A normalized prediction method for compound capture performance

By calculating the normalized relative recovery rate, sorting efficiency and composite property index of compounds, a linear formula is established, which solves the problem of low collector development efficiency in the existing technology and achieves efficient flotation of low-grade and fine-grained minerals. Selective separation reduces development costs.

CN115684546BActive Publication Date: 2024-10-22CENT SOUTH UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211345869.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-31
Publication Date
2024-10-22
Estimated Expiration
2042-10-31

AI Technical Summary

Technical Problem

Existing technologies for the development of collectors in the flotation separation of low-grade and fine-grained minerals rely on empirical rules and trial and error, resulting in time-consuming, high cost, low efficiency, and commonly used DFT calculations are difficult to achieve large-scale calculations and predictions.

Method used

A method of normalized prediction of compound capture performance is adopted to establish a linear formula to quickly and accurately predict the flotation performance of compounds by calculating the normalized relative recovery rate, normalized sorting efficiency and normalized composite property index. .

Benefits of technology

It achieves fast, accurate and efficient prediction of the flotation ability of unknown compounds, improves the prediction accuracy of the collector and the versatility of industrial applications, and reduces development costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115684546B_ABST
    Figure CN115684546B_ABST
Patent Text Reader

Abstract

The invention belongs to the field of mineral flotation, and specifically relates to a normalized prediction method for compound collection performance, which respectively calculates the normalized relative recovery rate Rr' and the normalized sorting efficiency SE' of different reference collectors, and calculates the normalized flotation index FI' of each reference collector by formula 1#imgabs0#, and calculates the normalized composite property index PI' of each reference collector by formula 2#imgabs1#, and takes the calculated FI' as the ordinate and the PI' as the abscissa to construct a linear relationship of formula 3 (FI'=A×PI'+B): then the normalized composite property index PI' of the compound to be evaluated is calculated according to formula 2, and the normalized flotation index FI' of the compound to be evaluated is calculated by formula 3, and the flotation performance of the collector to be evaluated is predicted and quantified. The prediction method of the method of the invention is simple, easy to implement, and the prediction result is accurate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of mineral flotation, and in particular relates to the field of reagent collection performance prediction. Background Art

[0002] Flotation is one of the greatest technologies of the 21st century, on the basis of which large-scale utilization of mineral resources by mankind has become possible. The key to successful flotation is a flotation surfactant with high selectivity for different minerals. With the increasing depletion of high-grade minerals, it is of great significance to achieve efficient flotation separation of low-grade and fine-grained minerals. The most basic method to achieve efficient separation of difficult-to-separate minerals is to develop highly selective collectors, which is also an important topic with persistent challenges. In the century-long history of flotation, the development of collectors has mainly relied on empirical rules and trial and error methods, which are very time-consuming, costly and inefficient.

[0003] With the rapid development of computer science and quantum chemistry, theoretical chemistry and computational chemistry have gradually been applied to reveal the intrinsic mechanism of flotation systems. The study of structure-activity relationship (SAR) of collector molecules has ushered in a key opportunity. DFT calculation has become a widely used tool for exploring separation mechanisms and predicting flotation behavior. It has high computational efficiency and accuracy and has become the most popular quantum mechanical model for studying the electronic structure, properties and interactions of crystal surfaces and collectors. However, the DFT calculations commonly used in flotation are mainly periodic calculations, which are time-consuming and expensive, and it is difficult to achieve large-scale calculations and predictions of collectors.

[0004] In the 1990s, quantitative structure-activity relationship (QSAR) models were applied to the field of mineral flotation to simulate the separation efficiency of collectors. However, QSAR or 3D-QSAR modeling methods require the preparation of a large number of collectors with the same skeleton, and can only predict the flotation behavior of collectors with the same skeleton. Therefore, QSAR with low versatility has great difficulties in industrial applications. Therefore, high-throughput prediction and evaluation of collectors remains a challenge. Summary of the invention

[0005] The purpose of the present invention is to provide a normalized prediction method for compound capture performance, aiming to provide a quantitative prediction method for predicting compound flotation performance.

[0006] A normalized prediction method for compound capture performance, comprising the following steps:

[0007] Step (1):

[0008] The normalized relative recovery rate Rr' and normalized separation efficiency SE' of different reference collectors were calculated respectively, and the normalized flotation index FI' of each reference collector was calculated by formula 1.

