One-way perspective film, one-way mirror, preparation method thereof and electronic device
By using a one-way perspective film composed of niobium pentoxide and silicon oxide layers in a single-way mirror, the problems of high coating cost and poor stability in the existing technology are solved, and low-cost, high-stability and diversified colors are achieved. The single-sided mirror meets market demand and is prepared by sputtering to reduce production costs.
Patent Information
- Application Number
- CN202110979363.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-08-25
AI Technical Summary
The silver, titanium, and titanium oxide coatings used in existing single-way mirrors are costly, have poor stability, and have a single color, making them unable to meet the diverse needs of the market.
A one-way perspective film composed of a first niobium pentoxide layer, a first silicon oxide layer, an absorption layer, a second niobium pentoxide layer, and a second silicon oxide layer is used. By adjusting the thickness and material combination of each layer, a film is formed. The anti-reflection layer and the anti-reflection layer achieve mirror and see-through effects, and are prepared by sputtering to reduce costs.
The low cost, high stability and diversified colors of single-sided mirrors are achieved to meet market demand, and good single-sided perspective effects and visual contrast are ensured by optimizing layer thickness and material combination.
Smart Images

Figure CN115728850B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of optical technology, and in particular to a one-way perspective film, a one-way mirror, a preparation method thereof, and an electronic device. Background Art
[0002] One-way mirror is a special coated glass, one side of which is a glass mirror (outer side), which can reflect light, and has a mirror effect similar to an ordinary mirror; while the other side (inner side) can see the scene outside the glass, which has a perspective effect, that is, the inside of the glass cannot be seen from the outside of the glass, but the situation outside the glass can be seen from the inside of the glass. One-way mirrors can be used in research rooms of university research institutions, large conference rooms and other places.
[0003] Currently, most one-way mirrors on the market use silver, titanium, and titanium oxide as coatings to form a one-way perspective effect. However, the above materials are not only expensive, but also have poor stability, which makes the coating easily ineffective. In addition, the existing one-way mirrors have a relatively single color, which does not meet people's diverse application needs. Therefore, it is necessary to provide a new one-way perspective film to improve the stability of the one-way mirror and make the one-way mirror have a variety of colors. Summary of the invention
[0004] In view of this, the present application provides a one-way perspective film, which has low production cost, stable performance, good one-way perspective effect, and various colors to meet market demand. The present application also provides a one-way mirror, a preparation method thereof, and an electronic device.
[0005] In a first aspect, the present application provides a one-way vision film, comprising a first niobium pentoxide layer, a first silicon oxide layer, an absorption layer, a second niobium pentoxide layer and a second silicon oxide layer arranged in sequence; the absorption layer has a thickness of 8nm-20nm.
[0006] The one-way perspective film of the present application forms a reflection-enhancing layer through the first niobium pentoxide layer and the first silicon oxide layer, so that the surface (R1 surface) of the one-way perspective film close to the first niobium pentoxide layer has a higher reflectivity, forming a mirror effect; the second niobium pentoxide layer and the second silicon oxide layer form an anti-reflection layer, so that the surface (R2 surface) of the one-way perspective film close to the second silicon oxide layer has a lower reflectivity, forming a perspective effect, and the absorption layer can absorb part of the light. When the thickness of the absorption layer is 8nm-20nm, it can be ensured that the R1 surface cannot see the R2 surface, and the R2 surface can see the R1 surface.
[0007] Optionally, the absorption layer includes one or more of silicon, indium, niobium, titanium and chromium.
[0008] Optionally, the thickness of the first niobium pentoxide layer and the second niobium pentoxide layer is 10 nm-120 nm.
[0009] Optionally, the thickness of the first silicon oxide layer and the second silicon oxide layer is 10 nm-160 nm.
[0010] Optionally, the first niobium pentoxide layer has a thickness of 30 nm-60 nm.
[0011] Optionally, the thickness of the first silicon oxide layer is 90nm-110nm.
[0012] Optionally, the second niobium pentoxide layer has a thickness of 60 nm-110 nm.
[0013] Optionally, the second silicon oxide layer has a thickness of 50nm-90nm.
[0014] Optionally, the visible light transmittance of the one-way perspective film is 10%-25%.
[0015] Optionally, the absolute value of the difference in visible light reflectivity between two side surfaces of the one-way perspective film is greater than or equal to 15%.
[0016] In a second aspect, the present application provides a one-way mirror, which includes a substrate and a one-way perspective film as described in the first aspect of the present application and arranged on a surface of the substrate.
[0017] Optionally, the substrate is disposed on the surface of the first niobium pentoxide layer.
[0018] Optionally, the substrate includes a transparent substrate, which includes one or more of glass, acrylic plate, explosion-proof film, release film, and polyethylene terephthalate (PET).
[0019] The one-way mirror provided in the second aspect of the present application has a good one-way perspective effect, is low in cost, has various colors, and has a wide range of applications.
[0020] In a third aspect, the present application provides a method for preparing a single-sided mirror, comprising:
[0021] A substrate is provided, and a first niobium pentoxide layer, a first silicon oxide layer, an absorption layer, a second niobium pentoxide layer and a second silicon oxide layer are sequentially deposited on the surface of the substrate to obtain the single-sided mirror; the absorption layer comprises one or more of silicon, indium, niobium, titanium and chromium; and the thickness of the absorption layer is 8nm-20nm.
[0022] In a fourth aspect, the present application provides an electronic device, comprising the one-way perspective film as described in the first aspect of the present application or the one-way mirror as described in the second aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1A schematic diagram of the structure of a one-way perspective film provided in one embodiment of the present application;
[0024] Figure 2 A schematic diagram of light transmission in a one-way perspective film provided in one embodiment of the present application;
[0025] Figure 3 A schematic diagram of the structure of a single-sided mirror provided in one embodiment of the present application;
[0026] Figure 4 This is a reflectivity test chart of the single-sided mirror R1 provided in Example 1 of the present application;
[0027] Figure 5 This is a transmittance test chart of the single-sided mirror R1 surface provided in Example 1 of the present application;
[0028] Figure 6 This is a reflectivity test chart of the single-sided mirror R2 surface provided in Example 1 of the present application;
[0029] Figure 7 This is a reflectivity test chart of the single-sided mirror R1 surface provided in Example 2 of the present application;
[0030] Figure 8 This is a transmittance test chart of the single-sided mirror R1 surface provided in Example 2 of the present application;
[0031] Fig. 9 This is a reflectivity test chart of the single-sided mirror R2 surface provided in Example 2 of the present application. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0033] See also Figure 1 , Figure 1 A schematic diagram of the structure of a one-way perspective film provided in an embodiment of the present application. The one-way perspective film comprises a first niobium pentoxide layer 11, a first silicon oxide layer 12, an absorption layer 13, a second niobium pentoxide layer 14, and a second silicon oxide layer 15 arranged in sequence. For ease of description, the outer side of the one-way perspective film in the present application refers to the side of the first niobium pentoxide layer 11; the inner side of the one-way perspective film refers to the side of the second silicon oxide layer 15.
