A TiZr-based amorphous solder for vacuum brazing Ti60 titanium alloy and its preparation method

Through the vacuum brazing technology of TiZr-based amorphous brazing material, the problems of low strength and easy corrosion of titanium alloy are solved, high-quality Ti60 titanium alloy welding is achieved, and the welding strength and corrosion resistance are improved, and the traditional crystal state is overcome. Inconvenient use of solder and high temperature defects.

CN115592298BInactive Publication Date: 2024-11-01LIAONING UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211378822.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-04
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing titanium alloy brazing technology, the brazing seams are low and easy to corrode, and the crystal brazing material is inconvenient to use, and defects are easily generated at high temperatures, resulting in low welding quality and poor corrosion resistance, especially for TiZr-based amorphous brazing material. Brazing Ti60 titanium alloy lacks involved.

Method used

Ti60 titanium alloy is vacuum brazed with TiZr-based amorphous brazing material. By designing the Ti43Zr27Mo5Cu10Be15 brazing components, it is prepared into an amorphous brazing strip, and after surface treatment and assembly, brazing is performed in a vacuum furnace to control the best brazing Temperature and insulation time to achieve high-quality brazing.

Benefits of technology

It improves the strength of the brazing joint and corrosion resistance, reduces the melting point of the brazing material, enhances the degree of alloying and composition uniformity, significantly improves the welding quality and joint strength, reduces thermal stress and segregation, and avoids the melting of the base material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115592298B_ABST
    Figure CN115592298B_ABST
Patent Text Reader

Abstract

The invention discloses a TiZr-based amorphous solder for vacuum brazing Ti60 titanium alloy and a preparation method thereof. The TiZr-based amorphous solder is added to the brazing of the titanium alloy. The Ti-based amorphous alloy has high strength and good corrosion resistance. Zr elements and Ti elements of the same family are mutually soluble. The melting point of the TiZr-based solder is further reduced. The TiZr-based solder has the advantages of adjustable composition, uniform chemical composition, convenient use, good fluidity, good spreadability, etc., and can effectively overcome the shortcomings of the current technology and improve the brazing quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding, and in particular to a TiZr-based amorphous solder for vacuum brazing Ti60 titanium alloy and a preparation method thereof. Background Art

[0002] Ti60 titanium alloy is a near-α high-temperature titanium alloy. This material has good high-temperature performance and structural stability. It can work for a long time in a high-temperature environment above 600°C. Therefore, it is suitable for use in high-temperature environments in the fields of aerospace, petrochemicals, shipbuilding, etc. In recent years, the application of titanium alloy structural parts has become more and more extensive, and the realization of high-quality connection of titanium alloys has broad application prospects.

[0003] Due to the excellent mechanical and corrosion resistance of titanium, as a strategic resource commonly used in aerospace and ocean fields, there is a wealth of research data on brazing filler metals for titanium and its alloys at home and abroad. Currently, the brazing filler metals for titanium and its alloys mainly include silver-based brazing filler metals, aluminum-based brazing filler metals, titanium-based brazing filler metals and palladium-based brazing filler metals. The brazing temperature of silver-based and aluminum-based brazing filler metals is low, which is far lower than the α→β phase transition temperature of titanium and its alloys. The brazing process hardly damages the structure and properties of the base material. The aluminum-based brazing filler metal also has little dissolution of the titanium base material, which is very suitable for brazing thin-walled structures such as honeycomb structures or heat exchangers. However, their brazed joints have low strength and the shear strength is often below 200Pa. The aluminum-based brazing filler metal only has tens of MPa, and the joints have poor corrosion resistance, which will cause failure in corrosive media. Titanium-based brazing filler metal has low dissolution, high brazing joint strength, good corrosion resistance, and can obtain brazing joints with excellent performance. Titanium-based brazing filler metal often uses Cu, Ni, etc. that can form low-melting eutectics with Ti as melting-reducing elements, and adds Zr that can be miscible with Ti to further reduce the melting point to obtain TiZr-based brazing filler metal. The addition of some beneficial alloying elements can further reduce the melting point of the brazing filler metal or regulate the brazing seam structure. However, titanium-based brazing filler metal has a high melting point, and brazing at a higher temperature may cause the base material to undergo a β transformation. It is also easy to become brittle and difficult to process and form, and the weld part has the disadvantages of being easy to corrode and break.

