A responsive pattern based on surface plasmon, preparation method and application thereof

By grafting modification and self-assembly of inorganic nanoparticles, combined with plasma etching and oxidative polymerization, a polyaniline shell is formed, which solves the problems of complex preparation of single-layer films of inorganic nanoparticles and uncontrollable color, and achieves responsiveness. Reversible changes in pattern and simplified preparation process are suitable for a variety of applications.

CN115561846BActive Publication Date: 2024-10-18HUAZHONG UNIV OF SCI & TECH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211184731.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-27
Publication Date
2024-10-18
Estimated Expiration
2042-09-27

AI Technical Summary

Technical Problem

In the existing technology, the preparation process of a single layer of inorganic nanoparticles is complicated, and the color cannot be dynamically controlled, which limits its wide application.

Method used

Inorganic nanoparticles are grafted and modified with functional group-terminated polymers, self-assembled to form a single-layer film, and plasma etching and oxidative polymerization are used to form a polyaniline shell to achieve surface plasmon responsiveness. Patterning.

Benefits of technology

It achieves reversible changes in pattern color, simplifies the preparation process, and has a wide range of applications, such as anti-counterfeiting, sensing, and information storage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115561846B_ABST
    Figure CN115561846B_ABST
Patent Text Reader

Abstract

The present invention discloses a responsive pattern based on surface plasmon, a preparation method and its application. The preparation method comprises the following steps: subjecting a dispersion of polymer-grafted inorganic nanoparticles to self-assembly to obtain a polymer-grafted inorganic nanoparticle monolayer film, and transferring the monolayer film to the surface of a substrate; patterning the monolayer film, and removing the polymer grafted on the surface of the inorganic nanoparticles on the monolayer film in the etched area; immersing the etched substrate in a solution containing aniline, so that the aniline undergoes an oxidative polymerization reaction on the surface of the inorganic nanoparticles in the etched area to form a polyaniline shell layer, and obtains a responsive pattern based on surface plasmon. The present invention combines the surface plasmon effect with a responsive medium, and solves the technical problems of the existing patterning technology, such as the complex process and the inability to dynamically control the color.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of polymer / inorganic nanocomposite materials, and more specifically, relates to a responsive pattern based on surface plasmon, a preparation method and application thereof. Background Art

[0002] Orderly arranged monolayer films of inorganic nanoparticles usually have unique optical properties, which is due to the local electric field generated by the surface plasmon resonance effect of the nanoparticles, which can effectively enhance the absorption of incident light. The surface plasmon resonance effect mainly depends on the properties of the inorganic nanoparticles themselves and their medium.

[0003] The local surface plasmon resonance effect of inorganic nanoparticles will change with the shape, size, and arrangement of the nanoparticles. For example, the surface plasmon resonance effect of a gold nanoparticle monolayer film will increase as the interparticle distance decreases, and its UV-visible light absorption characteristic peak will red-shift. However, the surface plasmon resonance effect of a monolayer film is often predetermined by its composition, making it difficult to give an inorganic nanoparticle monolayer film a reversible color change, thus limiting its wide application.

[0004] To achieve reversible pattern color change, one effective approach is to combine the plasmon resonance effect of inorganic nanoparticles with external stimulus-responsive media.

[0005] For example, the method used in the prior art is: a layer of SU-8 photoresist is coated on a silicon substrate, the coated substrate is covered with a photomask having a pattern and irradiated with ultraviolet light, the SU-8 exposed to ultraviolet light is cross-linked by polymerization to form a microstructure pattern on the substrate, the SU-8 not irradiated with ultraviolet light is removed, the patterned substrate is silanized and used to mold PDMS, and finally the molded PDMS film is transferred to an ITO substrate pre-deposited with a layer of metal nanoparticles, and then peeled off. However, the preparation process of this method is cumbersome, and the arrangement of nanoparticles does not have a long-range ordered arrangement structure through deposition, which affects the large-scale production and practical application of the preparation of plasma inorganic nanoparticle responsive patterns. Therefore, it is of great significance to develop a simple preparation method of responsive patterns based on surface plasmons. Summary of the invention

[0006] In view of the above defects or improvement needs of the prior art, the present invention provides a responsive pattern based on surface plasmon, a preparation method and its application, and its purpose is to provide a new preparation method that combines the surface plasmon effect with the responsive medium, thereby solving the technical problems of the existing patterning technology, such as the complex process and the inability to dynamically control the color.

[0007] To achieve the above object, according to one aspect of the present invention, a method for preparing a responsive pattern based on surface plasmon is provided, comprising the following steps:

[0008] (1) grafting inorganic nanoparticles with a functional group-terminated polymer by a ligand exchange method, and dispersing the polymer-grafted inorganic nanoparticles in a solvent to obtain a dispersion of the polymer-grafted inorganic nanoparticles; the dispersion undergoes self-assembly to obtain a monolayer film of the polymer-grafted inorganic nanoparticles, and the monolayer film is transferred to a substrate surface;

[0009] (2) pattern-etching the single-layer film, and removing the polymer grafted on the surface of the inorganic nanoparticles on the single-layer film in the etched area;

[0010] (3) Immersing the etched substrate in a solution containing aniline to cause aniline to undergo an oxidative polymerization reaction on the surface of the inorganic nanoparticles in the etched area to form a polyaniline shell layer, and the surface plasmon-based responsive pattern is formed by the inorganic nanoparticle monolayer film in the etched area and the polyaniline shell layer formed on the surface thereof.