[0034] In the present application, the outer surface (R1 surface) of the one-way perspective film is the first niobium pentoxide layer, and the light on the outer side does not produce half-wave loss when passing through the first niobium pentoxide layer to the first silicon oxide layer, so the reflection of light is enhanced, and the outer side of the one-way perspective film presents a mirror effect, and the inner surface (R2 surface) of the one-way perspective film is the second silicon oxide layer, and the light on the inner side produces half-wave loss when passing through the second silicon oxide layer to the second niobium pentoxide layer, thereby reducing the reflection of light, and the inner side of the one-way perspective film presents a perspective effect. The present application uses niobium pentoxide and silicon oxide to prepare the one-way perspective film, which greatly reduces the production cost and is conducive to the promotion of the product.
[0035] In the one-way perspective film of the present application, the absorption layer can absorb part of the light so that the transmittance of the one-way perspective film is within an appropriate range. In the embodiment of the present application, the absorption layer includes one or more of silicon, indium, niobium, titanium and chromium. In the embodiment of the present application, the thickness of the absorption layer is 8nm-20nm. Further, the thickness of the absorption layer is 15nm-20nm. The thickness of the absorption layer can be specifically but not limited to 8nm, 10nm, 12nm, 15nm, 17nm or 20nm. The greater the thickness of the absorption layer, the greater the amount of light absorbed, and the smaller the transmittance of the one-way perspective film, and the smaller the thickness of the absorption layer, the smaller the amount of light absorbed, and the greater the transmittance of the one-way perspective film. When the thickness of the absorption layer is 8nm-20nm, the absorption layer can have a good coordination effect with the first niobium pentoxide layer, the first silicon oxide layer, the second niobium pentoxide layer and the second silicon oxide layer, ensuring that the outer side of the one-way perspective film presents a mirror effect, while the inner side of the one-way perspective film presents a perspective effect. In the embodiment of the present application, the visible light transmittance of the one-way perspective film is 10%-25%. The visible light transmittance of the one-way perspective film may be, but is not limited to, 10%, 15%, 18%, 20%, 22%, or 25%.
[0036] In the embodiment of the present application, the thickness of the first niobium pentoxide layer and the second niobium pentoxide layer is 10nm-120nm. The thickness of the first niobium pentoxide layer and the second niobium pentoxide layer can be, but not limited to, 10nm, 30nm, 40nm, 50nm, 55nm, 60nm, 80nm, 90nm, 100nm or 120nm. In the embodiment of the present application, the thickness of the first silicon oxide layer and the second silicon oxide layer is 10nm-160nm. The thickness of the first silicon oxide layer and the second silicon oxide layer can be, but not limited to, 10nm, 30nm, 50nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm or 160nm. When the thickness of the first niobium pentoxide layer, the second niobium pentoxide layer, the first silicon oxide layer and the second silicon oxide layer is controlled within the above range, it can ensure that the one-way perspective film has good structural stability and is not easy to fall off, and the preparation cost of the one-way perspective film is low, which is conducive to the marketization of the product.
[0037] In the present application, by adjusting the thickness of the first niobium pentoxide layer, the first silicon oxide layer, the second niobium pentoxide layer and the second silicon oxide layer, the one-way perspective effect of the one-way perspective film can be optimized, the reflectivity of the outer side of the one-way perspective film can be enhanced and the reflectivity of the inner side of the one-way perspective film can be reduced, so as to achieve a good visual contrast effect of one side mirror surface and one side perspective surface. Figure 2 , Figure 2 A schematic diagram of light transmission in a one-way perspective film provided in one embodiment of the present application, wherein r1 is the amplitude reflection coefficient generated by the outer light at interface 1, r2 is the amplitude reflection coefficient generated by the outer light at interface 2, r3 is the amplitude reflection coefficient generated by the inner light at interface 2, and r4 is the amplitude reflection coefficient generated by the inner light at interface 1. The reflectivity of the one-way vision film at interface 1 is R1, and the reflectivity of the one-way vision film at interface 2 is R2, R1 = |r1-r2|, R2 = |r3-r4|, further, r1 = (N0-N1) / (N0+N1), r2 = (N1-N2) / (N1+N2)*e(-2δ), r3 = (N0-N2) / (N0+N2), r4 = (N2-N1) / (N1+N2)*e(-2δ), δ = 2π*N*D / λ, wherein N0 represents the refractive index of the incident medium, N1 represents the refractive index of silicon dioxide, N2 represents the refractive index of niobium pentoxide, δ represents the phase film thickness of the one-way vision film, D represents the physical film thickness of the one-way vision film, and λ represents the wavelength of light. When the optical path difference between the interfaces of each layer is an even multiple of a quarter wavelength, the reflection of the light can be increased, and when the optical path difference between the interfaces of each layer is an odd multiple of a quarter wavelength, the reflection of the light can be reduced.
[0038] According to the above formula and principle, the present application derives the optimized thickness relationship of the one-way perspective film. When the thickness of the first niobium pentoxide layer is 30nm-60nm and the thickness of the first silicon oxide layer is 90nm-110nm, the outer side of the one-way perspective film can have a higher reflectivity. When the thickness of the second niobium pentoxide layer is 60nm-110nm and the thickness of the second silicon oxide layer is 50nm-90nm, the inner side of the one-way perspective film can have a lower reflectivity. Further, the thickness ratio of the first niobium pentoxide layer to the first silicon oxide layer is 1:(1.5-3.5), and the thickness ratio of the second niobium pentoxide layer to the second silicon oxide layer is 1:(0.5-1.5). The thickness ratio of the first niobium pentoxide layer to the first silicon oxide layer can be, but not limited to, 1:1.5, 1:2, 1:2.5 or 1:3.5, and the thickness ratio of the second niobium pentoxide layer to the second silicon oxide layer can be, but not limited to, 1:0.5, 1:0.7, 1:1 or 1:1.5. In the embodiment of the present application, the absolute value of the difference in visible light reflectivity between the two sides of the one-way perspective film is greater than or equal to 15%, and the absolute value of the difference in visible light reflectivity between the two sides of the one-way perspective film may be, but is not limited to, 15%, 20%, 25%, 30%, 35% or 40%. The greater the difference in visible light reflectivity between the two sides of the one-way perspective film, the better the one-sided perspective effect and the more obvious the visual difference.
[0039] In the present application, the thickness relationship between the layers of the one-way perspective film will also affect the color of the film. Specifically, the reflectivity of the one-way perspective film to visible light can be changed by adjusting the thickness of each layer. Since the reflectivity of the one-way perspective film to light in different wavelength bands is also different, the one-way perspective film can present different colors.