[0004] Existing titanium alloy brazing generally uses crystalline brazing filler metals. Ordinary crystalline materials are mostly eutectic or near-eutectic components, mostly composed of brittle elements, and are often made into powder or paste, which is inconvenient to use and requires the use of brazing flux, which is prone to defects at high temperatures. After the brazing process, the brazing seam becomes the weak point of the entire workpiece, and the brazed joint has low strength and poor corrosion resistance. The melting temperature of crystalline brazing filler metals is higher than that of amorphous brazing filler metals. During the brazing process, the base material may be melted, causing welding defects.

[0005] The existing brazing technology at home and abroad does not involve the brazing of Ti60 titanium alloy with TiZr-based amorphous brazing filler metal. Therefore, the present invention aims to provide a vacuum brazing of Ti60 titanium alloy with TiZr-based amorphous brazing filler metal and a preparation method thereof. The TiZr-based amorphous brazing filler metal is added to the brazing of the titanium alloy. The Ti-based amorphous alloy has high strength and good corrosion resistance. The Zr element and the Ti element are of the same family and are mutually soluble. The melting point of the TiZr-based brazing filler metal is further reduced. It has the advantages of adjustable composition, uniform chemical composition, easy use, good fluidity, good spreadability, etc. It can effectively overcome the shortcomings of the current technology and improve the brazing quality. Summary of the invention

[0006] The purpose of the present invention is to provide a TiZr-based amorphous solder for vacuum brazing Ti60 titanium alloy and a preparation method thereof, so as to solve the problems existing in the above-mentioned prior art.

[0007] To achieve the above object, the present invention provides the following solutions:

[0008] The invention provides a TiZr-based amorphous solder vacuum brazing Ti60 titanium alloy, comprising two Ti60 titanium alloy mother materials, wherein the connection between the two Ti60 titanium alloy mother materials is fixed by a TiZr-based amorphous solder strip.

[0009] Preferably, the chemical elements and mass fractions contained in the Ti60 titanium alloy base material are: Al 5.8%, Sn4%, Zr4%, Nb 0.7%, Ta 1.5%, Si 0.4%, C 0.06%, and the rest are Ti and unavoidable impurities, with a total mass fraction of 100%.

[0010] Preferably, the two pieces of the Ti60 titanium alloy base material are connected by overlapping, T-shaped, beveled, bent or locked.

[0011] Preferably, the TiZr-based amorphous solder strip is made of Ti 43 Zr 27 Mo5C 10 Be 15 .

[0012] The present invention also provides a method for preparing the above-mentioned TiZr-based amorphous solder by vacuum brazing Ti60 titanium alloy, comprising the following steps:

[0013] S1. Obtain Ti60 titanium alloy base material by wire cutting;

[0014] S2. Preparation of TiZr-based amorphous brazing material strips;

[0015] S3. Surface treatment of the Ti60 titanium alloy base material and the TiZr-based amorphous brazing material strip;

[0016] S4. Assembling the surface treated Ti60 titanium alloy base material and TiZr-based amorphous brazing material strip;

[0017] S5. The assembled Ti60 titanium alloy base material and TiZr-based amorphous brazing material strip are placed in a vacuum furnace for brazing;

[0018] S6. After the welding is completed, the vacuum furnace is opened after the furnace is cooled to room temperature to obtain the TiZr-based amorphous brazing filler metal for vacuum brazing of Ti60 titanium alloy.

[0019] Preferably, step S2 specifically includes:

[0020] S21. Design solder composition;

[0021] S22. Prepare the ingredients according to the ingredients in step S21;

[0022] S23. The raw material in step S22 is vacuum melted;

[0023] S24. Obtain TiZr-based amorphous solder strips by spinning.

[0024] Preferably, in step S3, the surface treatment is: grinding the surface to be welded of the Ti60 titanium alloy base material until the metallic luster is exposed, so that the contact surface during brazing is flat and smooth without an oxide layer, and then using an ultrasonic cleaner to ultrasonically clean the Ti60 titanium alloy base material and the TiZr-based amorphous brazing material strip, and finally drying.

[0025] Preferably, in step S4, the assembly is as follows: assembling two pieces of Ti60 titanium alloy base materials in an overlapping manner, laying a TiZr-based amorphous brazing material strip between the two pieces of Ti60 titanium alloy base materials, bundling the two pieces of Ti60 titanium alloy base materials with tungsten wire to form a brazing sample, and placing the sample in a quartz tube and sealing the tube with high vacuum.