[0011] Preferably, the patterned etching in step (2) is performed using plasma etching technology; the excitation gas used in the plasma etching technology is at least one of air, argon, helium, and nitrogen, the etching time is 1-5 minutes, and the etching power is 1-20W.

[0012] Preferably, the inorganic nanoparticles in step (1) are quantum dots, inorganic metal nanoparticles or metal oxide nanoparticles, and the size of the inorganic nanoparticles is 3.5-100 nm; the distance between the inorganic nanoparticles in the polymer-grafted inorganic nanoparticle monolayer film is 1-40 nm; preferably, the inorganic metal nanoparticles are gold nanoparticles or silver nanoparticles, the metal oxide nanoparticles are ferroferric oxide nanoparticles or zinc dioxide nanoparticles, and the quantum dots are cadmium selenide quantum dots or zinc sulfide quantum dots.

[0013] Preferably, the polymer is an oil-soluble polymer, preferably, the oil-soluble polymer is one of polystyrene, polyethylene, polymethyl methacrylate and poly(4-vinylpyridine), the molecular weight of the polymer is 2000-50000 g / mol, and the functional group is a group containing a thiol group, a disulfide bond or a thioester bond.

[0014] Preferably, the self-assembly includes an oil / water interface assembly method, a LB film assembly method, a solvent evaporation assembly method, a Czochralski assembly method or an inkjet printing method.

[0015] Preferably, the solution containing aniline further comprises an oxidant and a surfactant, and the concentration of aniline in the solution containing aniline is 1-6 mM; preferably, the oxidant is one of ammonium persulfate, hydrogen peroxide, and ferric chloride, and the surfactant is one of sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, and sodium dodecylbenzenesulfonate, the time of the oxidative polymerization reaction is 1-24 h, and the pH value of the oxidative polymerization reaction is 0.5-7; the thickness of the polyaniline shell layer formed on the surface of the inorganic nanoparticles is regulated by changing the aniline concentration in the solution containing aniline and the time of the oxidative polymerization reaction.

[0016] Preferably, the substrate is at least one of a silicon wafer, glass and ITO conductive glass; and the solvent in step (1) is chloroform, toluene, benzene, ethyl acetate, acetone, tetrahydrofuran, N,N-dimethylformamide, dioxane or dichloromethane.

[0017] According to another aspect of the present invention, a surface plasmon-based responsive pattern is provided.

[0018] Preferably, the responsive pattern can realize reversible color change of the pattern under pH stimulation or electrical stimulation. Specifically, by adjusting the pH value of the external environment, polyaniline realizes reversible transformation between the partially oxidized state and the fully oxidized state, and the characteristic peak of ultraviolet-visible light absorption of the monolayer film is reversibly shifted, realizing reversible color change of the pattern. When a voltage is applied to the monolayer film, the voltage range is -1V-2V, and polyaniline realizes reversible transformation between the partially oxidized state and the reduced state, and the characteristic peak of ultraviolet-visible light absorption of the monolayer film is reversibly shifted, realizing reversible color change of the pattern.

[0019] According to another aspect of the present invention, there is provided an application of a surface plasmon-based responsive pattern in anti-counterfeiting, sensing or information storage.

[0020] In general, compared with the prior art, the above technical solution conceived by the present invention can at least achieve the following beneficial effects.

[0021] (1) The present invention prepares inorganic nanoparticles with surface modified polymers by a ligand exchange method, and obtains a polymer-grafted inorganic nanoparticle monolayer film by a self-assembly technique. The monolayer film is etched, and the surface of the inorganic nanoparticles in the etched area is exposed. The reduction of surface ligands causes the plasma resonance effect to change, thereby affecting its optical properties, resulting in a macroscopic color difference, thereby obtaining a patterned inorganic nanoparticle monolayer film. However, the color of the pattern at this time is irreversible. Through an oxidative polymerization reaction, a polyaniline shell layer is formed, while the unetched area does not change. The composite color composed of the polyaniline shell layer and the inorganic nanoparticle monolayer film is responsive, and its color can be reversibly changed under external stimuli. Thus, a responsive patterned inorganic nanoparticle monolayer film is obtained, and the reversibility of the pattern color is achieved. The preparation method is novel and simple and easy to implement, and can realize the design and preparation of the surface pattern of the monolayer film.

[0022] (2) The present invention uses a mask to cover the surface of the monolayer film, and utilizes plasma etching technology to remove the polymer ligands on the surface of the inorganic nanoparticles. The degree of polymer etching is controlled by etching time. The characteristic peaks of the ultraviolet-visible light absorption of the inorganic nanoparticle monolayer film will migrate with the degree of etching, and color differences will also appear on a macroscopic scale, thereby realizing the patterning of the monolayer film based on surface plasmons. This method is simple to operate and has a wide range of applications.