[0040] This application also provides a one-way mirror, see Figure 3 , Figure 3 A schematic diagram of the structure of a one-way mirror provided in an embodiment of the present application, wherein the one-way mirror comprises a substrate 20 and a one-way perspective film 10 disposed on the surface of the substrate. In an embodiment of the present application, the substrate comprises a transparent substrate. In some embodiments of the present application, the substrate comprises one or more of glass and a polymer transparent substrate, wherein the polymer transparent substrate comprises one or more of polyethylene terephthalate (PET), an acrylic sheet, an explosion-proof film, and a release film. In the present application, the one-way perspective film can be disposed on any surface of the substrate. In some embodiments of the present application, the substrate is disposed on the outside (R1 surface) of the one-way perspective film, that is, the substrate is adjacent to the first niobium pentoxide layer in the one-way perspective film, and the above-mentioned position setting can ensure that the one-way mirror has a good one-way perspective effect.
[0041] The present application also provides a method for preparing a single-sided mirror, comprising the following steps:
[0042] A substrate is provided, and a first niobium pentoxide layer, a first silicon oxide layer, an absorption layer, a second niobium pentoxide layer and a second silicon oxide layer are sequentially deposited on the surface of the substrate to obtain a single-sided mirror.
[0043] In the embodiment of the present application, the first niobium pentoxide layer, the first silicon oxide layer, the absorption layer, the second niobium pentoxide layer and the second silicon oxide layer are prepared by sputtering. Specifically, the first niobium pentoxide layer and the second niobium pentoxide layer are prepared by introducing argon gas and oxygen into a sputtering machine, bombarding the niobium target with argon gas, and the sputtered niobium reacts with oxygen to form niobium pentoxide and is deposited to form a niobium pentoxide layer. The first silicon oxide layer and the second silicon oxide layer are prepared by introducing argon gas and oxygen into a sputtering machine, bombarding the silicon target with argon gas, and the sputtered silicon reacts with oxygen to form silicon oxide and is deposited to form a silicon oxide layer.
[0044] In the present application, the absorption layer includes one or more of silicon, indium, niobium, titanium and chromium, and the absorption layer is prepared by bombarding the corresponding target material with argon gas. For example, when the absorption layer is a silicon layer, the silicon layer is obtained by bombarding the silicon target with argon gas and depositing it simultaneously.
[0045] In some embodiments of the present application, the method for preparing the one-way mirror is as follows:
[0046] Providing a substrate, placing the substrate in a sputtering machine, and evacuating the chamber of the machine to a vacuum;
[0047] Introduce argon gas into the furnace chamber of the machine, turn on the ion source after the gas is stable, and perform ion cleaning on the surface of the substrate and target. The ICP power of the ion source is 0.5kw-5kw, and the vacuum degree of the furnace chamber of the machine is 1×10 -3 -1×10 -2 Pa, ion cleaning time is 1min-60min;
[0048] Continue to introduce argon gas, and start to introduce oxygen, the flow rate of oxygen is 200sccm-300sccm, turn on the sputtering power of the niobium target, the sputtering power is 5kw-15kw, the working pressure of the coating is 0.07Pa-1Pa, and a first niobium pentoxide layer is deposited on the surface of the substrate, and the thickness of the first niobium pentoxide layer is 10nm-120nm;
[0049] Turn off the sputtering power of the niobium target, continue to introduce argon and oxygen, turn on the sputtering power of the silicon target, the sputtering power is 5kw-15kw, the working pressure of the coating is 0.07Pa-1Pa, and a first silicon oxide layer is deposited on the surface of the first niobium pentoxide layer. The thickness of the first silicon oxide layer is 10nm-160nm;
[0050] Stop the oxygen supply, turn on the sputtering power of the absorption layer target, the sputtering power is 5kw-15kw, the working pressure of the coating is 0.07Pa-1Pa, and the absorption layer is deposited on the surface of the first silicon oxide layer, and the thickness of the absorption layer is 8nm-20nm;
[0051] Continue to introduce argon gas, and start to introduce oxygen, the flow rate of oxygen is 200sccm-300sccm, turn on the sputtering power of the niobium target, the sputtering power is 5kw-15kw, the working pressure of the coating is 0.07Pa-1Pa, and a second niobium pentoxide layer is deposited on the surface of the substrate, and the thickness of the second niobium pentoxide layer is 10nm-120nm;
[0052] Turn off the sputtering power of the niobium target, continue to introduce argon and oxygen, turn on the sputtering power of the silicon target, the sputtering power is 5kw-15kw, the working pressure of the coating is 0.07Pa-1Pa, and a second silicon oxide layer is deposited on the surface of the second niobium pentoxide layer. The thickness of the second silicon oxide layer is 10nm-160nm; then an atomic mirror is obtained.
[0053] The preparation method of the atomic mirror provided in the present application has a simple process and high production efficiency. The prepared atomic mirror has high structural stability and good single-sided perspective effect.
[0054] The present application also provides an electronic device, which includes the one-way perspective film or one-way mirror of the present application. In some embodiments of the present application, the electronic device includes a shell, and the shell includes a shell substrate and a one-way perspective film, wherein the shell substrate can provide a setting position and support for other structures of the electronic device, and the shell substrate can be a glass substrate or a polymer transparent substrate. The one-way perspective film is arranged on the surface of the shell substrate, and the side with a higher reflectivity of the one-way perspective film faces the outside of the shell as the appearance surface of the shell. Since the light outside the shell is strong and the reflectivity of the appearance surface of the shell is high, a mirror effect is presented on the appearance surface of the shell, thereby shielding the product structure inside the shell. Further, a light source can be arranged inside the shell, and the light source can be an LED lamp or an organic light-emitting material. By designing the shape of the light source and the color of the light, a specific pattern can be formed, such as a product logo or a decorative pattern, etc. Since the one-way mirror has a certain transmittance, when the light source inside the shell is strong enough, the pattern inside the shell can also be seen from the outside of the shell, but the non-luminous area inside the shell is still invisible, that is, the luminous pattern inside the shell can be seen from the appearance surface of the shell, but the non-luminous area inside the shell is still a mirror, thereby playing a magical decorative effect.
[0055] In some other embodiments of the present application, the electronic device includes a display screen assembly, the display screen assembly includes a display panel and a one-way perspective film, and the one-way perspective film is arranged on the surface of the display panel. The side of the one-way perspective film with higher reflectivity faces the outside of the display screen assembly. When the display screen is off, the display screen presents a mirror effect; when the display screen is on, the picture on the display screen can be displayed normally. Specifically, when the display screen assembly is not emitting light (off), the light on the outside of the one-way perspective film is brighter, so the reflection of light is stronger, and the surface of the display screen has a mirror effect. When the display screen is emitting light (on), the light on the inside of the one-way perspective film is brighter, so the light intensity transmitted by the display screen is high, and the content displayed on the display screen can be seen from the outside of the display screen, thereby achieving normal display when the display screen is on, and having a mirror decorative effect when the display screen is off.
[0056] In the implementation manner of the present application, the electronic device may specifically be a mobile phone, a computer, an electronic cigarette, a smart bracelet, a wearable device, etc.
[0057] The technical solution of the present application is further described below with reference to a number of embodiments.