[0009]

[0010] The normalized relative recovery rate Rr' is the relative recovery rate Rr and the relative recovery rate theoretical maximum value Rr max The ratio ranges from greater than 0 to less than 1; the relative recovery rate Rr is the flotation recovery rate of the target mineral of each reference collector minus the natural flotation rate of the target mineral; Rr max =100%-the floating rate of the target ore;

[0011] The normalized sorting efficiency SE' is the sorting efficiency SE and the theoretical maximum value of sorting efficiency SE. max The ratio of is between greater than 0 and less than 1; wherein the separation efficiency SE is the flotation recovery rate of each reference collector for the target mineral minus the recovery rate of the gangue mineral; SE max =100% - the natural floating rate of the gangue ore;

[0012] The normalized composite property index PI' of each reference collector is calculated by formula 2:

[0013]

[0014] The Volume' is the normalized volume of each reference collector, that is, the volume Volume and the maximum volume Volume in the database max wherein the Volume is the volume of each reference collector;

[0015] The negSurArea' is the normalized negative charge surface area of ​​each reference collector, that is, the negative charge surface area negSurArea and the maximum negative charge surface area negSurArea in the database max wherein the negSurArea is the negatively charged surface area of ​​each reference collector;

[0016] The ICS' is the normalized molecular internal charge distribution state of each reference collector, that is, the molecular internal charge distribution state ICS and the maximum molecular internal charge distribution state ICS in the database. max wherein the ICS is the internal charge distribution state of each reference collector;

[0017] With the calculated FI' as the ordinate and the PI' as the abscissa, the linear formula of formula 3 is plotted and calculated:

[0018] FI'=A×PI'+B Formula 3:

[0019] Step (2):

[0020] According to formula 2 of step (1), the normalized composite property index PI' of the compound to be evaluated is calculated, and the normalized flotation index FI' of the compound to be evaluated is calculated using formula 3 to predict and quantify the flotation performance of the collector to be evaluated on the target ore and gangue ore of step (1).

[0021] The present invention has found that FI' and PI' calculated by formula 1 and formula 2 have an excellent linear relationship. Based on the constructed linear relationship formula, the flotation capacity of the flotation agent for the separation of the target ore-gangue ore can be quickly and accurately screened. The method of the present invention can quickly, accurately and efficiently predict the flotation capacity of unknown compounds.

[0022] In the present invention, the modeling of Formula 1 and Formula 2 is the key to quantifying the flotation capacity of the collector and improving the prediction accuracy.

[0023] The present invention has excellent universality for different mineral systems.

[0024] For example, the target ore is a sulfide ore or an oxide ore;

[0025] Preferably, the sulfide ore is at least one of pyrite, chalcopyrite, galena, sphalerite, sphalerite, molybdenite and chalcocite;

[0026] Preferably, the oxide ore is at least one of fluorite, calcite, scheelite and wolframite.

[0027] The gangue minerals are minerals that need to be separated from the target ore.

[0028] Preferably, in the present invention, the mineral system containing the target ore-gangue ore includes but is not limited to lead-iron sulfide ore, copper-iron sulfide ore, lead-zinc sulfide ore, copper-molybdenum sulfide ore, copper-iron-lead sulfide ore, copper-molybdenum-lead sulfide ore, lead-zinc-iron sulfide ore, copper-lead-zinc-iron sulfide ore or lead-zinc-iron-copper-molybdenum sulfide ore.

[0029] In the present invention, the reference collector is a known collector used for flotation of the target ore, preferably a typical collector in the industry.

[0030] Preferably, the reference collector comprises at least an ionic collector and a non-ionic collector;

[0031] Preferably, the ionic collector comprises at least one of a strong anionic collector and a weak anionic collector;

[0032] The nonionic collector comprises at least one of a heteroatom nonionic collector and a heterocyclic nonionic collector.

[0033] In the present invention, in order to improve the accuracy of prediction, the types of the selected collectors are preferably greater than or equal to 2 types, wherein the collectors having the same binding functional group or parent core are of the same type.

[0034] Preferably, the types of collectors are preferably 3 to 10. Preferably, the number of reference collectors selected from the same type of collector is greater than or equal to 3.