[0023] (3) The present invention regulates the thickness of the polyaniline formed on the surface of the inorganic nanoparticles by changing the aniline concentration in the solution containing aniline and the time of the oxidative polymerization reaction. In the present invention, the aniline concentration in the solution containing aniline is strictly controlled to be 1-6mM, and the time of the oxidative polymerization reaction is 1-24h. The aniline concentration in the solution containing aniline is relatively higher, the time of the oxidative polymerization reaction is relatively longer, and the thickness of the polyaniline formed on the surface of the inorganic nanoparticles is thicker, so that the initial composite color formed by the polyaniline shell and the inorganic nanoparticle monolayer film is more obvious. If the aniline concentration in the solution containing aniline is too low and the time of the oxidative polymerization reaction is too short, the polyaniline shell cannot form a film and cannot completely cover the etched area on the inorganic nanoparticle monolayer film.

[0024] (4) The interparticle distance of the inorganic nanoparticle monolayer film in the present invention is controllable, and the surface plasmon resonance effect can be regulated, thereby affecting the initial composite color formed by the polyaniline shell layer and the inorganic nanoparticle monolayer film.

[0025] (5) The pattern prepared by the present invention has the responsiveness and surface plasmon resonance effect of polyaniline and inorganic nanoparticles. By adjusting the pH conditions of the external environment or applying voltage, the ultraviolet-visible light absorption peak of the polyaniline-coated inorganic nanoparticle monolayer film region will undergo a reversible shift, and the color will also undergo a reversible change on a macroscopic scale. The pattern has multiple characteristics such as high resolution, customizability, and reversible color conversion, and can be widely used in fields such as anti-counterfeiting and information storage. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic structural diagram of a responsive pattern based on surface plasmon provided by the present invention;

[0027] Figure 2 It is a schematic diagram of the preparation process of the responsive pattern based on surface plasmon provided by the present invention;

[0028] Figure 3 (a) is a scanning electron microscope image of the orderly arranged monolayer film of polystyrene grafted gold nanoparticles obtained in Example 1 of the present invention; Figure 3 (b) is a transmission electron microscopy image of the orderly arranged monolayer film of polystyrene grafted gold nanoparticles obtained in Example 1 of the present invention;

[0029] Figure 4 (a) is an optical photograph of the responsive pattern of the polystyrene grafted gold nanoparticle monolayer film obtained in Example 1 at one angle. Figure 4 (b) is an optical photograph of the responsive pattern of the polystyrene grafted gold nanoparticle monolayer film obtained in Example 1 observed from another angle;

[0030] Figure 5 It is the ultraviolet-visible light spectrum (UV-vis) corresponding to the pH responsiveness of the pattern obtained in Example 1 of the present invention.

[0031] Figure 6 In Example 1 and Example 2 of the present invention, the single-layer film is subjected to plasma etching, and the etching time is 150s and 210s under the same power, and the corresponding ultraviolet-visible light spectrum (UV-vis) of the single-layer film. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0033] Electrochromic materials can achieve self-adjustable optical and color changes through voltage regulation, and are used in information encryption, anti-counterfeiting and other optoelectronic materials. Conductive polymers, as electrochromic materials, have attracted more and more attention due to their easy synthesis, low cost and stable chemical properties. Polyaniline is one of the most promising and promising conductive polymers, which has the advantages of multiple color changes, short response time and high optical contrast. The present invention utilizes the controllable surface plasma resonance effect of inorganic nanoparticle monolayers and the optical responsiveness of polyaniline to achieve the preparation of highly adjustable responsive patterns.

[0034] The present invention provides a method for preparing a responsive pattern based on surface plasmons, comprising the following steps:

[0035] (1) Preparation of inorganic nanoparticle monolayer film based on surface plasmon: functional group-terminated polymers are modified with inorganic nanoparticles by ligand exchange method, purified by centrifugation, and the polymer-modified inorganic nanoparticles are dispersed in a solvent; the polymer-modified inorganic nanoparticle dispersion is used to prepare a polymer-grafted inorganic nanoparticle monolayer film by self-assembly technology, and transferred to the surface of a substrate; wherein the inorganic nanoparticles include gold, silver, iron oxide, zinc dioxide nanoparticles, and quantum dots such as cadmium selenide and zinc sulfide; the size of the inorganic nanoparticles is 3.5-100 nm; the polymer ligand is an oil-soluble polymer, including polystyrene, polyethylene , polymethyl methacrylate; the functional group of the polymer end-capping is a group containing a thiol (-SH), a disulfide bond (-SS-) or a thioester bond (-CO-S-); the molecular weight of the polymer ligand is 2000-50000g / mol; the solvent is chloroform, toluene, benzene, ethyl acetate, acetone, tetrahydrofuran, N,N-dimethylformamide, dioxane, dichloromethane, which can make the inorganic nanoparticles have good dispersion; the self-assembly technology includes oil / water interface assembly method, LB film assembly method, solvent evaporation assembly method, pulling assembly method or inkjet printing method; the substrate is at least one of silicon wafer, glass and ITO conductive glass.