[0058] Example 1
[0059] A method for preparing a single-sided mirror, comprising:
[0060] A glass substrate is provided, wherein the thickness of the glass substrate is 3 mm, the glass substrate is ultrasonically cleaned with ethanol, then rinsed with deionized water, and dried in a vacuum environment;
[0061] Place the glass substrate on the workpiece turntable of the sputtering machine and evacuate the machine to make the pressure in the working chamber lower than 0.003 Pa;
[0062] The ion source was turned on and argon gas was introduced at a flow rate of 280 sccm. Ion cleaning was performed on the surface of the glass substrate. The power of the ion source ICP was 0.7 kW. The vacuum degree was 0.8 Pa and the time was 5 min.
[0063] Continuously introduce argon gas, and start introducing oxygen, turn on the sputtering power of the niobium target, the sputtering power is 8 kW, and deposit the first niobium pentoxide layer on the surface of the glass substrate. The coating working pressure is 0.43 Pa, the coating time is 186 s, and the thickness of the first niobium pentoxide layer is 56 nm;
[0064] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power supply of the silicon target was turned on. The sputtering power supply power was 8 kW. The first silicon oxide layer was deposited on the surface of the first niobium pentoxide layer. The coating working pressure was 0.43 Pa. The coating time was 327 s. The thickness of the first silicon oxide layer was 105 nm.
[0065] The oxygen was turned off, the silicon target was kept on, the sputtering power was 8 kW, a silicon layer was deposited on the surface of the first silicon oxide layer, the coating working pressure was 0.26 Pa, the coating time was 182 s, and the thickness of the silicon layer was 18 nm;
[0066] The sputtering power of the silicon target was turned off, oxygen was introduced, and the sputtering power of the niobium target was turned on. The sputtering power was 8 kW, and the second niobium pentoxide layer was deposited on the surface of the silicon layer. The coating working pressure was 0.43 Pa, the coating time was 340 s, and the thickness of the second niobium pentoxide layer was 102 nm.
[0067] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8 kW. A second silicon oxide layer was deposited on the surface of the second niobium pentoxide layer. The coating working pressure was 0.43 Pa. The coating time was 183 s. The thickness of the second silicon oxide layer was 55 nm. A one-way perspective film was formed to obtain a one-way mirror. The structure of the one-way mirror was substrate / Nb2O5 (56 nm) / SiO2 (105 nm) / Si (18 nm) / Nb2O5 (102 nm) / SiO2 (55 nm).
[0068] Example 2
[0069] A method for preparing a single-sided mirror, comprising:
[0070] A glass substrate is provided, wherein the thickness of the glass substrate is 3 mm, the glass substrate is ultrasonically cleaned with ethanol, then rinsed with deionized water, and dried in a vacuum environment;
[0071] Place the glass substrate on the workpiece turntable of the sputtering machine and evacuate the machine to make the pressure in the working chamber lower than 0.003 Pa;
[0072] The ion source was turned on and argon gas was introduced at a flow rate of 280 sccm. Ion cleaning was performed on the surface of the glass substrate. The power of the ion source ICP was 0.7 kW. The vacuum degree was 0.8 Pa and the time was 5 min.
[0073] Continue to introduce argon gas, and start to introduce oxygen, turn on the sputtering power of the niobium target, the sputtering power is 8kw, and deposit the first niobium pentoxide layer on the surface of the glass substrate. The coating working pressure is 0.45Pa, the coating time is 106s, and the thickness of the first niobium pentoxide layer is 32nm;
[0074] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8 kW. The first silicon oxide layer was deposited on the surface of the first niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 316 s. The thickness of the first silicon oxide layer was 95 nm.
[0075] Turn off oxygen, turn on the indium target, set the sputtering power to 8 kW, deposit an indium layer on the surface of the first silicon oxide layer, the coating working pressure is 0.25 Pa, the coating time is 180 s, and the thickness of the indium layer is 18 nm;
[0076] The sputtering power of the indium target was turned off, oxygen was introduced, and the sputtering power of the niobium target was turned on. The sputtering power was 8 kW, and the second niobium pentoxide layer was deposited on the surface of the indium layer. The coating working pressure was 0.45 Pa, the coating time was 206 s, and the thickness of the second niobium pentoxide layer was 62 nm.
[0077] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8 kW. A second silicon oxide layer was deposited on the surface of the second niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 286 s. The thickness of the second silicon oxide layer was 86 nm. A one-way perspective film was formed to obtain a one-way mirror. The structure of the one-way mirror was substrate / Nb2O5 (32 nm) / SiO2 (95 nm) / In (18 nm) / Nb2O5 (62 nm) / SiO2 (86 nm).
[0078] Example 3
[0079] A method for preparing a single-sided mirror, comprising:
[0080] A glass substrate is provided, wherein the thickness of the glass substrate is 3 mm, the glass substrate is ultrasonically cleaned with ethanol, then rinsed with deionized water, and dried in a vacuum environment;
[0081] Place the glass substrate on the workpiece turntable of the sputtering machine and evacuate the machine to make the pressure in the working chamber lower than 0.003 Pa;
[0082] The ion source was turned on and argon gas was introduced at a flow rate of 280 sccm. Ion cleaning was performed on the surface of the glass substrate. The power of the ion source ICP was 0.7 kW. The vacuum degree was 0.8 Pa and the time was 5 min.
[0083] Continuously introduce argon gas, and start introducing oxygen, turn on the sputtering power of the niobium target, the sputtering power is 8kw, and deposit the first niobium pentoxide layer on the surface of the glass substrate. The coating working pressure is 0.45Pa, the coating time is 127s, and the thickness of the first niobium pentoxide layer is 38nm;
[0084] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power supply of the silicon target was turned on. The sputtering power supply power was 8 kW. The first silicon oxide layer was deposited on the surface of the first niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 326 s. The thickness of the first silicon oxide layer was 98 nm.
[0085] Turn off oxygen, turn on the niobium target, set the sputtering power to 5kw, deposit a niobium layer on the surface of the first silicon oxide layer, the coating working pressure is 0.45Pa, the coating time is 180s, and the thickness of the film layer is 18nm;
[0086] The sputtering power of the niobium target was turned off, oxygen was introduced, and the sputtering power of the niobium target was turned on. The sputtering power was 8 kW, and the second niobium pentoxide layer was deposited on the surface of the niobium layer. The coating working pressure was 0.45 Pa, the coating time was 217 s, and the thickness of the second niobium pentoxide layer was 65 nm.
[0087] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8 kW. A second silicon oxide layer was deposited on the surface of the second niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 206 s. The thickness of the second silicon oxide layer was 62 nm. A one-way perspective film was formed to obtain a one-way mirror. The structure of the one-way mirror was substrate / Nb2O5 (38 nm) / SiO2 (98 nm) / Nb (18 nm) / Nb2O5 (65 nm) / SiO2 (62 nm).