[0035] Preferably, the target ore is a sulfide ore, and the reference collector comprises at least five or more compounds selected from the group consisting of xanthate collectors, black drug collectors, and thiol collectors;

[0036] Preferably, the target ore is an oxidized ore, and the reference collector comprises at least five or more compounds of oleic acid collectors, linoleic acid collectors, and hydroxamic acid collectors.

[0037] In the present invention, in order to improve the evaluation accuracy, the more the number of reference collectors, the better.

[0038] Taking into account the evaluation accuracy and computational efficiency, preferably, the number of compounds selected as the reference collector is greater than or equal to 5, preferably greater than or equal to 10.

[0039] In the present invention, the Rr, Rr', SE, SE' of the target ore and gangue ore of the reference collector can be obtained based on the existing database; the Rr, Rr', SE, SE' of each reference collector can also be calculated based on the existing conventional flotation process.

[0040] For example, by flotation method, the relative recovery rate Rr and separation efficiency SE of each reference collector for target ore-gangue ore are obtained. For another example, the maximum relative recovery rate Rr is calculated based on the natural floatability of the target ore and gangue ore (only adding frother). max and the maximum sorting efficiency SE max That is, in the stage of calculating the Rr and SE of each reference collector during flotation, the reference collector is omitted and only flotation is performed with an equal amount of frother to obtain the Rr of the target ore. max (R max = 100% - the floating rate of the target ore), in addition, the recovery rate of the target ore under the frother - the recovery rate of the gangue ore is SE max (SE max =100% - natural flotation rate of gangue ore). Then, the normalization method is performed to calculate the normalized relative recovery rate Rr' and the normalized separation efficiency SE'.

[0041] In the present invention, when calculating Rr and SE by flotation with reference collectors, the flotation conditions of the reference collectors are similar or the same.

[0042] For example, the dosage ratio of each reference collector is less than or equal to 5 times, preferably 0.9 to 1.2 times, and more preferably the same dosage; preferably, the dosage of each reference collector is 1×10 -6 mol / L~1×10 -2 mol / L, preferably 1×10 -5 mol / L~1×10 -3 mol / L, more preferably 1×10 --4 ~4×10 --4 mol / L.

[0043] A frother is also added to the flotation system, wherein the frother is at least one of pine alcohol, cresol acid, heavy pyridine, methyl isobutyl carbinol, eucalyptus oil, camphor oil, higher alcohols and synthetic frothers;

[0044] Preferably, the amount of frother in the flotation system is 1×10 -7 mol / L~1×10 -3 mol / L is preferably 1×10 -6 mol / L~1×10 -5 mol / L, more preferably 2×10 -6 ~4×10 -6 mol / L.

[0045] Preferably, the pH of the flotation stage is similar or the same, preferably, the pH of the flotation stage is in the pHa region, or in the pHb region; or in the pHc region; wherein the pH of the pHa region is less than 5; the pH of the pHb region is 5-9; and the pH of the pHc region is greater than 9. Preferably, the pH of each reference and the compound to be evaluated is in the same flotation pH region, and the difference is less than or equal to 2.

[0046] In the present invention, each reference collector and the compound to be evaluated can be calculated by Gaussian calculation to obtain the composite property index PI of each compound. The Gaussian calculation is specifically Gaussian 16 (MN15 / def2-TZVP). In the present invention, all property calculations are performed by Gaussian, without periodic calculations, and all calculations only involve collector molecules, without involving minerals or metal ions / atoms.

[0047] The present invention further includes a verification step (3): flotation of the target ore and gangue ore using the compound to be evaluated, calculating the actual flotation index FI based on formula 1 according to actual flotation data, and verifying the expected result by comparing the flotation index of the actual flotation with the calculated flotation index.

[0048] In the present invention, when performing flotation verification to calculate the Rr and SE of the collector to be evaluated, the flotation conditions are preferably close to the conditions when calculating the Rr and SE of the reference collector by flotation.

[0049] Preferably, in step (3), the conditions for flotation calculation of the normalized composite property index PI' and the normalized flotation index FI' of the compound to be predicted are the same as the flotation test conditions of the reference collector.

[0050] The preferred method of the present invention for quickly and quantitatively evaluating and predicting the flotation behavior of a collector based on the linear relationship between the composite property index and the flotation index comprises:

[0051] Step 1: Calculate the normalized relative recovery (Rr') and normalized separation efficiency (SE') of the target mineral by using a variety of representative collectors of the selected flotation separation system to quantify the collection capacity and selectivity of the collector, respectively. A new normalized flotation index (FI') was established.