[0036] (2) Covering the polymer-grafted inorganic nanoparticle monolayer film obtained in step (1) with a mask plate, and performing patterned etching using plasma etching technology; the polymer grafted on the surface of the inorganic nanoparticles on the monolayer film in the etched area is removed; the excitation gas used for the plasma etching is at least one of air, argon, helium, and nitrogen, the plasma etching time is 1-5 minutes, and the etching power used is 1-20W.

[0037] (3) After etching, immersing the substrate in a reaction solution containing aniline, and oxidatively polymerizing the aniline around the inorganic nanoparticles in the etched area to form a polyaniline shell layer through a surface polymerization method; the surfactant in the reaction solution is one of sodium dodecyl sulfate, hexadecyltrimethylammonium bromide, and sodium dodecylbenzene sulfonate, the oxidant is one of ammonium persulfate, hydrogen peroxide, and ferric chloride, the oxidative polymerization reaction time is 1-24 hours, and the pH value of the oxidative polymerization reaction is 0.5-7.

[0038] The preparation method of the invention is simple and controllable. The molecular weight of the functional group-terminated polymer can regulate the surface plasma resonance characteristics between particles in the nanoparticle monolayer film. The nanoparticle spacing ranges from 1 to 40 nm.

[0039] The present invention can adjust the thickness of the polyaniline coated on the surface of the inorganic nanoparticles by changing the monomer concentration and the reaction polymerization time in the solution containing aniline.

[0040] By adjusting the pH conditions of the external environment and applying voltage, under UV-visible light, the UV-visible light absorption peak of the polyaniline-coated inorganic nanoparticle monolayer film area will undergo a reversible shift, and the color will also change reversibly on a macroscopic scale, thus achieving responsive patterned preparation.

[0041] The following are specific embodiments:

[0042] Example 1

[0043] A responsive pattern based on surface plasmon is prepared according to the following method:

[0044] (1) Preparation of polymer grafted inorganic nanoparticle monolayer film: mercapto-terminated polystyrene with a molecular weight of 12,000 g / mol was used to graft the surface of gold nanoparticles with a diameter of 15 nm through two ligand exchange reactions. The gold nanoparticles were then dispersed in a toluene solution and self-assembled to prepare a monolayer film of polystyrene-modified gold nanoparticles in an orderly manner through an oil / water interface rapid assembly method. The monolayer film was then transferred to the surface of a substrate, which was an ITO conductive glass. The substrate was cleaned with acetone and ethanol before use.

[0045] (2) Selective etching of polymer-grafted inorganic nanoparticle monolayer film: A PDMS mask was prepared by scraping, and a customized "CHEM" letter pattern was engraved by laser. The mask was covered on top of the monolayer film, and etching was performed using a plasma cleaner with argon as the plasma excitation gas. The etching time was 150 s and the etching power was 6.8 W. The surface of the gold nanoparticles was partially exposed.

[0046] (3) After etching, the mask was removed and the substrate was quickly placed in a sodium dodecyl sulfate (40 mM) solution. After soaking for 30 min, the substrate was taken out and then placed in a mixed solution of aniline (1.5 mL, 2 mM) and sodium dodecyl sulfate (0.3 mL, 40 mM). The solution was gently shaken for 1 min. Then, an acidic (NH4)2S2O8 solution (1.5 mL, 2 mM, HCl was 10 mM) was added and gently shaken for 1 min. The solution was incubated at room temperature for 4 h. The substrate was taken out and gently washed with deionized water to remove the residual reaction solution on the surface. After drying, a responsive patterned monolayer film based on surface plasmon was obtained.

[0047] (4) pH-responsive patterned monolayer film: The patterned monolayer film obtained above was placed in solutions with different pH values. The pH solution was adjusted with HCl (1 M) and NaOH (1 M). The solution was immersed for 3 min. After reaching equilibrium, the UV-visible spectrum (UV-vis) was measured and its color change was observed. Figure 5 In this embodiment, after the surface plasmon-based responsive patterned monolayer film is immersed in 1M HCl acidic conditions, the color of the monolayer film appears light green. After being immersed in 1M NaOH, the color of the monolayer film turns blue, and the characteristic peak in the UV-vis spectrum graph shifts to the blue.

[0048] (5) Electrically responsive patterned monolayer film: ITO with two monolayer films deposited was used as the working electrode, a platinum wire electrode was used as the counter electrode, and an Ag / AgCl (3M KCl) electrode was used as the reference electrode. A NaCl (0.5M) HCl (0.01M) solution was used as the electrolyte. When an external voltage was applied to the patterned monolayer film on the ITO surface, the color change of the film was observed.

[0049] Example 2

[0050] The present invention can control the plasma etching time and etching power to adjust the removal degree of inorganic nanoparticle surface ligands in the monolayer film, thereby controlling the polyaniline growth site.