[0088] Example 4
[0089] A method for preparing a single-sided mirror, comprising:
[0090] A glass substrate is provided, wherein the thickness of the glass substrate is 3 mm, the glass substrate is ultrasonically cleaned with ethanol, then rinsed with deionized water, and dried in a vacuum environment;
[0091] Place the glass substrate on the workpiece turntable of the sputtering machine and evacuate the machine to make the pressure in the working chamber lower than 0.003 Pa;
[0092] The ion source was turned on and argon gas was introduced at a flow rate of 280 sccm. Ion cleaning was performed on the surface of the glass substrate. The power of the ion source ICP was 0.7 kW. The vacuum degree was 0.8 Pa and the time was 5 min.
[0093] Continue to introduce argon gas, and start to introduce oxygen, turn on the sputtering power of the niobium target, the sputtering power is 8kw, and deposit the first niobium pentoxide layer on the surface of the glass substrate. The coating working pressure is 0.45Pa, the coating time is 140s, and the thickness of the first niobium pentoxide layer is 42nm;
[0094] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power supply of the silicon target was turned on. The sputtering power supply power was 8 kW. The first silicon oxide layer was deposited on the surface of the first niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 340 s. The thickness of the first silicon oxide layer was 102 nm.
[0095] Turn off oxygen, turn on the niobium target, set the sputtering power to 5kw, deposit a niobium layer on the surface of the first silicon oxide layer, the coating working pressure is 0.45Pa, the coating time is 180s, and the thickness of the niobium layer is 18nm;
[0096] The sputtering power of the niobium target was turned off, oxygen was introduced, and the sputtering power of the niobium target was turned on. The sputtering power was 8 kW, and the second niobium pentoxide layer was deposited on the surface of the niobium layer. The coating working pressure was 0.45 Pa, the coating time was 233 s, and the thickness of the second niobium pentoxide layer was 70 nm.
[0097] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8 kW. A second silicon oxide layer was deposited on the surface of the second niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 233 s. The thickness of the second silicon oxide layer was 70 nm. A one-way perspective film was formed to obtain a one-way mirror. The structure of the one-way mirror was substrate / Nb2O5 (42 nm) / SiO2 (102 nm) / Nb (18 nm) / Nb2O5 (70 nm) / SiO2 (70 nm).
[0098] Example 5
[0099] A method for preparing a single-sided mirror, comprising:
[0100] A glass substrate is provided, wherein the thickness of the glass substrate is 3 mm, the glass substrate is ultrasonically cleaned with ethanol, then rinsed with deionized water, and dried in a vacuum environment;
[0101] Place the glass substrate on the workpiece turntable of the sputtering machine and evacuate the machine to make the pressure in the working chamber lower than 0.003 Pa;
[0102] The ion source was turned on and argon gas was introduced at a flow rate of 280 sccm. Ion cleaning was performed on the surface of the glass substrate. The power of the ion source ICP was 0.7 kW. The vacuum degree was 0.8 Pa and the time was 5 min.
[0103] Continue to introduce argon gas, and start to introduce oxygen, turn on the sputtering power of the niobium target, the sputtering power is 8kw, and deposit the first niobium pentoxide layer on the surface of the glass substrate. The coating working pressure is 0.45Pa, the coating time is 160s, and the thickness of the first niobium pentoxide layer is 48nm;
[0104] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8 kW. The first silicon oxide layer was deposited on the surface of the first niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 350 s. The thickness of the first silicon oxide layer was 105 nm.
[0105] Turn off oxygen, turn on the niobium target, set the sputtering power to 5kw, deposit a niobium layer on the surface of the first silicon oxide layer, the coating working pressure is 0.45Pa, the coating time is 180s, and the thickness of the niobium layer is 18nm;
[0106] The sputtering power of the niobium target was turned off, oxygen was introduced, and the sputtering power of the niobium target was turned on. The sputtering power was 8 kW, and the second niobium pentoxide layer was deposited on the surface of the niobium layer. The coating working pressure was 0.45 Pa, the coating time was 240 s, and the thickness of the second niobium pentoxide layer was 72 nm.
[0107] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8 kW. A second silicon oxide layer was deposited on the surface of the second niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 273 s. The thickness of the second silicon oxide layer was 82 nm. A one-way perspective film was formed to obtain a one-way mirror. The structure of the one-way mirror was substrate / Nb2O5 (48 nm) / SiO2 (105 nm) / Nb (18 nm) / Nb2O5 (72 nm) / SiO2 (82 nm).
[0108] Example 6
[0109] A method for preparing a single-sided mirror, comprising:
[0110] A glass substrate is provided, wherein the thickness of the glass substrate is 3 mm, the glass substrate is ultrasonically cleaned with ethanol, then rinsed with deionized water, and dried in a vacuum environment;
[0111] Place the glass substrate on the workpiece turntable of the sputtering machine and evacuate the machine to make the pressure in the working chamber lower than 0.003 Pa;
[0112] The ion source was turned on and argon gas was introduced at a flow rate of 280 sccm. Ion cleaning was performed on the surface of the glass substrate. The power of the ion source ICP was 0.7 kW. The vacuum degree was 0.8 Pa and the time was 5 min.
[0113] Continue to introduce argon gas, and start to introduce oxygen, turn on the sputtering power of the niobium target, the sputtering power is 8kw, and deposit the first niobium pentoxide layer on the surface of the glass substrate. The coating working pressure is 0.45Pa, the coating time is 106s, and the thickness of the first niobium pentoxide layer is 32nm;
[0114] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power supply of the silicon target was turned on. The sputtering power supply power was 8 kW. The first silicon oxide layer was deposited on the surface of the first niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 316 s. The thickness of the first silicon oxide layer was 92 nm.
[0115] Turn off oxygen, turn on the titanium target, set the sputtering power to 5 kW, deposit a titanium layer on the surface of the first silicon oxide layer, the coating working pressure is 0.45 Pa, the coating time is 150 s, and the thickness of the titanium layer is 15 nm;
[0116] The sputtering power of the titanium target was turned off, oxygen was introduced, and the sputtering power of the niobium target was turned on. The sputtering power was 8 kW, and the second niobium pentoxide layer was deposited on the surface of the niobium layer. The coating working pressure was 0.45 Pa, the coating time was 233 s, and the thickness of the second niobium pentoxide layer was 70 nm.
[0117] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8 kW. A second silicon oxide layer was deposited on the surface of the second niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 273 s. The thickness of the second silicon oxide layer was 85 nm. A one-way perspective film was formed to obtain a one-way mirror. The structure of the one-way mirror was substrate / Nb2O5 (32 nm) / SiO2 (92 nm) / Ti (15 nm) / Nb2O5 (70 nm) / SiO2 (85 nm).