[0052] Step 2 is to perform simple property calculations on the above collector molecules. The main calculated properties include: volume (Volume), negative charge surface area (negSurArea), and internal charge distribution state of the molecule (ICS). The above parameters are normalized to obtain normalized parameters: normalized volume (Volume'), normalized negative charge surface area (negSurArea'), and normalized internal charge distribution state of the molecule (ICS').

[0053] Step 3: First, the normalized volume (Volume') and the normalized negative charge surface area (negSurArea') are converted into Calculate the normalized new index I a ', used to quantify the influence of the hydrophobic end and the ore-philic end on the collector FI'. a ' and ICS, which is used to quantify the charge distribution in the collector molecule, through the formula The final normalized composite property index (PI') was obtained.

[0054] Step 4: Establish a linear relationship between the obtained PI' and FI', so as to obtain the A and B values ​​in the formula FI'=A×PI'+B, and then obtain a quantitative calculation formula of FI' based on PI' for a certain sorting system.

[0055] Step 5: Calculate the relevant property parameters of the new collector to be predicted (the compound to be evaluated), calculate the PI' of the new collector, and insert it into the calculation formula of PI' and FI' to quickly, conveniently and quantitatively evaluate and predict the flotation behavior of the new collector on the target mineral;

[0056] Step 6: Verify the prediction results using actual flotation tests, including but not limited to single mineral flotation tests, mixed ore flotation tests, actual ore flotation tests and (semi-) industrial experiments.

[0057] In the present invention, in the flotation test verification process of step 5, it is preferred that the flotation reagent system used is similar to the flotation data used to establish the evaluation formula in the early stage. Preferably, the reagent dosage differs by no more than 5 times, and the pulp pH is in the same range (<5, 5-9, >9); further preferably, the reagent dosage differs by no more than 2 times, and the pulp pH value differs by no more than 2 under the premise of being in the same range.

[0058] In the present invention, in the flotation test verification process of step 5, the flotation reagent should contain a frother in addition to the corresponding collector; preferably, at least one of pine alcohol, cresol acid, heavy pyridine, methyl isobutyl carbinol, eucalyptus oil, camphor oil, higher alcohols and synthetic frothers; preferably, the amount of the frother in the flotation reagent is 1×10 - 7 mol / L~1×10 -3 mol / L; more preferably, the amount of the foaming agent is 1×10 -6 mol / L~1×10 -5 mol / L.

[0059] In the present invention, during the flotation test verification process of step 5,

[0060] The flotation reagent does not contain any of the collectors, dispersants, or activators;

[0061] Preferably, the flotation reagent consists only of a collector and a frother.

[0062] The present invention has been found that by limiting the types and quantities of representative flotation collector molecules described in step one, the precision and accuracy of the evaluation method of the present invention and the flotation index formula of the present invention can be greatly improved, wherein the evaluation methods and formulas with more complete types and larger quantities have better precision and accuracy.

[0063] The present invention has found that, when predicting the flotation index of a novel flotation collector molecule, it is more effective to select an evaluation system and an evaluation formula established by using structures that are closer to the molecular structure of the novel flotation collector.

[0064] In the present invention, the flotation process can be achieved by means of existing equipment and means. For example, a single mineral, a mixed ore or an actual ore is crushed and slurried to obtain a pulp, and the flotation agent is added to the pulp to perform flotation.

[0065] The method for predicting the compound capture performance of the present invention selects i kinds of commonly used and typical reference collectors (standard collectors) in the industry according to the types of target ore and gangue ore, namely reference collector 1, reference collector 2, ... reference collector i;

[0066] Through the known database, or using collectors 1, 2, .....i to flotate the target ore and gangue ore, the normalized relative recovery rates Rr1', Rr2' and Rr3' corresponding to each reference collector are obtained respectively. r2 ',......Rr i '; and normalized sorting efficiency SE1', SE2'.....SE i ';

[0067] Then, the normalized flotation index FI' of each collector is calculated by formula 1, which corresponds to FI1', FI2'...FI i ';

[0068] Gauss calculation was used to calculate the volume, negative charge surface area and ICS of reference collector 1 to reference collector i, and then formula 2 was used to calculate and obtain P11', PI2', .....PI of each reference collector. i '..