[0051] A responsive pattern based on surface plasmon is prepared according to the following method:

[0052] (1) Preparation of polymer grafted inorganic nanoparticle monolayer film: mercapto-terminated polystyrene with a molecular weight of 12,000 g / mol was used to graft the surface of gold nanoparticles with a diameter of 15 nm through two ligand exchange reactions. The gold nanoparticles were then dispersed in a toluene solution and self-assembled to prepare a monolayer film of polystyrene-modified gold nanoparticles in an orderly manner through an oil / water interface rapid assembly method. The monolayer film was then transferred to the surface of a substrate, which was an ITO conductive glass. The substrate was cleaned with acetone and ethanol before use.

[0053] (2) Selective etching of polymer-grafted inorganic nanoparticle monolayer film: A PDMS mask was prepared by scraping, and a custom "CHEM" letter pattern was engraved by laser. The mask was covered on the monolayer film, and etching was performed using a plasma cleaner with argon as the plasma excitation gas. The etching time was 210 s and the etching power was 6.8 W. Almost all of the surface of the gold nanoparticles was exposed. By prolonging the etching time, the degree of etching of the polymer was deepened. See Figure 6 In the UV-vis spectrum, the characteristic peak of the plasma of the inorganic nanoparticle monolayer film is red-shifted compared with Example 1, and the etching degree affects the growth site of aniline on the surface of the nanoparticles. The deeper the etching degree, the greater the proportion of polyaniline on the surface of the inorganic nanoparticles, thus showing a more obvious color.

[0054] (3) After etching, the mask was removed and the substrate was quickly placed in a sodium dodecyl sulfate (40 mM) solution. After soaking for 30 min, the substrate was taken out and then placed in a mixed solution of aniline (1.5 mL, 2 mM) and sodium dodecyl sulfate (0.3 mL, 40 mM). The solution was gently shaken for 1 min. Then, an acidic (NH4)2S2O8 solution (1.5 mL, 2 mM, HCl was 10 mM) was added and gently shaken for 1 min. The solution was incubated at room temperature for 4 h. The substrate was taken out and gently washed with deionized water to remove the residual reaction solution on the surface. After drying, a responsive patterned monolayer film based on surface plasmon was obtained.

[0055] (4) The remaining steps are the same as steps (4) and (5) of Example 1.

[0056] Example 3

[0057] The present invention can adjust the thickness of the polyaniline coated on the surface of the inorganic nanoparticles by changing the monomer concentration in the reaction solution, the reaction polymerization time and the like.

[0058] A responsive pattern based on surface plasmon is prepared according to the following method:

[0059] (1) Preparation of polymer grafted inorganic nanoparticle monolayer film: mercapto-terminated polystyrene with a molecular weight of 12,000 g / mol was used to graft the surface of gold nanoparticles with a diameter of 15 nm through two ligand exchange reactions. The gold nanoparticles were then dispersed in a toluene solution and self-assembled to prepare a monolayer film of polystyrene-modified gold nanoparticles in an orderly manner through an oil / water interface rapid assembly method. The monolayer film was then transferred to the surface of a substrate, which was an ITO conductive glass. The substrate was cleaned with acetone and ethanol before use.

[0060] (2) Selective etching of polymer-grafted inorganic nanoparticle monolayer film: A PDMS mask was prepared by scraping, and a customized "CHEM" letter pattern was engraved by laser. The mask was covered on top of the monolayer film, and etching was performed using a plasma cleaner with argon as the plasma excitation gas. The etching time was 210 s and the etching power was 6.8 W. Almost all the surfaces of the gold nanoparticles were exposed.

[0061] (3) After etching, remove the mask, quickly place the substrate in a sodium dodecyl sulfate (40mM) solution, soak for 30 minutes and then take it out, then place the substrate in a mixed solution of aniline (1.5mL, 2mM) and sodium dodecyl sulfate (0.3mL, 40mM), gently shake for 1min, then add acidic (NH4)2S2O8 solution (1.5mL, 2mM, HCl is 10mM), gently shake for 1min, incubate at room temperature for 8h, take out the substrate, and gently wash it with deionized water to remove the residual reaction solution on the surface, and after drying, a responsive patterned monolayer film based on surface plasmon is obtained. Compared with the incubation time in Example 2, it can be found that the extension of the incubation time can increase the thickness of the polyaniline shell layer, and the color of the monolayer film pattern is deepened macroscopically.

[0062] (4) The remaining steps are the same as steps (4) and (5) of Example 1.

[0063] Example 4

[0064] A responsive pattern based on surface plasmon is prepared according to the following method:

[0065] (1) Preparation of polymer grafted inorganic nanoparticle monolayer film: mercapto-terminated polystyrene with a molecular weight of 12,000 g / mol was used to graft the surface of gold nanoparticles with a diameter of 15 nm through two ligand exchange reactions. The gold nanoparticles were then dispersed in a toluene solution and self-assembled to prepare a monolayer film of polystyrene-modified gold nanoparticles in an orderly manner through an oil / water interface rapid assembly method. The monolayer film was then transferred to the surface of a substrate, which was an ITO conductive glass. The substrate was cleaned with acetone and ethanol before use.