[0118] Example 7
[0119] A method for preparing a single-sided mirror, comprising:
[0120] A glass substrate is provided, wherein the thickness of the glass substrate is 3 mm, the glass substrate is ultrasonically cleaned with ethanol, then rinsed with deionized water, and dried in a vacuum environment;
[0121] Place the glass substrate on the workpiece turntable of the sputtering machine and evacuate the machine to make the pressure in the working chamber lower than 0.003 Pa;
[0122] The ion source was turned on and argon gas was introduced at a flow rate of 280 sccm. Ion cleaning was performed on the surface of the glass substrate. The power of the ion source ICP was 0.7 kW. The vacuum degree was 0.8 Pa and the time was 5 min.
[0123] Continue to introduce argon gas, and start to introduce oxygen, turn on the sputtering power of the niobium target, the sputtering power is 8kw, and deposit the first niobium pentoxide layer on the surface of the glass substrate. The coating working pressure is 0.45Pa, the coating time is 160s, and the thickness of the first niobium pentoxide layer is 48nm;
[0124] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8 kW. The first silicon oxide layer was deposited on the surface of the first niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 350 s. The thickness of the first silicon oxide layer was 102 nm.
[0125] The oxygen was turned off, the chromium target was turned on, the sputtering power was 5 kW, a chromium layer was deposited on the surface of the first silicon oxide layer, the coating working pressure was 0.45 Pa, the coating time was 100 s, and the thickness of the chromium layer was 10 nm;
[0126] The sputtering power of the chromium target was turned off, oxygen was introduced, and the sputtering power of the niobium target was turned on. The sputtering power was 8 kW, and the second niobium pentoxide layer was deposited on the surface of the niobium layer. The coating working pressure was 0.45 Pa, the coating time was 206 s, and the thickness of the second niobium pentoxide layer was 62 nm.
[0127] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8 kW. A second silicon oxide layer was deposited on the surface of the second niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 286 s. The thickness of the second silicon oxide layer was 86 nm. A one-way perspective film was formed to obtain a one-way mirror. The structure of the one-way mirror was substrate / Nb2O5 (48 nm) / SiO2 (102 nm) / Cr (10 nm) / Nb2O5 (62 nm) / SiO2 (86 nm).
[0128] Example 8
[0129] A method for preparing a single-sided mirror, comprising:
[0130] A glass substrate is provided, wherein the thickness of the glass substrate is 3 mm, the glass substrate is ultrasonically cleaned with ethanol, then rinsed with deionized water, and dried in a vacuum environment;
[0131] Place the glass substrate on the workpiece turntable of the sputtering machine and evacuate the machine to make the pressure in the working chamber lower than 0.003 Pa;
[0132] The ion source was turned on and argon gas was introduced at a flow rate of 280 sccm. Ion cleaning was performed on the surface of the glass substrate. The power of the ion source ICP was 0.7 kW. The vacuum degree was 0.8 Pa and the time was 5 min.
[0133] Continuously introduce argon gas, and start introducing oxygen, turn on the sputtering power of the niobium target, the sputtering power is 8kw, and deposit the first niobium pentoxide layer on the surface of the glass substrate. The coating working pressure is 0.45Pa, the coating time is 231s, and the thickness of the first niobium pentoxide layer is 72nm;
[0134] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8 kW. The first silicon oxide layer was deposited on the surface of the first niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 289 s. The thickness of the first silicon oxide layer was 86 nm.
[0135] Turn off oxygen, turn on the silicon target, set the sputtering power to 5 kW, deposit a silicon layer on the surface of the first silicon oxide layer, set the coating working pressure to 0.45 Pa, set the coating time to 200 s, and set the thickness of the silicon layer to 20 nm;
[0136] The sputtering power of the silicon target was turned off, oxygen was introduced, and the sputtering power of the niobium target was turned on. The sputtering power was 8 kW, and the second niobium pentoxide layer was deposited on the surface of the niobium layer. The coating working pressure was 0.45 Pa, the coating time was 240 s, and the thickness of the second niobium pentoxide layer was 72 nm.
[0137] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8 kW. A second silicon oxide layer was deposited on the surface of the second niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 273 s. The thickness of the second silicon oxide layer was 82 nm. A one-way perspective film was formed to obtain a one-way mirror. The structure of the one-way mirror was substrate / Nb2O5 (72 nm) / SiO2 (86 nm) / Si (20 nm) / Nb2O5 (72 nm) / SiO2 (82 nm).
[0138] Example 9
[0139] A method for preparing a single-sided mirror, comprising:
[0140] A glass substrate is provided, wherein the thickness of the glass substrate is 3 mm, the glass substrate is ultrasonically cleaned with ethanol, then rinsed with deionized water, and dried in a vacuum environment;
[0141] Place the glass substrate on the workpiece turntable of the sputtering machine and evacuate the machine to make the pressure in the working chamber lower than 0.003 Pa;
[0142] The ion source was turned on and argon gas was introduced at a flow rate of 280 sccm. Ion cleaning was performed on the surface of the glass substrate. The power of the ion source ICP was 0.7 kW. The vacuum degree was 0.8 Pa and the time was 5 min.
[0143] Argon gas was continuously introduced, and oxygen was started to be introduced, and the sputtering power of the niobium target was turned on. The sputtering power was 8 kW, and the first niobium pentoxide layer was deposited on the surface of the glass substrate. The coating working pressure was 0.45 Pa, the coating time was 173 s, and the thickness of the first niobium pentoxide layer was 52 nm.
[0144] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power supply of the silicon target was turned on. The sputtering power supply power was 8 kW. The first silicon oxide layer was deposited on the surface of the first niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 310 s. The thickness of the first silicon oxide layer was 93 nm.
[0145] Turn off oxygen, turn on the indium target, set the sputtering power to 5 kW, deposit an indium layer on the surface of the first silicon oxide layer, set the coating working pressure to 0.45 Pa, set the coating time to 150 s, and set the thickness of the indium layer to 15 nm;
[0146] The sputtering power of the indium target was turned off, oxygen was introduced, and the sputtering power of the niobium target was turned on. The sputtering power was 8 kW, and the second niobium pentoxide layer was deposited on the surface of the niobium layer. The coating working pressure was 0.45 Pa, the coating time was 140 s, and the thickness of the second niobium pentoxide layer was 42 nm.
[0147] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8kw, and a second silicon oxide layer was deposited on the surface of the second niobium pentoxide layer. The coating working pressure was 0.45Pa, and the coating time was 263s. The thickness of the second silicon oxide layer was 82nm, forming a one-way perspective film to obtain a one-way mirror. The structure of the one-way mirror was substrate / Nb2O5 (52nm) / SiO2 (93nm) / In (15nm) / Nb2O5 (42nm) / SiO2 (82nm).
[0148] Example 10
[0149] A method for preparing a single-sided mirror, comprising:
[0150] A glass substrate is provided, wherein the thickness of the glass substrate is 3 mm, the glass substrate is ultrasonically cleaned with ethanol, then rinsed with deionized water, and dried in a vacuum environment;
[0151] Place the glass substrate on the workpiece turntable of the sputtering machine and evacuate the machine to make the pressure in the working chamber lower than 0.003 Pa;
[0152] The ion source was turned on and argon gas was introduced at a flow rate of 280 sccm. Ion cleaning was performed on the surface of the glass substrate. The power of the ion source ICP was 0.7 kW. The vacuum degree was 0.8 Pa and the time was 5 min.