[0069] With (FI1', PI1'), (FI2', PI2').....(FI i ',PI i ') as coordinates, draw a linear curve, and calculate linear formula 3.

[0070] Then, Gaussian and normalized operations were used to calculate the normalized volume Volume', negative charge surface area negSurArea' and molecular internal charge separation state ICS' of the compound to be evaluated, and the PI of the compound to be evaluated was calculated using formula 2. a '; Substitute this index into linear formula 3 to calculate the FI of the compound to be evaluated a ';

[0071] Use the compound to be evaluated as a collector to flot the target ore and gangue ore and calculate its Rr b ' and SE b '; Then use formula 1 to calculate the actual FI b '; Compare the predicted FI a ' and the real calculated FI b ', calculate the error and verify the evaluation accuracy.

[0072] Beneficial Effects

[0073] The present invention innovatively constructs a normalized flotation index FI' on the premise of balancing the capture capacity and selectivity. It is worth mentioning that the relative recovery rate replaces the recovery rate in FI', which eliminates the influence of natural floatability differences on the evaluation method and better quantifies the true effect of the agent. Through simple calculation of the key parameters of the collector molecule, a rapid qualitative prediction method for FI' is constructed. Furthermore, by combining the parameters, a normalized property index PI' is created. PI' comprehensively considers the influence of the hydrophobic end and the ore-philic end of the collector on FI', and considers the influence of the difference between the two ends on FI'. The results confirm that PI' and FI' have an excellent linear relationship, which provides a theoretical basis for constructing a quantitative calculation formula from PI' to FI'. The above qualitative and quantitative prediction methods were verified using collectors with different structures, and the results show that all methods are reliable. The idea of ​​constructing an evaluation scale in this study provides a new idea for QSAR research in related fields. The qualitative and quantitative evaluation scales and formulas obtained in the embodiments of the present invention can be directly used for prediction of the same separation system under conventional flotation system. If different target minerals need to be predicted or FI' needs to be predicted under unconventional reagent system, it is only necessary to update the scales and constant values ​​in the formulas according to the process of this work. BRIEF DESCRIPTION OF THE DRAWINGS

[0074] Figure 1 It is the technical roadmap of the present invention;

[0075] Figure 2 It is a flotation flow chart of an embodiment;

[0076] Figure 3 The molecular structure diagram of the collector used in the embodiment;

[0077] Figure 4 The PI'-FI' linear relationship and conversion formula of the embodiment;

[0078] Figure 5 The verification results of the embodiment are as follows; DETAILED DESCRIPTION

[0079] Example 1

[0080] This embodiment takes the galena-pyrite separation system as an example to illustrate the specific implementation process of the present invention ( Figure 1 ) and verify the reliability of the prediction results of the method of the present invention.

[0081] A method for quickly and qualitatively evaluating and predicting the flotation behavior of a collector by calculating property parameters comprises the following steps:

[0082] Step 1: Figure 3 The 22 reference collectors recorded in the literature were calculated to obtain (FI i ' and PI i')

[0083] Step a: Rr of 22 reference collectors i ' and sorting efficiency SE i '

[0084] Using a variety of representative collectors in the galena-pyrite separation system ( Figure 3 ) were used to calculate the normalized relative recovery (Rr') and normalized separation efficiency (SE') of the target mineral.

[0085] The actual flotation process is as follows: Figure 2 As shown, the flotation reagent system is: all collector dosages are 2×10 - 4 mol / L, the slurry pH was 7, and the foaming agent was pinene alcohol, with a dosage of 2.5×10 -6 mol / L.

[0086] R max / SE max The way to obtain is: Rr max =100%-R 0(目标矿物) ;SE max =100%-R 0(脉石矿物)

[0087] R0 is the natural flotation rate of a mineral (floatability / recovery rate); the flotation conditions are: the pH of the slurry is 7, the frother is pine alcohol, and the dosage is 2.5×10 -6 mol / L.

