A wear-resistant material and preparation method thereof

By forming a combined structure of nano-Fe2O3 particle coating and soft metal coating on the surface of the steel substrate, the problems of fretting wear and silver embrittlement in the existing technology are solved, the fatigue life and bonding force of the material are significantly improved, and the service life is extended.

CN115725932BActive Publication Date: 2024-10-22GUIZHOU UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211341333.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-31
Publication Date
2024-10-22
Estimated Expiration
2042-10-31

AI Technical Summary

Technical Problem

Existing metal surface treatment technology is prone to fretting wear under high load and long-term service conditions. In particular, the silver-plated layer is prone to silver brittleness, resulting in shortened material life and insufficient bonding force, making it difficult to effectively prevent fretting wear.

Method used

It adopts a combined structure in which the surface of the steel substrate is covered with a nano-Fe2O3 particle coating and a soft metal coating. The nano-Fe2O3 particle coating is formed through sliding friction processing, and the soft metal coating is deposited by magnetron sputtering to control the thickness and porosity of the coating. Improve bonding force and lubrication effect, extend material life.

Benefits of technology

It significantly improves the fretting wear fatigue life of the material, prevents the silver layer from entering the matrix during the fretting extrusion process, avoids silver brittleness, and extends the service life of the wear-resistant material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115725932B_ABST
    Figure CN115725932B_ABST
Patent Text Reader

Abstract

The present invention provides a wear-resistant material and a preparation method thereof, belonging to the technical field of metal surface treatment. The nano Fe2O3 particle coating in the present invention can improve the bonding force between the soft metal coating and the steel substrate, thereby improving the fretting fatigue life of the soft metal coating; during fretting wear, the nano Fe2O3 particles in the nano Fe2O3 particle coating reduce the fretting wear of the wear-resistant material by rolling, and at the same time, the nano Fe2O3 particle coating and the soft metal coating jointly play a lubricating role, significantly reducing the fretting wear of the wear-resistant material. In addition, the present invention controls the thickness and porosity of the nano Fe2O3 particle coating, so that during the wear process of applying positive stress, the soft metal in the soft metal coating is squeezed into the gap of the nano Fe2O3 particle coating, thereby achieving the wrapping and bonding of the nano Fe2O3 particles, protecting the nano Fe2O3 particle coating from peeling off, and improving the fretting fatigue life of the wear material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal surface treatment, and in particular relates to a wear-resistant material and a preparation method thereof. Background Art

[0002] Wear is one of the main failure modes of mechanical parts. Fretting wear in closely fitting parts in the fields of machinery, aerospace, nuclear reactors, transportation vehicles, etc. can cause material loss and dimensional changes in components, and even accelerate the initiation and expansion of cracks, thus greatly reducing the fatigue life of components.

[0003] In order to eliminate or slow down micro-motion wear, material surface modification is the main research direction. Among them, the simple hard phase film layer is easy to fall off during micro-motion wear due to its high hardness and poor toughness, which seriously reduces the service life of the film layer. Silver plating, molybdenum plating, copper plating, aluminum plating and multi-layer soft coating in soft coating technology have good life extension effects under low load and short term, but there is insufficient bonding between the coating and the substrate. When the load is large and long-term service conditions are required, the service life is still short. In particular, the silver plating layer is prone to silver brittleness under long-term service conditions, which accelerates micro-motion failure. Summary of the invention

[0004] The object of the present invention is to provide a wear-resistant material and a preparation method thereof. The wear-resistant material of the present invention has good fretting wear resistance and a high fretting wear fatigue life.

[0005] The invention provides a wear-resistant material, comprising a steel substrate, a nano Fe2O3 particle coating loaded on the surface of the steel substrate, and a soft metal coating covering the surface of the nano Fe2O3 particle coating; the nano Fe2O3 particle coating has a thickness of 0.1 to 1 μm and a porosity of 5 to 15%.

[0006] Preferably, the particle size of the nano-Fe2O3 particles is 5 to 70 nm.

[0007] Preferably, the soft metal coating has a thickness of 2 to 6 μm.

[0008] Preferably, the soft metal in the soft metal coating includes one of Ag, Mo, Cu and Al.

[0009] The present invention also provides a method for preparing the wear-resistant material described in the above scheme, comprising the following steps:

[0010] The steel substrate is subjected to sliding friction processing to generate an oxidation reaction to form a nano Fe2O3 particle coating; the positive pressure of the sliding friction processing is 20 to 150 N, and the processing area per unit time is 1 to 5 mm 2 / min;

[0011] Soft metal is deposited on the surface of the nano Fe2O3 particle coating by magnetron sputtering to form a soft metal coating to obtain the wear-resistant material.