[0066] (2) Selective etching of polymer-grafted inorganic nanoparticle monolayer film: A PDMS mask was prepared by scraping, and a customized "CHEM" letter pattern was engraved by laser. The mask was covered on top of the monolayer film, and etching was performed using a plasma cleaner with argon as the plasma excitation gas. The etching time was 210 s and the etching power was 6.8 W. Almost all the surfaces of the gold nanoparticles were exposed.

[0067] (3) The present invention can control the thickness of polyaniline coated on the surface of inorganic nanoparticles by changing the monomer concentration, reaction polymerization time, etc. in the solution containing aniline. After etching, remove the mask, quickly place the substrate in a sodium dodecyl sulfate (40mM) solution, soak for 30 minutes and then take it out, then place the substrate in a mixed solution of aniline (1.5mL, 4mM) and sodium dodecyl sulfate (0.3mL, 40mM), gently shake for 1min, then add acidic (NH4)2S2O8 solution (1.5mL, 2mM, HCl is 10mM), gently shake for 1min, stand and incubate at room temperature for 8h, take out the substrate, and gently wash it with deionized water to remove the residual reaction solution on the surface, and after drying, a responsive patterned monolayer film based on surface plasmon is obtained. Comparing the reaction results of different aniline concentrations in Example 3, it can be found that with the same incubation time, increasing the concentration will increase the thickness of the polyaniline shell layer, and the color of the monolayer film pattern will deepen macroscopically.

[0068] (4) The remaining steps are the same as steps (4) and (5) of Example 1.

[0069] Example 5

[0070] A responsive pattern based on surface plasmon is prepared according to the following method:

[0071] (1) Preparation of polymer grafted inorganic nanoparticle monolayer film: mercapto-terminated polystyrene with a molecular weight of 2000 g / mol was used to graft the surface of gold nanoparticles with a diameter of 15 nm through two ligand exchange reactions, which were then dispersed in a toluene solution. The polystyrene-modified gold nanoparticle monolayer with orderly arrangement was prepared by self-assembly through the LB film technique and transferred to the surface of a substrate, which was an ITO conductive glass. The substrate was cleaned with acetone and ethanol before use.

[0072] (2) Selective etching of polymer-grafted inorganic nanoparticle monolayer film: A PDMS mask was prepared by scraping, and a dot matrix with a diameter of about 50 μm was customized by laser engraving. The mask was covered on top of the monolayer film, and etching was performed using a plasma cleaner with argon as the plasma excitation gas. The etching time was 120 s and the etching power was 6.8 W. The surface of the gold nanoparticles was partially exposed.

[0073] (3) After etching, the mask was removed and the substrate was quickly placed in a sodium dodecyl sulfate (40 mM) solution. After soaking for 30 min, the substrate was taken out and then placed in a mixed solution of aniline (1.5 mL, 2 mM) and sodium dodecyl sulfate (0.3 mL, 40 mM). The solution was gently shaken for 1 min. Then, an acidic (NH4)2S2O8 solution (1.5 mL, 2 mM, HCl was 10 mM) was added and gently shaken for 1 min. The solution was incubated at room temperature for 8 h. The substrate was taken out and gently washed with deionized water to remove the residual reaction solution on the surface. After drying, a responsive patterned monolayer film based on surface plasmon was obtained.

[0074] (4) The remaining steps are the same as steps (4) and (5) of Example 1.

[0075] Example 6

[0076] A responsive pattern based on surface plasmon is prepared according to the following method:

[0077] (1) Preparation of polymer grafted inorganic nanoparticle monolayer film: mercapto-terminated polystyrene with a molecular weight of 2000 g / mol was used to graft the surface of gold nanoparticles with a diameter of 5 nm through two ligand exchange reactions, and then the gold nanoparticles were dispersed in a chloroform solution. The polystyrene-modified silver nanoparticles were orderly arranged in a monolayer film prepared by an oil / water interface rapid assembly method and transferred to the surface of a substrate, wherein the substrate was ITO conductive glass, and the substrate was cleaned with acetone and ethanol before use.

[0078] (2) Selective etching of polymer-grafted inorganic nanoparticle monolayer film: A PDMS mask was prepared by scraping, and a customized "CHEM" letter pattern was engraved by laser. The mask was covered on top of the monolayer film, and etching was performed using a plasma cleaner with argon as the plasma excitation gas. The etching time was 90 s and the etching power was 6.8 W. The surface of the silver nanoparticles was almost completely exposed.

[0079] (3) After etching, the mask was removed and the substrate was quickly placed in a sodium dodecyl sulfate (40 mM) solution. After soaking for 30 min, the substrate was taken out and then placed in a mixed solution of aniline (1.5 mL, 2 mM) and sodium dodecyl sulfate (0.3 mL, 40 mM). The solution was gently shaken for 1 min. Then, an acidic (NH4)2S2O8 solution (1.5 mL, 2 mM, HCl was 10 mM) was added and gently shaken for 1 min. The solution was incubated at room temperature for 12 h. The substrate was taken out and gently washed with deionized water to remove the residual reaction solution on the surface. After drying, a responsive patterned monolayer film based on surface plasmon was obtained.

[0080] (4) The remaining steps are the same as steps (4) and (5) of Example 1.