[0088] Formula 1 was then used to obtain the normalized flotation index FI of 22 reference collectors. i '. The results are listed in Table 1. In the table: R1 is the recovery rate of the target mineral galena, R2 is the recovery rate of the gangue mineral pyrite, and the SE separation efficiency is the difference between R1 and R2. The relative recovery rate of Rr is the difference between R and R0 (natural flotation, that is, the recovery rate when only the frother is added). In this embodiment, the R0 of galena is 35%, and the R0 of pyrite is 25%);

[0089] The FI' of each reference collector is calculated by formula 1;

[0090] Step b: Gaussian operation of properties of 22 reference collectors, Gaussian 16 (MN15 / def2-TZVP):

[0091] The above collector molecules were subjected to simple property calculation and normalization, and the main calculated properties included: normalized volume (Volume'), normalized negative charge surface area (negSurArea'), and normalized molecular internal charge distribution state (ICS'). The results are listed in Table 2.

[0092] The normalized volume (Volume') and the normalized negative charge surface area (negSurArea') are first calculated by the formula to obtain the normalized new index I a ', used to quantify the influence of the hydrophobic end and the ore-philic end on the collector FI'. a ' and ICS, which is used to quantify the charge distribution in the collector molecule', the PI of 22 collectors was obtained by formula i '(The calculation formula is shown in Formula 2). The results are listed in Table 2.

[0093] Step c:

[0094] The obtained PI i ' and FI i 'A linear relationship is established to obtain the A and B values ​​in the formula FI'=A×PI'+B, and then the quantitative calculation formula of FI' based on PI' for a certain sorting system is obtained. Figure 4 The linear formula drawn was used to evaluate the separation ability of the tested compound on galena-pyrite:

[0095] Step 2:

[0096] By Gaussian calculation, the new collector to be predicted is calculated ( Figure 3 The relevant property parameters (volume, negative charge surface area, ICS) of Test.1~4) in the above formula are normalized and the Pi of the new collector is calculated by using Formula 2. a ', respectively into the calculation formula of FI' = A × PI' + B in step (a), to quickly, conveniently and quantitatively evaluate and predict the FI of the new collector to the target mineral a The calculated value of '(FI', also called FI' cal , the results are shown in Table 3).

[0097] Step 3: Verification:

[0098] The new collector to be predicted is used as the collector, and the flotation process of step a of step (I) is used to flotate the galena-pyrite, and the Rr and separation efficiency SE of the actual test are calculated and normalized, and the actual FI is calculated by formula 1. b Experimental test value of '(FI', also marked as FI' exp );

[0099] Verify FI a ' and FI b The error of ', that is, the error between the calculated value of FI' and the experimental test value, verifies the accuracy of its evaluation.

[0100] Verification results can be found in Figure 5 and Table 3-4.

[0101] Table 1 Flotation results and normalized flotation index of No.1-22 collector selected in this embodiment.

[0102]

[0103] Table 2 Key parameters and normalized composite parameter results of No.1-22 collectors selected in this example.

[0104]

[0105] Table 3 Calculation results of key parameters of collectors in Test.1-4 and PI and FI cal Calculation results

[0106]

[0107] Table 4 Actual flotation test results of Test.1-4 collector, FI exp Calculation results and error analysis

[0108]

[0109] like Figure 4 As shown, there is a good linear relationship between FI' and PI' of collector molecules No.1-22 (R 2 =0.96). The value of A is -1.027 and the value of B is 1.104, which means that PI' and FI' are strictly negatively correlated. Under conventional flotation schemes, the collectors of galena and pyrite flotation systems can directly apply the obtained formula (FI'=-1.027PI'+1.104) to quickly and accurately quantitatively evaluate FI'.

[0110] In order to determine the accuracy of the above quantitative prediction, the PI' value was tested. First, the Test.1-4 collector was calculated and incorporated into the above linear relationship to obtain FI' (FI' cal ) are shown in Table 4. At the same time, the experimental value of FI' (FI' exp ). Figure 5 Draw the FI' exp value, and calculated its relationship with FI' cal The error is shown in Table 4.

[0111] The PI' values ​​of the collectors from Test.1 to Test.4 are 0.426, 0.496, 0.532 and 0.813, respectively, showing a gradually increasing trend, which means that their FI' cal Gradually decreased to 0.667, 0.595, 0.558 and 0.269 respectively. FI' cal With FI' exp The errors are 0.056, -0.029, -0.033 and 0.027 respectively. It can be seen that the quantitative prediction results are reliable and accurate. Figure 5 It was further confirmed in Test.1-4 that the FI' of the collector exp It fell near the standard line.