[0012] Preferably, the hardness of the processing head used for sliding friction processing is 2000-3000 HV, and the hardness of the steel substrate is HRC30-HRC50.

[0013] Preferably, the roughness of the steel substrate is 0.2-1.2 μm.

[0014] Preferably, the structure of the steel matrix includes one or more of tempered martensite, tempered troostite, tempered troostite, bainite and pearlite.

[0015] Preferably, the magnetron sputtering includes sequentially performing medium frequency magnetron sputtering and direct current magnetron sputtering.

[0016] Preferably, the chamber pressure of the medium frequency magnetron sputtering and the direct current magnetron sputtering is independently 0.4-0.5 Pa, the bias voltage is -100 V, the current is independently 12-15 A, and the gas environment is N2; the time of the medium frequency magnetron sputtering is 20-30 min, and the time of the direct current magnetron sputtering is 90-150 min.

[0017] The present invention provides a wear-resistant material, comprising a steel substrate, a nano Fe2O3 particle coating loaded on the surface of the steel substrate, and a soft metal coating covering the surface of the nano Fe2O3 particle coating; the thickness of the nano Fe2O3 particle coating is 0.1-1 μm, and the porosity is 5-15%. The present invention uses the nano Fe2O3 particle coating as an intermediate layer to improve the bonding force between the soft metal coating and the steel substrate, thereby improving the fretting fatigue life of the soft metal coating; during fretting, the nano Fe2O3 particles in the nano Fe2O3 particle coating can reduce the fretting wear of the wear-resistant material by rolling, and at the same time, the nano Fe2O3 and the soft metal coating can also play a lubricating role together during the fretting wear process, significantly reducing the fretting wear of the wear-resistant material. In addition, the present invention controls the thickness and porosity of the nano Fe2O3 particle coating so that during the wear process of applying positive stress, the soft metal in the soft metal coating is squeezed into the gap of the nano Fe2O3 particle coating, thereby wrapping and bonding the nano Fe2O3 particles, protecting the highly brittle nano Fe2O3 particle coating from peeling off, and thus improving the fretting fatigue life of the wear material. The results of the embodiment show that the nano Fe2O3 particle coating of the present invention can prevent the silver in the silver layer from entering the substrate during the fretting extrusion process, thereby avoiding the occurrence of silver brittleness. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 Schematic diagram of the friction micromachining process used in Example 1;

[0019] Figure 2 This is a SEM image of the nano-Fe2O3 particle coating of Example 1 at a magnification of 20 μm;

[0020] Figure 3 This is the SEM image of the nano-Fe2O3 particle coating of Example 1 at a magnification of 50nm;

[0021] Figure 4 This is a comparison chart of the friction coefficients of S1 to S3;

[0022] Figure 5 This is a comparison chart of the wear rates of S1 to S3;

[0023] Figure 6 This is the SEM analysis image of S3 after wear at a magnification of 500 μm;

[0024] Figure 7 This is the SEM analysis image of S3 after wear at a magnification of 2 μm;

[0025] Figure 8 This is the EDS spectrum of S3 after wear. DETAILED DESCRIPTION

[0026] The invention provides a wear-resistant material, comprising a steel substrate, a nano Fe2O3 particle coating loaded on the surface of the steel substrate, and a soft metal coating covering the surface of the nano Fe2O3 particle coating; the nano Fe2O3 particle coating has a thickness of 0.1 to 1 μm and a porosity of 5 to 15%.

[0027] In the present invention, the particle size of the nano Fe2O3 particles is preferably 5 to 70 nm, more preferably 20 to 50 nm, and further preferably 30 to 40 nm. In the present invention, the thickness of the soft metal coating is preferably 2 to 6 μm, more preferably 3 to 5 μm. In the present invention, the soft metal in the soft metal coating preferably includes one of Ag, Mo, Cu and Al.

[0028] The present invention uses the nano Fe2O3 particle coating as an intermediate layer to improve the bonding force between the soft metal coating and the steel substrate, thereby improving the fretting fatigue life of the soft metal coating; during fretting, the nano Fe2O3 particles in the nano Fe2O3 particle coating can reduce the fretting wear of the wear-resistant material by rolling, and at the same time, the nano Fe2O3 and the soft metal coating can also play a lubricating role together during the fretting wear process, significantly reducing the fretting wear of the wear-resistant material. In addition, the present invention controls the thickness and porosity of the nano Fe2O3 particle coating so that during the wear process of applying positive stress, the soft metal in the soft metal coating is squeezed into the gap of the nano Fe2O3 particle coating, thereby achieving the wrapping and bonding of the nano Fe2O3 particles, protecting the highly brittle nano Fe2O3 particle coating from peeling off, thereby improving the fretting fatigue life of the wear material.