[0026] Preferably, in step S5, the brazing is as follows: placing the assembled sample in a vacuum furnace, heating the temperature from room temperature to 500°C at a rate of 5°C / min, and then heating the temperature to a preset brazing temperature at a rate of 10°C / min, keeping the temperature at this temperature, and finally stopping heating, keeping the vacuum furnace in a vacuum state, and cooling to room temperature.

[0027] Preferably, the brazing temperature is 1000-1040° C., and the holding time is 15-30 min.

[0028] Compared with the prior art, the present invention has achieved the following beneficial technical effects:

[0029] 1. Use TiZr-based amorphous alloy brazing filler metal instead of traditional crystalline brazing filler metal for Ti60 titanium alloy brazing, overcoming the shortcomings of low brazing seam strength and easy corrosion in the prior art.

[0030] 2. Adding Zr elements that are miscible with Ti elements to the solder composition design to obtain TiZr solder can further reduce the solder melting point, reduce the impact on the parent material structure, and regulate the solder joint structure to improve the solder joint quality.

[0031] 3. The composition of amorphous solder is adjustable, the degree of alloying is high, and it is easy to use. Ordinary crystalline materials are mostly eutectic or near-eutectic components, mostly composed of brittle elements, and are often made into powder or paste, which is inconvenient to use, and requires the use of flux, which is prone to defects at high temperatures. Amorphous solder is made by a rapid solidification method, with a high degree of alloying and strong adjustable composition. TiZr-based amorphous solder has a certain ductility and can be directly prepared into strips. The parts to be welded can be pre-assembled into the required shape, and the solder can be accurately loaded into the weld, which can significantly improve the strength and reliability of the joint and achieve the purpose of precise welding.

[0032] 4. Amorphous solder has uniform chemical composition, high brazing quality and good corrosion resistance. Amorphous solder solidifies quickly, so atoms do not have time to diffuse, and the internal atoms are kept in a disordered arrangement state, so the organization is uniform and can melt in a relatively small temperature range when heated. The brazing time is greatly shortened, segregation is significantly reduced, the diffusion depth is increased, and the brazing quality and corrosion resistance are greatly improved.

[0033] 5. TiZr-based amorphous solder has a low melting point, good fluidity and good spreadability, so its melting point is lower than that of traditional materials. Therefore, the thermal stress and grain growth generated during the welding process are greatly reduced, and the welding quality is improved.

[0034] 6. TiZr-based amorphous solder has good spreadability, a small melting temperature range, short melting time, good homeotropic fluidity, full capillary adsorption, and improved welding quality.

[0035] 7. The quality of thin-walled welds brazed with TiZr-based amorphous solder is high. The base material does not melt during the brazing process, and the amorphous solder has a low brazing temperature and a long brazing time, so there will be no corrosion of the base material.

[0036] 8. Determining the optimal brazing temperature and holding time through experiments is conducive to the diffusion of alloy elements, reducing the amount of intermetallic compounds in the brazing seam and improving the brazing quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0038] Figure 1 This is a schematic diagram of an assembly process for preparing a TiZr-based amorphous solder for vacuum brazing Ti60 titanium alloy provided by the present invention;

[0039] In the figure: 1: Ti60 titanium alloy base material, 2: TiZr-based amorphous brazing material strip. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The purpose of the present invention is to provide a TiZr-based amorphous solder for vacuum brazing Ti60 titanium alloy and a preparation method thereof, so as to solve the problems existing in the prior art.

[0042] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0043] Embodiment 1:

[0044] This embodiment provides a TiZr-based amorphous solder vacuum brazing Ti60 titanium alloy and a preparation method thereof, such as Figure 1 As shown, it includes two pieces of Ti60 titanium alloy base materials 1, the two pieces of Ti60 titanium alloy base materials 1 are overlapped with each other, and the connection between the two is brazed and fixed by a TiZr-based amorphous brazing material strip 2.

[0045] The Ti60 titanium alloy base material 1 contains the following chemical elements and their mass fractions: Al 5.8%, Sn 4%, Zr 4%, Nb 0.7%, Ta 1.5%, Si 0.4%, C 0.06%, and the rest are Ti and unavoidable impurities, with a total mass fraction of 100%. A 10 mm × 10 mm × 2 mm square base material and a 100 mm × 10 mm × 2 mm strip base material are obtained by wire cutting.