[0112] The present invention innovatively reconstructs the flotation index (FI) by weighing the capture capacity (relative recovery rate of target minerals) and selectivity (separation efficiency) to represent the comprehensive flotation performance of the collector, and normalizes the flotation index through normalization so that it can be widely used. On the other hand, the properties of the collector are quantified by the key parameters of the collector molecule: the volume used to quantify the size of the hydrophobic end; the negSurArea used to quantify the negative charge area of ​​the collector molecule; and the ICS used to quantify the internal charge distribution state of the collector molecule. The normalized key parameters are selected and fused into the normalized property index PI'. The normalization process solves the problem of different magnitudes of different parameters. The normalized property index PI' is used to quickly and quantitatively predict the FI' of the collector. Through the excellent linear relationship between the normalized property index PI' and the normalized flotation index FI', a formula for quickly and quantitatively calculating the FI' of the new collector is established. The feasibility of the quantitative evaluation method of the present invention is verified by four collectors with different structures. The innovative FI', PI' and the relationship formula between them will provide theoretical support for the structure-activity relationship of surfactants in flotation and related fields, and also have great application prospects.

Claims

1. A method for normalizing the capture performance of a compound, characterized in that the steps include: Step (1): The normalized relative recovery rate Rr' and normalized separation efficiency SE' of different reference collectors were calculated respectively, and the normalized flotation index FI' of each reference collector was calculated by formula 1. Formula 1: The normalized relative recovery rate Rr' is the relative recovery rate Rr and the relative recovery rate theoretical maximum value Rr max The ratio ranges from greater than 0 to less than 1; the relative recovery rate Rr is the flotation recovery rate of the target mineral of each reference collector minus the natural flotation rate of the target mineral; Rr max = 100% - floating rate of target ore; The target ore is a sulfide ore or an oxide ore; The reference collector is a known collector used for flotation of the target ore: the reference collector comprises at least an ionic collector and a non-ionic collector; the ionic collector comprises at least one of a strong anionic collector and a weak anionic collector; The nonionic collector comprises at least one of a heteroatom nonionic collector and a heterocyclic nonionic collector; When the target ore is a sulfide ore, the reference collector comprises at least five or more compounds of xanthate collectors, black medicine collectors, and thiol collectors; When the target ore is an oxidized ore, the reference collector comprises at least five or more compounds selected from the group consisting of oleic acid collectors, linoleic acid collectors, and hydroxamic acid collectors; The normalized sorting efficiency SE' is the sorting efficiency SE and the theoretical maximum value of sorting efficiency SE. max The ratio of is between greater than 0 and less than 1; wherein the separation efficiency SE is the flotation recovery rate of each reference collector for the target mineral minus the recovery rate of the gangue mineral; SE max = 100% - the natural flotation rate of the gangue ore; The normalized composite property index PI' of each reference collector is calculated by formula 2: Formula 2: The Volume' is the normalized volume of each reference collector, that is, the volume Volume and the maximum volume Volume in the database max wherein the Volume is the volume of each reference collector; The negSurArea' is the normalized negative charge surface area of ​​each reference collector, that is, the negative charge surface area negSurArea and the maximum negative charge surface area negSurArea in the database max wherein the negSurArea is the negatively charged surface area of ​​each reference collector; The ICS' is the normalized molecular internal charge distribution state of each reference collector, that is, the molecular internal charge distribution state ICS and the maximum molecular internal charge distribution state ICS in the database. max wherein the ICS is the internal charge distribution state of each reference collector; Gauss calculation is used to calculate the volume Volume, negative charge surface area negSurArea and ICS of each reference collector, and the calculated FI' is the ordinate and the PI' is the abscissa. The linear formula of formula 3 is plotted and calculated: FI' = A × PI' + B Formula 3: Step (2): According to formula 2 of step (1), the normalized volume Volume', negative charge surface area negSurArea' and molecular internal charge separation state ICS' of the compound to be evaluated are calculated by Gaussian and normalized operations, the normalized composite property index PI' of the compound to be evaluated is calculated, and the normalized flotation index FI' of the compound to be evaluated is calculated by formula 3 to predict and quantify the flotation performance of the collector to be evaluated on the target ore and gangue ore of step (1).

2. The normalized prediction method for compound capture performance according to claim 1, characterized in that: The sulfide ore is at least one of pyrite, chalcopyrite, galena, sphalerite, sphalerite, molybdenite and chalcocite.

