.
[0081] 50 mL of 10 mM NaOH and 400 mL of deionized water were added, mechanically stirred at 60° C. for 30 min, and then 2.5 mL of ethyl orthosilicate / methanol (v / v=1:4) was added.
[0082] The synthesized solution was mechanically stirred and heated at 60°C, reacted for 12 hours, separated by a magnet, washed three times with deionized water and ethanol in sequence, vacuum dried at 50°C for 12 hours, and calcined at 300°C for 4 hours to obtain Fe3O4@mSiO2.
[0083] (2) Preparation of recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10
[0084] 15 mg of Fe3O4@mSiO2 was added to 25 mL of PBS buffer containing 15 mg of polypeptide CysCHHC10, stirred at 25°C for 12 h, then washed 6 times with deionized water and freeze-dried to obtain the product.
[0085] Example 7
[0086] (1) Preparation of magnetic mesoporous surface nanoparticles Fe3O4@mSiO2
[0087] 500 mg of CTAB (hexadecyltrimethylammonium bromide) was dissolved in 50 mL of deionized water, and then 50 mg of Fe3O4 nanoparticles were added to the mixed solution and ultrasonicated for 30 min.
[0088] 50 mL of 10 mM NaOH and 400 mL of deionized water were added, mechanically stirred at 60° C. for 30 min, and then 2.5 mL of ethyl orthosilicate / methanol (v / v=1:4) was added.
[0089] The synthesized solution was mechanically stirred and heated at 60°C, reacted for 12 hours, separated by a magnet, washed three times with deionized water and ethanol in sequence, vacuum dried at 50°C for 12 hours, and calcined at 350°C for 4 hours to obtain Fe3O4@mSiO2.
[0090] (2) Preparation of recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@mSiO2@CysCHHC10
[0091] 15 mg Fe3O4@mSiO2 was added to 25 mL PBS buffer containing 10 mg polypeptide CysCHHC10, stirred at 25°C for 12 h, then washed 6 times with deionized water and freeze-dried to obtain the product.
[0092] Comparative Example 1
[0093] The ferrosoferric oxide nanoparticles in Example 1 were replaced with non-magnetic silicon dioxide nanoparticles, and the remaining conditions were the same as in Example 1, to prepare comparative nanoparticles 1.
[0094] Comparative Example 2
[0095] The mesoporous structure of silicon dioxide formed on the surface of ferroferric oxide in Example 1 was replaced with a core-shell structure of ferroferric oxide wrapped by silicon dioxide, and the other conditions were the same as those in Example 1, to prepare comparative nanoparticles 2.
[0096] Comparative Example 3
[0097] Comparative nanoparticles 3 were prepared according to the method of Example 1, except that the comparative nanoparticles 3 did not form a mesoporous structure of silicon dioxide on the surface of ferrosoferric oxide, but only directly loaded the polypeptide on the surface of ferrosoferric oxide.
[0098] Comparative Example 4
[0099] The antibacterial and recycling properties of single ferroferric oxide were tested directly.
[0100] Comparative Example 5
[0101] The single antibacterial peptide CysCHHC10 was directly used to test its antibacterial and recycling properties.
[0102] Test Case
[0103] The antibacterial rate in this test example was measured according to GB / T 21510-2008 “Test Method for Antibacterial Performance of Nano-inorganic Materials”, where the experimental bacteria were Escherichia coli CICC 10899 and Staphylococcus aureus CICC 10384.
[0104] The antibacterial and recycling performance are shown in Table 1.