[0046] TiZr-based amorphous brazing material strip 2 uses Ti 43 Zr 27 Mo5C 10 Be 15 , and its preparation method comprises:

[0047] Step 1: Designing solder composition; by consulting literature to summarize the effects of different elements on the microstructure, interface reaction and mechanical properties of the brazed joint, designing the solder composition used in the present invention, the present invention relates to elements such as Ti and Zr, and TiZr-based solder further reduces the melting point of the solder, and can regulate the brazing seam structure;

[0048] Step 2: Prepare the ingredients according to the ingredients in step 1; prepare the ingredients according to the composition expression of the titanium-based multi-component amorphous alloy designed in step 1, weigh accurately to 3 decimal places, and each alloy ingot weighs about 15g. The metal raw materials selected in the experiment are all of industrial grade purity;

[0049] Step 3: vacuum melting the raw materials in step 2 using a high vacuum non-consumable arc melting system;

[0050] Step 4: Obtain the TiZr-based amorphous solder strip 2 by spinning the strip.

[0051] After the above materials are prepared, the Ti60 titanium alloy base material 1 and the TiZr-based amorphous brazing material strip 2 need to be surface treated; the surface to be welded of the Ti60 titanium alloy base material is polished until the metallic luster is exposed, so that the contact surface during brazing is flat and smooth without an oxide layer, and then the Ti60 titanium alloy base material and the TiZr-based amorphous brazing material strip are ultrasonically cleaned using an ultrasonic cleaner, and finally dried;

[0052] After cleaning, the surface-treated Ti60 titanium alloy base material 1 and the TiZr-based amorphous brazing material strip 2 are assembled; two pieces of Ti60 titanium alloy base materials 1 are assembled in an overlapping manner, and the overlapping area is 10mm×10mm. A TiZr-based amorphous brazing material strip is laid between the two pieces of Ti60 titanium alloy base materials. The two pieces of Ti60 titanium alloy base materials are tied tightly with tungsten wire to form a brazing sample. The sample is placed in a quartz tube. In order to reduce the concentration of oxygen in the quartz tube and reduce the oxidation of the base material, the air in the tube is evacuated with a vacuum pump before the experiment, and then argon gas is introduced to fill the quartz tube, which is repeated 3 times to reduce the oxygen content in the tube to ensure the welding quality.

[0053] The assembled Ti60 titanium alloy base material 1 and the TiZr-based amorphous brazing material strip 2 are placed in a vacuum furnace for brazing; the vacuum furnace adopts a GSL-1600X atmosphere protection tubular high-temperature furnace, which uses bipolar silicon platinum and molybdenum rod heaters as the main working heating control elements, and is protected by 99.99% argon gas. The rated temperature is 1600°C, and a 708P temperature controller is used to automatically control the working temperature, with good temperature control accuracy (±1°C). In addition, the tubular high-temperature furnace is also equipped with a vacuum device, which can work in a variety of environments, and is largely The practical application scope of this tubular high-temperature furnace is increased in a certain degree. The working temperature of this tubular high-temperature furnace is high, the temperature control accuracy is good, the operation is simple and the maintenance is convenient. It is widely used in industrial production and scientific research. The heating rate is set to 5℃ / min, from room temperature to 500℃, and then to the set welding temperature of 1000℃ at 10℃ / min. After keeping warm for 15 minutes, it is cooled to room temperature with the furnace. During the cooling process, the welding sample is annealed to improve the performance of the base material, effectively reduce the thermal stress generated during welding, and reduce the brittleness of the brazing weld, so that TiZr-based amorphous brazing filler metal vacuum brazing Ti60 titanium alloy can be obtained.

[0054] Embodiment 2:

[0055] This embodiment is the same as embodiment 1, the only difference being that the heat preservation time is 30 minutes.

[0056] Embodiment 3:

[0057] This embodiment is the same as embodiment 1, except that the welding temperature is controlled at 1020°C.

[0058] Embodiment 4:

[0059] This embodiment is the same as embodiment 1, except that the welding temperature is controlled at 1020° C. and the holding time is 30 minutes.

[0060] Embodiment 5:

[0061] This embodiment is the same as embodiment 1, except that the welding temperature is controlled at 1040°C.

[0062] Embodiment 6:

[0063] This embodiment is the same as embodiment 1, except that the welding temperature is controlled at 1040° C. and the holding time is 30 minutes.

