An accelerated corrosion test method for large aircraft components

By designing component-level test pieces and combining accelerated corrosion tests with periodic infiltration and atomization methods, the test site and facilities for accelerated corrosion of large components structures are solved, and an efficient and low-cost test process is achieved, and the test process is simplified.

CN115656022BActive Publication Date: 2024-11-12XIAN AIRCRAFT DESIGN INST OF AVIATION IND OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211406169.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-10
Publication Date
2024-11-12
Estimated Expiration
2042-11-10

AI Technical Summary

Technical Problem

When conducting accelerated corrosion tests for large components of aircraft, the prior art requires large sites and facilities, which leads to high difficulty, long cycle, high cost and low efficiency.

Method used

Design component-level test pieces, and use periodic infiltration and atomization to conduct accelerated corrosion tests. The acceleration corrosion factor is determined through component-level test results, correct the acceleration test relationship of large component structures, and use atomization to conduct accelerated corrosion tests to simplify the test. process.

Benefits of technology

It has achieved simplification of accelerated corrosion tests for large components of the aircraft, improved efficiency, reduced costs, and shortened test cycles, and is suitable for engineering applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115656022B_ABST
    Figure CN115656022B_ABST
Patent Text Reader

Abstract

The present application belongs to the field of aircraft corrosion testing, and is an accelerated corrosion testing method for large aircraft component structures. By designing an accelerated corrosion test of a component-level test piece, there is no need to conduct a periodic infiltration test of the large component structure, and only an accelerated corrosion test of an atomization method with a simpler implementation method needs to be conducted. The accelerated corrosion comparison test of the component-level test piece is used to obtain an accelerated corrosion factor, thereby determining a second equivalent relationship under the atomization method for the large component structure. After the accelerated corrosion test time of the large component structure is calculated according to the periodic infiltration application method, the corrosion time is divided by the accelerated corrosion factor to obtain the atomization accelerated corrosion time of the large component structure; the second equivalent relationship is multiplied by the atomization accelerated corrosion time to obtain the equivalent corrosion years of the large component structure; by adopting this method, the simplification of the accelerated corrosion test of large aircraft structures can be achieved, which has the characteristics of high efficiency, low cost, and short cycle, and is convenient for engineering applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of aircraft corrosion testing, and in particular relates to an accelerated corrosion testing method for large aircraft component structures. Background Art

[0002] In the actual aircraft service process, it is inevitable that it is affected by various corrosive environmental media, which causes corrosion of aircraft structural metal materials and aging of non-metallic materials, thus affecting the aircraft life. Therefore, the influence of the corrosive environment must be considered in the fatigue design process of aircraft structures. When designing aircraft structures, it is very difficult to consider the influence of environmental corrosion on the structure according to the actual time history during service, and it cannot meet the requirements of model development progress. In engineering, accelerated corrosion test technology is generally used to simulate this influence. For key fatigue parts under corrosive conditions, the commonly used accelerated corrosion test method is cyclic infiltration. The cyclic infiltration environmental spectrum (hereinafter referred to as "cyclic infiltration spectrum") is a laboratory accelerated environmental spectrum used by laboratories in many countries to carry out the influence of pre-corrosion on structural fatigue life. This test environmental spectrum can well reproduce the corrosion damage characteristics of field aircraft metal structures. Its effectiveness has been verified in the development of multiple domestic models, and therefore it is widely used in the development of domestic and foreign models. However, for large aircraft component structures, due to the large geometric size of the test piece, when using the cyclic infiltration spectrum, a larger test site and related test supporting facilities are required, which brings great inconvenience to the smooth implementation of the test, increases the test difficulty, cycle and test cost, and is not conducive to model development.

[0003] Therefore, how to effectively implement accelerated corrosion testing of large-scale test pieces is a problem that needs to be solved. Summary of the invention

[0004] The purpose of this application is to provide a method for accelerated corrosion testing of large aircraft components to solve the problem that a large area is required for corrosion testing of large-sized test pieces, resulting in great test difficulty, long cycle, high cost and low efficiency.

[0005] The technical solution of the present application is: an accelerated corrosion test method for large aircraft component structures, comprising: determining the composition of the corrosive solution in the cyclic immersion spectrum and the first equivalent acceleration relationship based on the local environmental characteristics of the large aircraft component structure; analyzing and determining the susceptible structural parts and material types of the large component structure based on the structural configuration and material characteristics of the corresponding large aircraft component; using the same material type as the susceptible structural parts of the large component structure to design a component-level test piece with typical structural characteristics; using the same solution as in the cyclic immersion spectrum of the large component, and conducting an accelerated corrosion test on the component-level test piece in a periodic immersion and atomization implementation mode respectively; establishing an accelerated corrosion factor for two accelerated corrosion tests with the same solution composition and different implementation modes based on the accelerated corrosion test results of the component-level test piece; using the accelerated corrosion factor to correct the first equivalent acceleration relationship of the periodic immersion accelerated test of the large component structure to obtain a second equivalent acceleration relationship; implementing the accelerated corrosion environment spectrum in an atomization manner, determining the implementation period of the accelerated corrosion environment spectrum of the large component structure using the second equivalent acceleration relationship, conducting an accelerated corrosion test in an atomization manner, and completing the accelerated corrosion test of the large component.