[0029] The present invention also provides a method for preparing the wear-resistant material described in the above scheme, comprising the following steps:

[0030] The steel substrate is subjected to sliding friction processing to generate an oxidation reaction to form a nano Fe2O3 particle coating; the positive pressure of the reciprocating sliding friction processing is 20-150N, and the processing area per unit time is 1-5mm 2 ;

[0031] Soft metal is deposited on the surface of the nano Fe2O3 particle coating by magnetron sputtering to form a soft metal coating to obtain a wear-resistant material.

[0032] The present invention performs sliding friction processing on the steel substrate, generates an oxidation reaction, and forms a nano Fe2O3 particle coating. In the present invention, the hardness of the processing head used for sliding friction processing is preferably 2000-3000HV, and more preferably 2500-2800HV. The present invention has no special requirements on the material of the processing head, and it can meet the hardness in the above range. Specifically, a cemented carbide processing head can be selected. In the present invention, the hardness of the steel substrate is preferably HRC30-HRC50, and more preferably HRC40-HRC45. In the present invention, the steel substrate preferably includes low carbon steel, medium carbon steel, high carbon steel or alloy steel, and the alloy steel is preferably 40CrNiMo; the structure of the steel substrate preferably includes one or more of tempered martensite, tempered troostite, tempered troostite, bainite and pearlite. In the present invention, the roughness of the steel substrate is preferably 0.2-1.2μm, and more preferably 0.4-0.6μm. In the present invention, before the steel matrix is ​​subjected to sliding friction processing, the raw material of the steel matrix is ​​preferably subjected to heat treatment, processing and grinding. The present invention has no special limitation on the heat treatment and processing, and the target structure and shape can be obtained by a method familiar to those skilled in the art. The present invention has no special limitation on the grinding, and the steel matrix can be processed to the target roughness by a process familiar to those skilled in the art. The present invention has no special limitation on the process for obtaining the steel matrix structure, and the process familiar to those skilled in the art can be used. Specifically, in an embodiment of the present invention, when the structure of the steel matrix is ​​tempered troostite, the acquisition method is: heat the 40CrNiMo steel material to 850°C and keep it warm for 40 minutes, take it out and cool it in quenching oil, and then temper it at 450°C, keep it warm for 2 hours and air cool it to obtain a steel matrix raw material with a structure of tempered troostite. When the structure of the steel matrix is ​​tempered martensite, the method for obtaining it is: heat-insulating low carbon steel or medium carbon steel at a temperature 30°C higher than the austenitizing temperature, tempering at 150°C to 250°C for 2h after oil quenching, and obtaining a steel matrix raw material with a structure of tempered martensite. When the structure of the steel matrix is ​​tempered bainite, the method for obtaining it is: heat-insulating medium carbon steel at a temperature 30°C higher than the austenitizing temperature, tempering at a temperature of 500°C to 650°C after oil quenching, and obtaining a steel matrix raw material with a structure of tempered bainite. When the structure of the steel matrix is ​​pearlite, the method for obtaining it is: heating high carbon steel to above the critical point to form austenite and then air cooling to obtain a steel matrix raw material with a structure of pearlite. When the structure of the steel matrix is ​​bainite, the obtaining method is: heating the bainite alloy steel to above the critical point to form austenite, and then air cooling or air cooling and isothermal treatment are performed to obtain a steel matrix raw material with a bainite structure.

[0033] In the present invention, the sliding friction processing is preferably a reciprocating sliding friction processing. In the present invention, the positive pressure of the sliding friction processing is 20N to 150N, preferably 40 to 100N, more preferably 50 to 70N; the processing area per unit time is 1 to 5mm 2 , more preferably 2 to 4 mm 2 The present invention controls the thickness of the Fe2O3 coating to 0.1 to 1 μm by controlling the positive pressure of the sliding friction processing and the processing area per unit time. In the present invention, the linear speed of the processing head in the sliding friction processing is preferably 30 to 300 mm / s, more preferably 40 to 200 mm / s, and further preferably 60 to 100 mm / s.