[0064] Comparative analysis of Example 1 and Example 2 shows that at this temperature, the use of Ti 43 Zr 27 Mo5C 10 Be 15The brazing seam of the Ti60 joint obtained by brazing with brazing filler metal is well formed, and there are no defects such as unmelted brazing filler metal, incomplete penetration, and pores. The microstructure in the brazing seam after 15 minutes of heat preservation is divided into two regions, namely the diffusion zone on both sides of the base metal and the brazing seam region. There are continuous and irregular gray rod-shaped microstructures in the diffusion zone on both sides of the base metal, and there are a large number of irregular gray blocky intermetallic compounds A, dark gray microstructure B, black microstructure C and dark microstructure D in the brazing seam region; the morphology of the brazing seam after 30 minutes of heat preservation is similar to that of the brazing seam after 15 minutes of heat preservation. There are continuous and irregular gray rod-shaped microstructures in the diffusion zone on both sides of the base metal, and there are large blocks of gray intermetallic compounds, dark microstructures, dark gray microstructures and black microstructures in the brazing seam region; it can be clearly seen by magnifying the diffusion zone on the base metal side by 500 times that the black microstructure is distributed in lamellar layers.

[0065] Comparative analysis of Example 3 and Example 4 shows that at this temperature, the brazing seam is well formed without defects such as unmelted brazing material, incomplete penetration, and pores. The internal structure of the brazing seam with insulation for 15 minutes is divided into two areas, namely the diffusion zone on both sides of the base material and the brazing seam area. There are continuously distributed irregular gray rod-shaped structures in the diffusion zone on both sides of the base material, and there are a large number of irregular gray block-shaped intermetallic compounds A, dark gray structure B, black structure C and dark structure D in the brazing seam area; the internal structure morphology of the brazing seam with insulation for 30 minutes is similar to that of the brazing seam with insulation for 15 minutes. There are continuously distributed gray rod-shaped structures in the diffusion zone of the base material, and there are a large number of large gray block-shaped structures in the brazing seam area, in which the dark structure, black structure and dark gray structure separate these intermetallic compounds; it can be clearly seen by magnifying the diffusion zone on the base material side by 500 times that there are leaf-shaped intermetallic compounds in the dark structure and flaky metal compounds in the black structure; it can be clearly seen by magnifying the brazing seam area by 500 times that the dark structure morphology of the brazing seam area is the same as that at the edge of the brazing seam, and the structure morphology of the brazing seam is mainly composed of gray structure A, dark structure B, black structure C and dark gray structure D.

[0066] A comparative analysis of Example 5 and Example 6 shows that the structure in the brazing seam after insulation for 15 minutes is divided into two regions, namely the diffusion zone on both sides of the base material and the brazing seam region. There is a continuously distributed gray columnar structure in the diffusion zone of the base material, and gray blocky intermetallic compounds A, dark structure B, black structure C and dark gray structure D appear in the brazing seam region; the internal structure morphology of the brazing seam after insulation for 30 minutes is similar to that of the brazing seam after insulation for 15 minutes; it can be clearly seen by magnifying the diffusion zone on the base material side by 500 times that there are leaf-shaped intermetallic compounds in the dark structure of the brazing seam, and flaky metal compounds in the black structure.

[0067] Shear performance experiments were conducted on Examples 1-6. Three samples were tested for each example under the same conditions. The following table shows the shear performance of Ti 43 Zr27 Mo5C 10 Be 15 Average shear strength of Ti60 specimens brazed with solder.

[0068]

[0069] It can be seen that as the brazing temperature increases, the strength of the joint at room temperature increases first and then decreases. 43 Zr 27 Mo5C 10 Be 15 When used as solder, the average shear strength of the joint reaches a maximum value of 530MPa at 1020℃ for 30min.

[0070] Then, the microhardness of Example 4 was measured, and the maximum hardness reached 450.6 HV.

[0071] In summary, using Ti 43 Zr 27 Mo5C 10 Be 15 The brazing material can realize the brazing connection of Ti60. The Ti60 / Ti 43 Zr 27 Mo5C 10 Be 15 The typical interface structure of the / Ti60 joint is: Ti60 / Ti2Cu diffusion layer / α-Ti+(Ti,Zr)2Cu / Ti2Cu diffusion layer / Ti60; with the increase of brazing temperature, the Ti60 / Ti 43 Zr 27 Mo5C 10 Be 15 / Ti60 joints react more and more fully; Ti and Zr elements in the base materials and brazing filler metals on both sides diffuse with each other. With the increase of brazing temperature and the extension of holding time, the organization in the brazing seam gradually grows and fills the brazing seam. Through the analysis of the tensile strength and microhardness of the specimens, it can be found that: 43 Zr 27 Mo5C 10 Be 15 When used as solder for brazing, the shear strength of the joint can reach 530MPa at 1020℃ for 30min.