[0105] Table 1 Antibacterial and recycling performance results of Examples 1-7 and Comparative Examples 1-5
[0106]
[0107]
[0108] Note: -- means no antibacterial properties
[0109] According to the data in Table 1, the magnetic nanoparticle antibacterial agent provided by the present invention has high antibacterial performance and recovery performance. At the same time, after comparing Example 1 with Comparative Examples 1-5, it can be found that the magnetic nanoparticles with a mesoporous structure constructed based on the Fe-S bond improve the stability of the load and increase the circulation capacity on the one hand, and avoid clustering between nanoparticles on the other hand, ensuring the performance of the nanoparticles. Without using the mesoporous structure of silicon dioxide formed on the surface of ferroferric oxide, Fe-S bonds cannot be formed, and antibacterial polypeptides cannot be loaded. The antibacterial rate and minimum antibacterial concentration of the core-shell structure are lower than those in Example 1, and the number of cycles is also less.
Claims
1. A method for preparing recyclable magnetic mesoporous antimicrobial peptide nanoparticles based on Fe-S bonds, characterized in that: The preparation method comprises the following steps: Step (1), preparation of magnetic mesoporous surface nanoparticles Fe3O4@ m SiO2 Hexadecyltrimethylammonium bromide and ferroferric oxide nanoparticles in a mass ratio of 5-10:1 are placed in deionized water, ultrasonically mixed, sodium hydroxide solution is added, mechanically stirred at 50-60°C, and then a mixed solvent is added to react for 10-13 hours; after the reaction, the magnetic material is separated, washed with deionized water and ethanol, vacuum dried at 40-50°C for 10-12 hours to remove the solvent, placed in a nitrogen protective atmosphere, and calcined at 300-350°C to obtain magnetic mesoporous surface nanoparticles Fe3O4@ with a shell-core structure of mesoporous silica-coated magnetic ferroferric oxide m SiO2; The mixed solvent is a mixture of ethyl orthosilicate and methanol, wherein the volume ratio of ethyl orthosilicate to methanol is 1:2-4; Step (2), preparation of recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@ based on Fe-S bonds m SiO2@CysHHC10 The magnetic mesoporous surface nanoparticles Fe3O4@ m SiO2 and antimicrobial peptides were added to PBS buffer and stirred at room temperature for 10-15 hours. The magnetic material was separated and washed with deionized water. After lyophilization to remove the solvent, recyclable magnetic mesoporous antimicrobial peptide nanoparticles Fe3O4@ were obtained based on Fe-S bonds. m SiO2@CysHHC10; The antibacterial polypeptide is a CysHHC10 polypeptide containing a thiol group at the end.
2. The method for preparing recyclable magnetic mesoporous antimicrobial peptide nanoparticles based on Fe-S bonds according to claim 1, characterized in that: In step (1), the mass ratio of hexadecyltrimethylammonium bromide to ferrosoferric oxide nanoparticles is 10:
1.
3. The method for preparing recyclable magnetic mesoporous antimicrobial peptide nanoparticles based on Fe-S bonds according to claim 1, characterized in that: The temperature of mechanical stirring in step (1) is 60°C.
4. The method for preparing recyclable magnetic mesoporous antimicrobial peptide nanoparticles based on Fe-S bonds according to claim 1, characterized in that: The vacuum drying temperature in step (1) is 50° C. and the vacuum drying time is 12 h.
5. The method for preparing recyclable magnetic mesoporous antimicrobial peptide nanoparticles based on Fe-S bonds according to claim 1, characterized in that: The calcination temperature in step (1) is 350°C.
6. The method for preparing recyclable magnetic mesoporous antimicrobial peptide nanoparticles based on Fe-S bonds according to claim 1, characterized in that: In step (2), Fe3O4@ m The mass ratio of SiO2 and antimicrobial peptide is 1:
1.
7. A recyclable magnetic mesoporous antimicrobial peptide nanoparticle constructed based on Fe-S bonds, prepared by the method according to any one of claims 1 to 6.
8. Use of the recyclable magnetic mesoporous antimicrobial peptide nanoparticles constructed based on Fe-S bonds as claimed in claim 7 in the preparation of antibacterial agents.
9. The use according to claim 8, characterized in that: Bacteria targeted by antimicrobials include Escherichia coli and Staphylococcus aureus.