[0034] The present invention controls the hardness of the processing head and the steel substrate, the processing head linear speed and the normal pressure within the above range, which is conducive to large shear deformation of the steel substrate surface during the sliding friction process, so that a large number of dislocations are rapidly multiplied on the surface, and then the nano subcrystals on the steel substrate surface are transformed into large-angle nanocrystals, which is conducive to rapid and efficient oxidation of the nanocrystals at a relatively low temperature, thereby obtaining a nano Fe2O3 particle coating during the continued friction process. In the sliding friction process of the present invention, rapid friction micromachining generates heat, and when the instantaneous temperature reaches 200-400°C, an oxidation reaction will occur on the workpiece surface to generate Fe2O3. After the Fe2O3 is formed, continued sliding friction processing will cause these oxides to break and transform into nano iron oxide particles.

[0035] After forming the nano Fe2O3 particle coating, the present invention uses magnetron sputtering to deposit soft metal on the surface of the nano Fe2O3 particle coating to form a soft metal coating to obtain a wear-resistant material. In the present invention, the magnetron sputtering process preferably includes sequentially performing medium frequency magnetron sputtering and DC magnetron sputtering. In the present invention, the chamber pressure of the medium frequency magnetron sputtering and DC magnetron sputtering is preferably independently 0.4-0.5Pa, more preferably 0.45-0.48Pa, the bias voltage is preferably -100V, the current is preferably independently 12-15A, more preferably 13-14A, and the gas environment is preferably N2; the sputtering time of the medium frequency magnetron sputtering is preferably 20-30min, more preferably 25-28min, and the sputtering time of the DC magnetron sputtering is preferably 90-150min, more preferably 100-120min.

[0036] The present invention utilizes the sliding friction generated during surface-to-surface contact or point-to-surface contact by means of surface finishing micromachining to prepare a nano-Fe2O3 particle coating, and utilizes magnetron sputtering to prepare a soft metal layer on the surface of the nano-Fe2O3 particle coating. The preparation of the gradient coating meets the development requirements of high performance, low cost and environmental protection in the industry, and has a broad market space.

[0037] In order to further illustrate the present invention, the wear-resistant material and the preparation method thereof provided by the present invention are described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0038] Example 1

[0039] The 40CrNiMo steel material was heated to 850°C and kept at this temperature for 40 minutes, and then taken out and cooled in quenching oil. Then, it was tempered at 450°C, kept at this temperature for 2 hours, and air-cooled to obtain a steel matrix raw material with a structure of tempered troostite and a hardness of 43.2HRC.

[0040] The obtained steel matrix raw material is heat-treated and processed into parts, and the surface is finely ground to obtain a steel matrix with a roughness value of 0.3 μm (denoted as S1).

[0041] Use Figure 1 The friction micromachining process shown in the figure is to press a carbide-type machining head with a hardness of 2500 HV on the ground surface to perform reciprocating sliding friction micromachining to obtain a nano Fe2O3 particle coating. The friction positive pressure is 40N, the sliding speed is 40mm / s, and the wear scar length is 5mm.

[0042] Silver was plated on the nano-Fe2O3 particle coating to form a soft metal layer with a thickness of 5 μm to obtain a wear-resistant material (denoted as S3). Among them, the chamber pressure of the medium-frequency magnetron sputtering was 0.5 Pa, the bias voltage was -100 V, the current was 12 A, the gas environment was N2, and the sputtering time was 30 min; the chamber pressure of the DC magnetron sputtering was 0.5 Pa, the bias voltage was -100 V, the current was 12 A, the gas environment was N2, and the sputtering time was 90 min.

[0043] The nano-Fe2O3 particle coating of Example 1 was subjected to SEM analysis at different magnifications. The results are as follows: Figures 2-3 As shown. Among them, Figure 3 The inset in the figure shows the element content in the nano-Fe2O3 particle coating. Figures 2-3 It can be seen that the thickness of the nano-Fe2O3 particle coating is 1μm, and the particle size of the nano-Fe2O3 in the nano-Fe2O3 particle coating is 20-30nm. Figure 3 As can be seen from the illustration, the surface nano-oxide is iron oxide, and from the ratio of the iron and oxygen element contents, it can be judged that it is Fe2O3.

[0044] The present invention measures the porosity of the coating by observing the cross section of the oxide layer using an image analysis method: the average porosity of five random fields of view of 200-fold images is taken as the final porosity of the coating. The porosity of the nano-Fe2O3 particle coating of Example 1 is 5.29%.

[0045] Comparative Example 1

[0046] The 40CrNiMo steel material was heated to 850°C and kept at this temperature for 40 minutes, and then taken out and cooled in quenching oil. Then, it was tempered at 450°C, kept at this temperature for 2 hours, and air-cooled to obtain a steel matrix raw material with a structure of tempered troostite and a hardness of 43.2HRC.