3. The normalized prediction method for compound capture performance according to claim 1, characterized in that: The oxide ore is at least one of fluorite, calcite, scheelite and wolframite.

4. The normalized prediction method for compound capture performance according to claim 1, characterized in that: The mineral system containing the target ore-gangue ore includes but is not limited to lead-iron sulfide ore, copper-iron sulfide ore, lead-zinc sulfide ore, copper-molybdenum sulfide ore, copper-iron-lead sulfide ore, copper-molybdenum-lead sulfide ore, lead-zinc-iron sulfide ore, copper-lead-zinc-iron sulfide ore or lead-zinc-iron-copper-molybdenum sulfide ore.

5. The normalized prediction method for compound capture performance according to claim 1, characterized in that: The number of compounds selected as reference collectors is greater than or equal to 10.

6. The normalized prediction method for compound capture performance according to claim 1, characterized in that: By flotation method, the relative recovery rate Rr and separation efficiency SE of each reference collector for the target ore-gangue ore are obtained; The maximum relative recovery rate Rr is calculated based on the natural floatability of the target ore and the gangue ore. max and the maximum sorting efficiency SE max After normalization calculation, the normalized relative recovery rate Rr' and the normalized sorting efficiency SE' were obtained.

7. The normalized prediction method for compound capture performance according to claim 6, characterized in that: The dosage of each reference collector is close or the same.

8. The normalized prediction method for compound capture performance according to claim 6, characterized in that: The dosage ratio of each reference collector is less than or equal to 5 times.

9. The normalized prediction method for compound capture performance according to claim 8, characterized in that: The dosage ratio of each reference collector is 0.9~1.2 times.

10. The normalized prediction method for compound capture performance according to claim 9, characterized in that: The dosage of each reference collector is the same.

11. The normalized prediction method for compound capture performance according to claim 1, characterized in that: A foaming agent is also added to the flotation system, and the foaming agent is at least one of pine alcohol, cresol acid, heavy pyridine, methyl isobutyl carbinol, eucalyptus oil, camphor oil and synthetic foaming agents.

12. The normalized prediction method for compound capture performance according to claim 1, characterized in that: A frother is also added to the flotation system, and the frother is a higher alcohol.

13. The normalized prediction method for compound capture performance according to claim 11, characterized in that: The amount of frother in the flotation system is 1 × 10 -7 mol / L ~ 1 × 10 -3 mol / L.

14. The normalized prediction method for compound capture performance according to claim 11, characterized in that: The amount of frother in the flotation system is 1 × 10 -6 mol / L ~ 1 × 10 -5 mol / L.

15. The normalized prediction method for compound capture performance according to claim 1, characterized in that: The pH of the flotation stage is similar or the same.

16. The normalized prediction method for compound capture performance according to claim 15, characterized in that: The pH in the flotation stage is in the pHa zone, or in the pHb zone; or in the pHc zone; Among them, the pH in the pHa zone is less than 5; the pH in the pHb zone is 5~9; and the pH in the pHc zone is greater than 9.

17. The normalized prediction method for compound capture performance according to claim 16, characterized in that: The pH values ​​of the flotation of the reference and the compound to be evaluated are in the same flotation pH range, and the difference is less than or equal to 2.

18. The normalized prediction method for compound capture performance according to claim 17, characterized in that: The flotation pH of each reference collector is the same.

19. The normalized prediction method for compound capture performance according to any one of claims 1 to 18, characterized in that: The method further includes a verification step (3): flotation of the target ore and gangue ore using the compound to be evaluated, calculating the actual normalized flotation index FI' based on the actual flotation data and formula 1, and verifying the expected result by comparing the flotation index of the actual flotation with the calculated flotation index.

20. The normalized prediction method for compound capture performance according to claim 19, characterized in that: In step (3), the conditions for flotation calculation of the normalized composite property index PI' and the normalized flotation index FI' of the compound to be predicted are the same as the flotation test conditions of the reference collector.

Citation Information

Patent Citations

  • PH adjustment in the flotation of sulphide minerals

    AU2002233051B2

  • Technique for improving complex vulcanizing copper mine ore floatation indicators

    CN101172267A

  • Method for separating calcium carbonate and gypsum

    CN105307774A

  • Bauxite treatment method