[0081] Example 7

[0082] A responsive pattern based on surface plasmon is prepared according to the following method:

[0083] (1) Preparation of polymer grafted inorganic nanoparticle monolayer film: mercapto-terminated polystyrene with a molecular weight of 22,000 g / mol was used to graft the surface of silver nanoparticles with a diameter of 10 nm through two ligand exchange reactions, which were then dispersed in a toluene solution. A polystyrene-modified silver nanoparticle monolayer with orderly arrangement was prepared by self-assembly through the pulling method, and then transferred to the surface of a substrate, which was an ITO conductive glass. The substrate was cleaned with acetone and ethanol before use.

[0084] (2) Selective etching of polymer-grafted inorganic nanoparticle monolayer film: A PMMA mask was prepared by scraping, and a dot matrix with a diameter of about 100 μm was customized by laser engraving. The mask was covered on top of the monolayer film, and etching was performed using a plasma cleaner with argon as the plasma excitation gas. The etching time was 90 s and the etching power was 10.5 W. The silver nanoparticles were partially exposed.

[0085] (3) After etching, the mask was removed and the substrate was quickly placed in a sodium dodecyl sulfate (40 mM) solution. After soaking for 30 min, the substrate was taken out and then placed in a mixed solution of aniline (1.5 mL, 2 mM) and sodium dodecyl sulfate (0.3 mL, 40 mM). The solution was gently shaken for 1 min. Then, an acidic (NH4)2S2O8 solution (1.5 mL, 2 mM, HCl was 10 mM) was added and gently shaken for 1 min. The solution was incubated at room temperature for 12 h. The substrate was taken out and gently washed with deionized water to remove the residual reaction solution on the surface. After drying, a responsive patterned monolayer film based on surface plasmon was obtained.

[0086] (4) The remaining steps are the same as steps (4) and (5) of Example 1.

[0087] Example 8

[0088] A responsive pattern based on surface plasmon is prepared according to the following method:

[0089] (1) Preparation of polymer grafted inorganic nanoparticle monolayer film: amino-terminated polymethyl methacrylate with a molecular weight of 22,000 g / mol was used to graft the surface of silver nanoparticles with a diameter of 30 nm through two ligand exchange reactions, which were then dispersed in a toluene solution and self-assembled to prepare a monolayer film of polystyrene-modified silver nanoparticles in an orderly arrangement through an oil / water interface rapid assembly method, and then transferred to the surface of a substrate, which was an ITO conductive glass. The substrate was cleaned with acetone and ethanol before use.

[0090] (2) Selective etching of polymer-grafted inorganic nanoparticle monolayer film: A PMMA mask was prepared by scraping, and straight lines of different widths were customized by laser engraving. The mask was covered on top of the monolayer film, and a plasma cleaner was used to continuously etch with argon as the plasma excitation gas. The etching time was 150 s and the etching power was 10.5 W to partially expose the surface of the silver nanoparticles.

[0091] (3) After etching, the mask was removed and the substrate was quickly placed in a sodium dodecyl sulfate (40 mM) solution. After soaking for 30 min, the substrate was taken out and then placed in a mixed solution of aniline (1.5 mL, 2 mM) and sodium dodecyl sulfate (0.3 mL, 40 mM). The solution was gently shaken for 1 min. Then, an acidic (NH4)2S2O8 solution (1.5 mL, 2 mM, HCl was 10 mM) was added and gently shaken for 1 min. The solution was incubated at room temperature for 12 h. The substrate was taken out and gently washed with deionized water to remove the residual reaction solution on the surface. After drying, a responsive patterned monolayer film based on surface plasmon was obtained.

[0092] (4) The remaining steps are the same as steps (4) and (5) of Example 1.

[0093] Example 9

[0094] A responsive pattern based on surface plasmon is prepared according to the following method:

[0095] (1) Preparation of polymer grafted inorganic nanoparticle monolayer film: amino-terminated polymethyl methacrylate with a molecular weight of 50,000 g / mol was used to graft the surface of silver nanoparticles with a diameter of 30 nm through two ligand exchange reactions, and then dispersed in a toluene solution. The monolayer film of polystyrene-modified silver nanoparticles with orderly arrangement was prepared by self-assembly through the oil / water interface rapid assembly method, and then transferred to the surface of a substrate, which was an ITO conductive glass. The substrate was cleaned with acetone and ethanol before use.

[0096] (2) Selective etching of polymer-grafted inorganic nanoparticle monolayer film: A PMMA mask was prepared by scraping, and straight lines of different widths were customized by laser engraving. The mask was covered on top of the monolayer film, and a plasma cleaner was used to continuously etch with argon as the plasma excitation gas. The etching time was 180 s and the etching power was 10.5 W to partially expose the surface of the silver nanoparticles.

[0097] (3) After etching, the mask was removed and the substrate was quickly placed in a sodium dodecyl sulfate (40 mM) solution. After soaking for 30 min, the substrate was taken out and then placed in a mixed solution of aniline (1.5 mL, 2 mM) and sodium dodecyl sulfate (0.3 mL, 40 mM). The solution was gently shaken for 1 min. Then, an acidic (NH4)2S2O8 solution (1.5 mL, 2 mM, HCl was 10 mM) was added and gently shaken for 1 min. The solution was incubated at room temperature for 24 h. The substrate was taken out and gently washed with deionized water to remove the residual reaction solution on the surface. After drying, a responsive patterned monolayer film based on surface plasmon was obtained.