[0047] The obtained steel matrix raw material is processed into parts after heat treatment and the surface is finely ground to obtain a steel matrix with a roughness value of 0.3 μm.

[0048] Silver was plated on the steel substrate to form a soft metal layer with a thickness of 5 μm to obtain a wear-resistant material (denoted as S2). The pressure in the chamber of the medium-frequency magnetron sputtering was 0.5 Pa, the bias voltage was -100 V, the current was 12 A, the gas environment was N2, and the sputtering time was 30 min; the pressure in the chamber of the DC magnetron sputtering was 0.5 Pa, the bias voltage was -100 V, the current was 12 A, the gas environment was N2, and the sputtering time was 90 min.

[0049] The steel substrate (marked as S1), the wear-resistant material of comparative example 1 (marked as S2) and the wear-resistant material of embodiment 1 (marked as S3) were subjected to a micro-motion wear test to test the friction coefficient and wear rate. The load was 600N and the time was 12h. The friction coefficients of S1 to S3 are as follows: Figure 4 As shown in Table 1, the wear rates of S1 to S3 are Figures 4-5 As shown in Table 1.

[0050] Table 1 Friction coefficient and wear rate of S1~S3

[0051] S1 S2 S3 Friction coefficient 0.089 0.074 0.111 Wear depth(μm) 13.27 11.421 5.07

[0052] Depend on Figures 4-5 As shown in Table 1, although the friction coefficients of S1, S2 and S3 are close, the wear depths vary significantly. The wear depth of S3 is 1 / 3 of that of S1, indicating that S3 has a higher fretting wear fatigue life.

[0053] SEM analysis of worn S3 at different magnifications was performed, and the results are as follows: Figures 6-7 As shown. Figures 6-7 It can be seen that the nano-oxide on the surface of the S3 sample still exists and has not fallen off.

[0054] EDS analysis was performed on the worn S3, and the results are as follows: Figure 8 As shown. Figure 8 It can be seen that after wear, Ag exists on the surface of the nano-Fe2O3 particle coating.

[0055] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A wear-resistant material, characterized in that: It comprises a steel substrate, a nano Fe2O3 particle coating loaded on the surface of the steel substrate, and a soft metal coating covering the surface of the nano Fe2O3 particle coating; the nano Fe2O3 particle coating has a thickness of 0.1 to 1 μm and a porosity of 5 to 15%; The particle size of the nano Fe2O3 particles is 5 to 70 nm; The thickness of the soft metal coating is 2 to 6 μm; The soft metal in the soft metal coating includes one of Ag, Mo, Cu and Al; The preparation method of the wear-resistant material comprises the following steps: The steel substrate is subjected to sliding friction processing to generate an oxidation reaction to form a nano Fe2O3 particle coating; the positive pressure of the sliding friction processing is 20 to 150 N, and the processing area per unit time is 1 to 5 mm 2 / min; Soft metal is deposited on the surface of the nano Fe2O3 particle coating by magnetron sputtering to form a soft metal coating to obtain the wear-resistant material.

2. The method for preparing the wear-resistant material according to claim 1, characterized in that: The following steps are involved: The steel substrate is subjected to sliding friction processing to generate an oxidation reaction to form a nano Fe2O3 particle coating; the positive pressure of the sliding friction processing is 20 to 150 N, and the processing area per unit time is 1 to 5 mm 2 / min; Soft metal is deposited on the surface of the nano Fe2O3 particle coating by magnetron sputtering to form a soft metal coating to obtain the wear-resistant material.

3. The preparation method according to claim 2, characterized in that: The hardness of the processing head used for sliding friction processing is 2000-3000 HV, and the hardness of the steel substrate is HRC30-HRC50.

4. The preparation method according to claim 2, characterized in that: The roughness of the steel substrate is 0.2-1.2 μm.

5. The preparation method according to claim 2 or 4, characterized in that: The structure of the steel matrix includes one or more of tempered martensite, tempered troostite, tempered troostite, bainite and pearlite.

6. The preparation method according to claim 2, characterized in that: The magnetron sputtering includes sequentially performing medium frequency magnetron sputtering and direct current magnetron sputtering.

7. The preparation method according to claim 6, characterized in that: The chamber pressure of the medium frequency magnetron sputtering and direct current magnetron sputtering is independently 0.4-0.5 Pa, the bias voltage is -100 V, the current is independently 12-15 A, and the gas environment is N2; the time of the medium frequency magnetron sputtering is 20-30 minutes, and the time of the direct current magnetron sputtering is 90-150 minutes.