[0153] Continuously introduce argon gas, and start introducing oxygen, turn on the sputtering power of the niobium target, the sputtering power is 8kw, and deposit the first niobium pentoxide layer on the surface of the glass substrate. The coating working pressure is 0.45Pa, the coating time is 133s, and the thickness of the first niobium pentoxide layer is 25nm;
[0154] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power supply of the silicon target was turned on. The sputtering power supply power was 8 kW. The first silicon oxide layer was deposited on the surface of the first niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 340 s. The thickness of the first silicon oxide layer was 102 nm.
[0155] Turn off oxygen, turn on the chromium target, set the sputtering power to 5 kW, deposit a chromium layer on the surface of the first silicon oxide layer, the coating working pressure is 0.45 Pa, the coating time is 150 s, and the thickness of the chromium layer is 15 nm;
[0156] The sputtering power of the chromium target was turned off, oxygen was introduced, and the sputtering power of the niobium target was turned on. The sputtering power was 8 kW, and the second niobium pentoxide layer was deposited on the surface of the niobium layer. The coating working pressure was 0.45 Pa, the coating time was 240 s, and the thickness of the second niobium pentoxide layer was 72 nm.
[0157] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8 kW. A second silicon oxide layer was deposited on the surface of the second niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 263 s. The thickness of the second silicon oxide layer was 82 nm. A one-way perspective film was formed to obtain a one-way mirror. The structure of the one-way mirror was substrate / Nb2O5 (25 nm) / SiO2 (102 nm) / Cr (15 nm) / Nb2O5 (72 nm) / SiO2 (82 nm).
[0158] Embodiment 11
[0159] A method for preparing a single-sided mirror, comprising:
[0160] A glass substrate is provided, wherein the thickness of the glass substrate is 3 mm, the glass substrate is ultrasonically cleaned with ethanol, then rinsed with deionized water, and dried in a vacuum environment;
[0161] Place the glass substrate on the workpiece turntable of the sputtering machine and evacuate the machine to make the pressure in the working chamber lower than 0.003 Pa;
[0162] The ion source was turned on and argon gas was introduced at a flow rate of 280 sccm. Ion cleaning was performed on the surface of the glass substrate. The power of the ion source ICP was 0.7 kW. The vacuum degree was 0.8 Pa and the time was 5 min.
[0163] Continuously introduce argon gas, and start introducing oxygen, turn on the sputtering power of the niobium target, the sputtering power is 8kw, and deposit the first niobium pentoxide layer on the surface of the glass substrate. The coating working pressure is 0.45Pa, the coating time is 127s, and the thickness of the first niobium pentoxide layer is 38nm;
[0164] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power supply of the silicon target was turned on. The sputtering power supply power was 8 kW. The first silicon oxide layer was deposited on the surface of the first niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 326 s. The thickness of the first silicon oxide layer was 98 nm.
[0165] Turn off oxygen, turn on the niobium target, set the sputtering power to 5kw, deposit a niobium layer on the surface of the first silicon oxide layer, the coating working pressure is 0.45Pa, the coating time is 180s, and the thickness of the niobium layer is 18nm;
[0166] The sputtering power of the niobium target was turned off, oxygen was introduced, and the sputtering power of the niobium target was turned on. The sputtering power was 8 kW, and the second niobium pentoxide layer was deposited on the surface of the niobium layer. The coating working pressure was 0.45 Pa, the coating time was 340 s, and the thickness of the second niobium pentoxide layer was 102 nm.
[0167] The niobium target was turned off, the gas source was continuously supplied, and the sputtering power of the silicon target was turned on. The sputtering power was 8 kW. A second silicon oxide layer was deposited on the surface of the second niobium pentoxide layer. The coating working pressure was 0.45 Pa. The coating time was 143 s. The thickness of the second silicon oxide layer was 42 nm. A one-way perspective film was formed to obtain a one-way mirror. The structure of the one-way mirror was substrate / Nb2O5 (38 nm) / SiO2 (98 nm) / Nb (18 nm) / Nb2O5 (102 nm) / SiO2 (42 nm).
[0168] In order to highlight the beneficial effects of the present application, the following comparative examples are set.
[0169] Comparative Example 1
[0170] The difference between Comparative Example 1 and Example 1 is that the deposition conditions of the silicon layer in Comparative Example 1 are: turn off the oxygen, keep the silicon target on, the sputtering power is 8kw, the silicon layer is deposited on the surface of the first silicon oxide layer, the coating working pressure is 0.45Pa, the coating time is 600s, the thickness of the silicon layer is 68nm, and a film layer is formed to obtain coated glass. The structure of the coated glass is substrate / Nb2O5 (56nm) / SiO2 (105nm) / Si (68nm) / Nb2O5 (102nm) / SiO2 (55nm).
[0171] Comparative Example 2
[0172] The difference between Comparative Example 2 and Example 1 is that the deposition conditions of the silicon layer in Comparative Example 2 are: turn off the oxygen, keep the silicon target on, the sputtering power is 8kw, the silicon layer is deposited on the surface of the first silicon oxide layer, the coating working pressure is 0.45Pa, the coating time is 60s, the thickness of the silicon layer is 5nm, and a film layer is formed to obtain coated glass with a structure of substrate / Nb2O5(56nm) / SiO2(105nm) / Si(5nm) / Nb2O5(102nm) / SiO2(55nm).
[0173] Effect Example
[0174] In order to verify the performance of the one-way mirror produced in the present application, the present application also provides an effect embodiment.
[0175] 1) The reflectivity and transmittance of the single-sided mirrors of Examples 1-11 and the coated glass of Comparative Examples 1-2 were tested by a spectrophotometer. The test equipment used was an X-rite Color I5 spectrophotometer. The test parameters were as follows: repeatability: 0.03RMS CIELab; light source: pulsed xenon lamp, calibrated D65; spectral range: 360-750nm; wavelength interval: 10nm; reflection aperture: 25mm / 10mm / 6mm; total transmission aperture: 22mm / 10mm / 6mm; photometric range: 0-200% reflectivity; photometric resolution: 0.01%, measurement time: 2.5s. During the test, the side of the single-sided mirror close to the glass substrate was the R1 side, and the other side was the R2 side.