[0098] (4) The remaining steps are the same as steps (4) and (5) of Example 1.

[0099] Comparative Example 1

[0100] This comparative example 1 is the same as the example 1, but the etching time is 30s, the surface polymer of the nanoparticles in the monolayer film is not removed, no growth site is provided for the surface polymerization reaction of aniline, and the reversible color change of the monolayer film cannot be achieved.

[0101] Comparative Example 2

[0102] Comparative Example 2 is the same as Example 1, but the aniline concentration is 0.5 mM. The aniline concentration is too low, so the thickness of the polyaniline shell layer on the surface of the inorganic nanoparticles is very thin, the color change is not obvious, and the reversible color change of the single-layer film cannot be achieved.

[0103] Comparative Example 3

[0104] Comparative Example 3 is the same as Example 1, but the oxidative polymerization reaction time is 0.5 h. In a short time, the thickness of the polyaniline shell layer on the surface of the inorganic nanoparticles is very thin, the color change is not obvious, and the reversible color change of the single-layer film cannot be achieved.

[0105] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a responsive pattern based on surface plasmon, characterized in that: The following steps are involved: (1) Grafting inorganic nanoparticles with functional group-terminated polymers by ligand exchange method, and dispersing the polymers in a solvent to obtain a dispersion of polymer-grafted inorganic nanoparticles; the dispersion undergoes self-assembly to obtain a monolayer film of polymer-grafted inorganic nanoparticles, and the monolayer film is transferred to a substrate surface; (2) The single-layer film is patterned and etched, and the polymer grafted on the surface of the inorganic nanoparticles on the single-layer film in the etched area is removed; the etching time is 1-5 minutes; (3) immersing the etched substrate in a solution containing aniline, so that the aniline undergoes an oxidative polymerization reaction on the surface of the inorganic nanoparticles in the etched area to form a polyaniline shell layer, and the surface plasmon-based responsive pattern is formed by the inorganic nanoparticle monolayer film in the etched area and the polyaniline shell layer formed on the surface thereof; The concentration of aniline in the solution containing aniline is 1-6 mM; and the time of the oxidative polymerization reaction is 1-24 h.

2. The preparation method according to claim 1, characterized in that The patterned etching in step (2) is performed by using a plasma etching technique; the excitation gas used in the plasma etching technique is at least one of air, argon, helium, and nitrogen, and the etching power is 1-20W.

3. The preparation method according to claim 1, characterized in that: The inorganic nanoparticles in step (1) are quantum dots, inorganic metal nanoparticles or metal oxide nanoparticles, and the size of the inorganic nanoparticles is 3.5-100 nm; the distance between the inorganic nanoparticles in the polymer-grafted inorganic nanoparticle monolayer film is 1-40 nm.

4. The preparation method according to claim 3, characterized in that: The inorganic metal nanoparticles are gold nanoparticles or silver nanoparticles, the metal oxide nanoparticles are ferroferric oxide nanoparticles or zinc dioxide nanoparticles, and the quantum dots are cadmium selenide quantum dots or zinc sulfide quantum dots.

5. The preparation method according to claim 1, characterized in that: The polymer is an oil-soluble polymer.

6. The preparation method according to claim 5, characterized in that: The oil-soluble polymer is one of polystyrene, polyethylene, polymethyl methacrylate and poly (4-vinyl pyridine), the molecular weight of the polymer is 2000-50000 g / mol, and the functional group is a group containing a thiol group, a disulfide bond or a thioester bond.

7. The preparation method according to any one of claims 1 to 6, characterized in that: The self-assembly includes oil / water interface assembly method, LB film assembly method, solvent evaporation assembly method, pulling assembly method or inkjet printing method.

8. The preparation method according to any one of claims 1 to 6, characterized in that: The aniline-containing solution further comprises an oxidant and a surfactant.

9. The preparation method according to claim 8, characterized in that: The oxidant is one of ammonium persulfate, hydrogen peroxide and ferric chloride; the surfactant is one of sodium dodecyl sulfate, hexadecyltrimethylammonium bromide and sodium dodecylbenzenesulfonate; the pH value of the oxidative polymerization reaction is 0.5-7; and the thickness of the polyaniline shell layer formed on the surface of the inorganic nanoparticles is regulated by changing the aniline concentration in the solution containing aniline and the time of the oxidative polymerization reaction.

10. The preparation method according to any one of claims 1 to 6, characterized in that: The substrate is at least one of a silicon wafer, glass and ITO conductive glass; the solvent in step (1) is chloroform, toluene, benzene, ethyl acetate, acetone, tetrahydrofuran, N,N-dimethylformamide, dioxane or dichloromethane.

Citation Information

Patent Citations

  • Dual-ligand Janus nano-particle as well as preparation method and application thereof

    CN109776843A