[0006] Preferably, at least two groups of component-level test pieces are provided, one group for accelerated corrosion test in periodic immersion mode and the other group for accelerated corrosion test in atomization mode simultaneously, and the accelerated corrosion factor is determined based on the results of the two groups of component-level accelerated corrosion tests.

[0007] Preferably, the second equivalent acceleration relationship is the product of the first equivalent acceleration relationship and the accelerated corrosion factor.

[0008] Preferably, the local environmental characteristics of the large aircraft component structure include temperature, humidity, precipitation, solid precipitation, phoenix, fog, salt spray, seawater, chloride ion concentration, sulfur ion concentration in the air, atmospheric pollutants and industrial waste gas.

[0009] The present application discloses an accelerated corrosion test method for large aircraft component structures. By designing an accelerated corrosion test of a component-level test piece, there is no need to conduct a periodic immersion test of the large component structure. Only an accelerated corrosion test of an atomization method with a simpler implementation method is required. The second equivalent acceleration relationship of the large component structure under the atomization method is determined by utilizing the accelerated corrosion test of the component-level test piece. The second equivalent acceleration relationship is the first equivalent acceleration relationship divided by the accelerated corrosion factor. After the accelerated corrosion test time of the large component structure is calculated according to the periodic immersion application method, the corrosion time is divided by the accelerated corrosion factor to obtain the atomization accelerated corrosion time of the large component structure. The equivalent corrosion years of the large component structure are obtained by dividing the second equivalent relationship by the atomization accelerated corrosion time. By adopting this method, the simplification of the accelerated corrosion test of large aircraft structure components can be achieved, which has the characteristics of high efficiency, low cost, and short cycle, and is convenient for engineering application. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] In order to more clearly illustrate the technical solution provided by the present application, the following is a brief introduction to the accompanying drawings. Obviously, the accompanying drawings described below are only some embodiments of the present application.

[0011] Figure 1 This is a schematic diagram of the overall process of this application. DETAILED DESCRIPTION

[0012] In order to make the purpose, technical solutions and advantages of the implementation of this application clearer, the technical solutions in the embodiments of this application will be described in more detail below in conjunction with the drawings in the embodiments of this application.

[0013] An accelerated corrosion test method for large aircraft component structures is provided, in which an atomization accelerated corrosion test is added. The atomization accelerated corrosion test has a relatively fast corrosion time and is relatively convenient to implement because oxygen is more sufficient during the implementation process. The corrosion time of the periodic immersion method is relatively slow, but it is inconvenient to implement for large component structures.

[0014] like Figure 1 As shown, the following steps are included:

[0015] Step S100, determining the composition of the corrosion solution in the immersion spectrum and the first equivalent acceleration relationship according to the local environmental characteristics of the aircraft large component structure;

[0016] The local environmental characteristics of large aircraft structures include temperature, humidity, precipitation, solid precipitation, wind, fog, salt spray, seawater, chloride ion concentration, sulfur ion concentration in the air, atmospheric pollutants and industrial waste gas.

[0017] Step S200, analyzing and determining the corrosion-prone structural parts and material types of the large component structure based on the structural configuration and material properties of the corresponding large component of the aircraft;

[0018] Step S300, designing a component-level test piece with typical structural characteristics by using the same material type as the corrosion-prone structural part of the large component structure;

[0019] Step S400, using the same solution as in the cyclic immersion spectrum of the large component, to perform an accelerated corrosion test on the component-level test piece in the implementation mode of cyclic immersion and atomization respectively;

[0020] In order to ensure the efficiency of the test, at least two groups of component-level test pieces are set up, one group for accelerated corrosion test in periodic immersion mode, and the other group for accelerated corrosion test in atomization mode. The accelerated corrosion factor is determined based on the results of the two groups of component-level accelerated corrosion tests. This method can obtain the accelerated corrosion factor more quickly and accurately.

[0021] Since the test environment of the component-level test piece is the same as that of the large-component structure, the test results of the two can be compared to obtain the acceleration relationship of the large-component structure.