[0072] The present invention uses specific examples to illustrate the principles and implementation methods of the present invention. The above examples are only used to help understand the method and core ideas of the present invention. At the same time, for those skilled in the art, according to the ideas of the present invention, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A TiZr-based amorphous solder vacuum brazing Ti60 titanium alloy, characterized in that: It comprises two pieces of Ti60 titanium alloy base materials, and the connection between the two pieces of Ti60 titanium alloy base materials is fixed by a TiZr-based amorphous brazing material strip; The TiZr-based amorphous brazing material strip is made of Ti 43 Zr 27 Mo5C 10 Be 15 ; Brazing is as follows: the assembled sample is placed in a vacuum furnace, the temperature is raised from room temperature to 500°C at a rate of 5°C / min, and then raised to the preset brazing temperature at a rate of 10°C / min, and the temperature is kept at this temperature, and finally the heating is stopped, and the vacuum furnace is kept in a vacuum state and cooled to room temperature; The brazing temperature is 1000-1040℃ and the holding time is 15-30min.

2. The TiZr-based amorphous solder vacuum brazing Ti60 titanium alloy according to claim 1, characterized in that: The chemical elements and mass fractions contained in the Ti60 titanium alloy base material are: Al 5.8%, Sn 4%, Zr 4%, Nb 0.7%, Ta 1.5%, Si 0.4%, C 0.06%, and the rest are Ti and unavoidable impurities, with a total mass fraction of 100%.

3. The TiZr-based amorphous solder vacuum brazing Ti60 titanium alloy according to claim 1, characterized in that: The two pieces of the Ti60 titanium alloy base material are connected by overlapping, T-shaped, beveled, bent or locked.

4. A method for preparing TiZr-based amorphous solder for vacuum brazing Ti60 titanium alloy, characterized in that: The following steps are involved: S1. Obtain Ti60 titanium alloy base material by wire cutting; S2. Preparation of TiZr-based amorphous solder strip; the TiZr-based amorphous solder strip is made of Ti 43 Zr 27 Mo5C 10 Be 15 ; S3. Surface treatment of the Ti60 titanium alloy base material and the TiZr-based amorphous brazing material strip; S4. Assembling the surface treated Ti60 titanium alloy base material and TiZr-based amorphous brazing material strip; S5. Place the assembled Ti60 titanium alloy base material and TiZr-based amorphous brazing material strip into a vacuum furnace for brazing; brazing is as follows: place the assembled sample in a vacuum furnace, heat the temperature from room temperature to 500°C at a rate of 5°C / min, and then heat it to a preset brazing temperature at a rate of 10°C / min, keep the temperature at this temperature, and finally stop heating, keep the vacuum furnace in a vacuum state and cool to room temperature; the brazing temperature is 1000-1040°C, and the holding time is 15-30min; S6. After the welding is completed, the vacuum furnace is opened after the furnace is cooled to room temperature to obtain the TiZr-based amorphous brazing filler metal for vacuum brazing of Ti60 titanium alloy.

5. The method for preparing TiZr-based amorphous solder for vacuum brazing Ti60 titanium alloy according to claim 4, characterized in that: Step S2 specifically includes: S21. Design solder composition; S22. Prepare the ingredients according to the ingredients in step S21; S23. The raw material in step S22 is vacuum melted; S24. Obtain TiZr-based amorphous solder strips by spinning.

6. The method for preparing TiZr-based amorphous solder for vacuum brazing Ti60 titanium alloy according to claim 5, characterized in that: In step S3, the surface treatment is as follows: the surface to be welded of the Ti60 titanium alloy base material is polished until the metallic luster is exposed, so that the contact surface during brazing is flat and smooth without an oxide layer, and then the Ti60 titanium alloy base material and the TiZr-based amorphous brazing material strip are ultrasonically cleaned using an ultrasonic cleaner, and finally dried.

7. The method for preparing TiZr-based amorphous solder for vacuum brazing Ti60 titanium alloy according to claim 5, characterized in that: In step S4, the assembly is as follows: assembling two pieces of Ti60 titanium alloy mother materials in an overlapping manner, laying a TiZr-based amorphous brazing material strip between the two pieces of Ti60 titanium alloy mother materials, bundling the two pieces of Ti60 titanium alloy mother materials with tungsten wire to form a brazing sample, and placing the sample in a quartz tube and sealing the tube with high vacuum.