[0176] See also Figure 4-Figure 6 ,in, Figure 4 This is a reflectivity test chart of the single-sided mirror R1 provided in Example 1 of the present application; Figure 5 This is a transmittance test chart of the single-sided mirror R1 surface provided in Example 1 of the present application; Figure 6 This is a reflectivity test chart of the single-sided mirror R2 provided in Example 1 of the present application. Figure 4-Figure 6 The test results are as follows: the full-band reflectivity or transmittance of each surface of the single-sided mirror is averaged, and the average reflectivity of the R1 surface of the single-sided mirror in Example 1 is 42.8%, the average reflectivity of the R2 surface is 21.6%, and the average transmittance of the single-sided mirror is 15.6%. Please refer to Figure 7-Figure 9 ,in, Figure 7 This is a reflectivity test chart of the single-sided mirror R1 surface provided in Example 2 of the present application; Figure 8 This is a transmittance test chart of the single-sided mirror R1 surface provided in Example 2 of the present application; Fig. 9 This is a reflectivity test chart of the single-sided mirror R2 provided in Example 2 of the present application. Figure 7-Figure 9 The test results of the single-sided mirror were averaged, and the average reflectivity or transmittance of the full-band reflectivity or transmittance of each surface of the single-sided mirror was averaged. It was found that the average reflectivity of the R1 surface of the single-sided mirror of Example 2 was 52.6%, the average reflectivity of the R2 surface was 15.6%, and the average transmittance of the single-sided mirror was 19.9%. The same method was used to test the reflectivity and transmittance of the single-sided mirrors of Examples 3-11 and the coated glass of Comparative Examples 1-2. Please refer to Table 1 for the test results of the transmittance and reflectivity of the single-sided mirrors of Examples 1-11 and the coated glass of Comparative Examples 1-2.
[0177] Table 1 Optical parameters of the single-sided mirrors of Examples 1-11 and the coated glass of Comparative Examples 1-2
[0178]
[0179]
[0180] As can be seen from Table 1, the single-sided mirror R1 surface provided in the embodiment of the present application has a higher reflectivity, and the R2 surface has a lower reflectivity. Under the coordination of the transmittance, it can be ensured that the single-sided mirror R1 surface presents a mirror effect, while the R2 surface presents a perspective effect, thereby achieving a good single-sided perspective effect. However, in Comparative Example 1, since the transmittance of the coated glass is too low, the R1 surface and the R2 surface of the coated glass do not have a perspective effect; in Comparative Example 2, since the transmittance of the coated glass is too high, the R1 surface and the R2 surface of the coated glass both have a perspective effect.
[0181] 2) The chromaticity [Lab (CIE)] of the single-sided mirror of Examples 1-11 was tested using a chromaticity tester, wherein L represents the lightness index, A represents the red-green color index, and b represents the yellow-blue color index. The chromaticity values of the single-sided mirror of Examples 1-11 are shown in Table 2.
[0182] Table 2 Color parameter table of single-sided mirror of Examples 1-11
[0183]
[0184]
[0185] It can be seen from Table 2 that the one-way perspective film provided in the present application can present different colors, achieve diverse appearance effects, and meet market demand.
[0186] 3) The adhesion of the one-way perspective film in the one-way mirror of Examples 1-11 was tested using a hundred-grid adhesion method, and the testing method included:
[0187] a. Use a grating knife (blade angle is 15°-30°) to cut the surface of the one-way vision film ≥ 10mm 2 Draw 10×10 1mm×1mm grids in the place where the film is placed, and each line should be deep enough to reach the bottom layer of the one-way vision film;
[0188] b. Use a brush to clean the debris in the test area;
[0189] c. Adhesion force 350g / cm 2 ~400g / cm 2 Use adhesive tape (3M No. 600 or equivalent) to firmly stick the small network to be tested, and use an eraser to rub the tape vigorously to increase the contact area and strength between the tape and the tested area;
[0190] d. Grab one end of the tape and quickly tear it off at 90 degrees. Perform the same test twice at the same location to observe the peeling of the one-way vision film and classify it as follows:
[0191] 5B: The mesh has no peeling;
[0192] 4B: The area of the peeled portion is no more than 5% of the area of the tape in contact with the surface;
[0193] 3B: The area of the peeled portion is greater than 5% of the area of the tape in contact with the surface, but not more than 15%;
[0194] 2B: The area of the peeled portion is greater than 15% of the area of the tape in contact with the surface, but not more than 35%;
[0195] 1B: The area of the peeled portion is greater than 35% and not more than 65% of the area of the tape in contact with the surface;
[0196] 0B: The area of the peeled portion is greater than 65% of the area of the tape in contact with the surface;
[0197] The adhesion test results of the single-sided mirrors of Examples 1-11 are shown in Table 3.
[0198] Table 3 Adhesion test results of one-way perspective films of Examples 1-11
[0199]
[0200]
[0201] It can be seen from Table 3 that the one-way perspective film provided in the present application has a relatively high bonding force to the substrate, and the problem of film layer falling off is not likely to occur.
[0202] The above is a preferred embodiment of the present application, but it should not be understood as limiting the scope of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application, and these improvements and modifications are also considered to be within the scope of protection of the present application.
Claims
1. A one-way perspective film, It is characterized in that It comprises a first niobium pentoxide layer, a first silicon oxide layer, an absorption layer, a second niobium pentoxide layer and a second silicon oxide layer which are arranged in sequence; the absorption layer has a thickness of 8nm-20nm, the absorption layer comprises one or more of silicon, indium, niobium, titanium and chromium, the first niobium pentoxide layer has a thickness of 30nm-60nm; the first silicon oxide layer has a thickness of 90nm-110nm; the second niobium pentoxide layer has a thickness of 60nm-110nm; the second silicon oxide layer has a thickness of 50nm-90nm.
2. The one-way vision film according to claim 1, It is characterized in that The thickness ratio of the first niobium pentoxide layer to the first silicon oxide layer is 1:(1.5-3.5).
3. The one-way vision film according to claim 1, It is characterized in that The thickness ratio of the second niobium pentoxide layer to the second silicon oxide layer is 1:(0.5-1.5).
4. The one-way vision film according to claim 1, It is characterized in that The visible light transmittance of the one-way perspective film is 10%-25%.
5. The one-way vision film according to claim 1, It is characterized in that The absolute value of the difference in visible light reflectivity between the two side surfaces of the one-way perspective film is greater than or equal to 15%.
6. A one-way mirror, It is characterized in that The one-way mirror comprises a substrate and the one-way perspective film according to claim 1 arranged on a surface of the substrate.
7. The one-way mirror according to claim 6, It is characterized in that The substrate is disposed on a surface of the first niobium pentoxide layer away from the first silicon oxide layer.
8. A method for preparing a single-sided mirror as claimed in any one of claims 6 to 7, It is characterized in that include: A substrate is provided, and a first niobium pentoxide layer, a first silicon oxide layer, an absorption layer, a second niobium pentoxide layer and a second silicon oxide layer are sequentially deposited on the surface of the substrate to obtain the single-sided mirror; the absorption layer comprises one or more of silicon, indium, niobium, titanium and chromium; and the thickness of the absorption layer is 8nm-20nm.
9. An electronic device, It is characterized in that The electronic device comprises the one-way perspective film as claimed in any one of claims 1 to 5 or the one-way mirror as claimed in claim 6 or 7.
Citation Information
Patent Citations
One-way transparent glass film
CN106827742A
One -way perspective insulates against heat and prevents impression of hand glass door