[0022] Step S500, establishing accelerated corrosion factors for two accelerated corrosion tests with the same solution composition and different implementation methods according to the accelerated corrosion test results of the component-level test piece;

[0023] Step S600, using the accelerated corrosion factor to correct the first equivalent acceleration relationship of the large component structure periodic immersion accelerated test to obtain a second equivalent acceleration relationship. The second equivalent acceleration relationship is the first equivalent acceleration relationship multiplied by the accelerated corrosion factor.

[0024] Step S700, implement an accelerated corrosion environment spectrum by atomization, the accelerated corrosion environment spectrum includes solution composition and application method, the solution composition includes pH value, temperature and time, etc., the accelerated corrosion environment spectrum of the large component structure is the same as the accelerated corrosion environment spectrum of the element-level test piece, the second equivalent acceleration relationship is used to determine the implementation period of the accelerated corrosion environment spectrum of the large component structure, and an accelerated corrosion test by atomization is performed to complete the accelerated corrosion test of the large component structure.

[0025] The present application designs an accelerated corrosion test for component-level test pieces. There is no need to conduct a periodic immersion test for large component structures. Only an accelerated corrosion test using an atomization method with a simpler implementation method is needed. The accelerated corrosion test for component-level test pieces is used to determine the second equivalent acceleration relationship for the large component structure under the atomization method. The second equivalent acceleration relationship is the first equivalent acceleration relationship multiplied by the accelerated corrosion factor. After the accelerated corrosion test time for the large component structure is calculated based on the periodic immersion application method, the corrosion time is divided by the accelerated corrosion factor to obtain the atomization accelerated corrosion time for the large component structure. The equivalent corrosion years of the large component structure can be obtained by multiplying the second equivalent relationship by the atomization accelerated corrosion time.

[0026] For example, the first equivalent acceleration relationship is 2a / h, the accelerated corrosion test of the periodic immersion method under the component-level test is 2h corrosion, and the accelerated corrosion test of the atomization method under the component-level test is 1h corrosion, then the accelerated corrosion factor is 2, and the second equivalent acceleration relationship is 2×2=4a / h; when the calculated accelerated corrosion test time of the periodic immersion application method of the large component structure is 12h, the corrosion time of the atomization application method of the large component structure is 12h÷2=6h, and the corresponding equivalent service life of the large component is 4a / h×6h=24a.

[0027] Therefore, by adopting this method, the accelerated corrosion test of large aircraft structural components can be simplified, which has the characteristics of high efficiency, low cost, and short cycle, and is convenient for engineering applications.

[0028] The above is only a specific implementation of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application shall be based on the protection scope of the claims.

Claims

1. An accelerated corrosion test method for large aircraft components. It is characterized in that include: According to the local environmental characteristics of large aircraft components, the composition of the corrosion solution in the immersion spectrum and the first equivalent acceleration relationship are determined; Based on the structural configuration and material properties of the corresponding large components of the aircraft, analyze and determine the corrosion-prone structural parts and material types of the large components; Design component-level test pieces with typical structural properties using the same material type as the corrosion-prone structural parts of the large component structure; The accelerated corrosion test of the component-level test pieces was carried out by using the same solutions as in the large component immersion spectrum, respectively, in the implementation mode of periodic immersion and atomization; Based on the results of accelerated corrosion tests on component-level test pieces, the accelerated corrosion factors of two accelerated corrosion tests with the same solution composition and different implementation methods were established; The first equivalent acceleration relationship of the periodic immersion accelerated test of large component structure is corrected by the accelerated corrosion factor to obtain the second equivalent acceleration relationship. The accelerated corrosion environment spectrum is implemented by atomization, the implementation period of the accelerated corrosion environment spectrum of the large component structure is determined by using the second equivalent acceleration relationship, and the accelerated corrosion test by atomization is carried out to complete the accelerated corrosion test of the large component.

2. The accelerated corrosion test method for large aircraft components as claimed in claim 1, Features: At least two groups of component-level test pieces are provided, one group is used for accelerated corrosion test in a periodic immersion mode, and the other group is used for accelerated corrosion test in an atomization mode simultaneously, and the accelerated corrosion factor is determined based on the results of the two groups of component-level accelerated corrosion tests.

3. The accelerated corrosion test method for large aircraft components as claimed in claim 1, Features: The second equivalent acceleration relationship is the product of the first equivalent acceleration relationship and the accelerated corrosion factor.

4. The accelerated corrosion test method for large aircraft components as claimed in claim 1, Features: The local environmental characteristics of the large aircraft component structure include temperature, humidity, precipitation, solid precipitation, wind, fog, salt spray, seawater, chloride ion concentration, sulfur ion concentration in the air, atmospheric pollutants and industrial waste gas.