Positive electrode additive, positive electrode sheet and lithium-ion battery

By using LixH2-xC2O4 as a cathode additive in lithium-ion batteries, the problem of high decomposition voltage of lithium oxalate is solved, and high lithium replenishment capacity and stability are achieved at low voltage. It is suitable for a variety of lithium-ion battery systems and improves Battery cycle performance and energy density.

CN115732689BActive Publication Date: 2024-10-29SHENZHEN BYD LITHIUM BATTERY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202111011831.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-31
Publication Date
2024-10-29
Estimated Expiration
2041-08-31

AI Technical Summary

Technical Problem

When lithium oxalate is used as a lithium replenishing agent in existing lithium-ion batteries, the decomposition voltage is higher than the charging cut-off voltage of common cathode materials, resulting in an unstable structure of the battery's cathode active material and affecting cycle performance. It is especially unsuitable for low-voltage lithium-ion battery systems.

Method used

Using LixH2-xC2O4 as the cathode additive, part of Li is replaced by H to form vacancy defects, reduce the decomposition and lithium potential, ensure the release of active lithium at a lower voltage, avoid irreversible damage to the cathode active material, and control the particle size to 50nm -20μm range to improve decomposition speed and stability.

Benefits of technology

It achieves high lithium replenishment capacity under low decomposition voltage, takes into account the structural stability and cycle performance of the battery, is suitable for a variety of lithium-ion battery systems, and improves the energy density and cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115732689B_ABST
    Figure CN115732689B_ABST
Patent Text Reader

Abstract

The present application provides a positive electrode additive, the general formula of which is Li x H 2‑x C2O4, where x is in the range of 0<x<2. In this cathode additive, part of Li is replaced by H, which escapes at a lower voltage to generate vacancy defects, which is beneficial to reduce Li x H 2‑x The decomposition and delithiation potential of the C2O4 material avoids the irreversible damage to the structure of the positive electrode active material of the battery caused by using a higher decomposition voltage to delithiate the material. The present application also provides a positive electrode sheet and a lithium ion battery containing the positive electrode additive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to positive electrode additives, positive electrode sheets and lithium-ion batteries. Background Art

[0002] With the development of economy and technology, portable electronic devices (mobile phones, tablets, etc.), drones, electric vehicles and other industries are in urgent need of energy storage devices with longer cycle life. In order to make lithium-ion batteries, an energy storage device, meet the above requirements, the industry usually takes the measure of pre-adding lithium replenishers that can provide active lithium to the lithium-ion battery system to make up for the irreversible loss of active lithium by the negative electrode of the battery. Lithium oxalate is a lithium-rich material, but its decomposition voltage to produce active lithium ions is above 4.7V, which is higher than the charging cut-off voltage of common ternary positive electrode active materials. Therefore, it is not suitable as a positive electrode lithium replenisher for batteries, especially for low-voltage lithium-ion battery systems such as ternary batteries. Otherwise, it will seriously affect the structural stability of the positive electrode active materials of the battery and reduce the cycle performance of the battery. Summary of the invention

[0003] In view of this, the present application provides a new cathode additive Li x H 2-x C2O4 can release active lithium at a lower decomposition voltage, avoiding the irreversible damage to the structure of the active material of the battery positive electrode caused by using a higher decomposition voltage.

[0004] In the first aspect, the present application provides a positive electrode additive, the general formula of which can be Li x H 2-x C2O4, where the value range of x is: 0<x<2.

[0005] Compared with Li2C2O4, Li x H 2-x Part of the Li in C2O4 material is replaced by H, which escapes at a lower voltage to produce vacancy defects, which are beneficial to reduce the Li x H 2-x The decomposition and delithiation potential of C2O4 material, therefore, the material may have a lower decomposition and delithiation potential and is suitable for use as a positive electrode lithium supplement for batteries.

[0006] In this application, x cannot be equal to 2, otherwise Li x H 2-x C2O4 is lithium oxalate. Although its theoretical mass specific capacity can reach 526 mAh / g, its decomposition potential is high and its compatibility with the charging cut-off voltage of conventional batteries is poor. x H 2-xIn C2O4 materials, the role of H is to reduce the decomposition and delithiation potential of the material, but it does not participate in providing active lithium ions to the negative electrode. When the value of x is small, the proportion of H that can form defect vacancies is high, and Li x H 2-x The decomposition potential of C2O4 material is reduced, which is compatible with the charging cut-off voltage of conventional batteries and can be used as a lithium supplement in many common battery systems.

[0007] In some embodiments of the present application, the value range of x is controlled to be: 0.5≤x≤1.9. x can be 0.5, 0.6, 0.8, 1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8 or 1.9, etc. At this time, the positive electrode additive can have both a lower lithium replenishment voltage and a higher lithium replenishment capacity. When x is within this range, the presence of H ensures that Li x H 2-x The decomposition potential of C2O4 material is not higher than 4.6V (for example, 4.4-4.6V). Charging the battery above this decomposition voltage will not have a serious impact on the structure of the positive electrode active material, will not significantly deteriorate the cycle performance of the battery, and can simultaneously ensure the Li x H 2-x C2O4 material has a higher specific capacity for lithium replenishment, achieving a better lithium replenishment effect. In some embodiments, the value range of x is: 1.2≤x≤1.9. Preferably, the value range of x is: 1.5≤x≤1.9. At this time, the lithium replenishment decomposition voltage of the positive electrode additive is below 4.6V, and its lithium replenishment capacity is very high.

[0008] In the embodiment of the present application, the particle size of the positive electrode additive is 50nm-20μm. The particle size of the positive electrode additive is controlled within this range to ensure that the Li x H 2-x C2O4 materials in the total Li x H 2-x The proportion of C2O4 in the material is relatively high, which facilitates its rapid decomposition and replenishment of lithium. At the same time, its own preparation is relatively easy and its stability in the air is relatively high. x H 2-x The particle size of C2O4 material is too large, and its specific surface area is large, which will cause the Li x H 2-x The proportion of C2O4 material is low, and the speed of decomposition to release active lithium is very slow. When the battery reaches the charge cut-off voltage, its decomposition degree is low; while Li x H 2-x Although C2O4 material is beneficial for decomposition and release of lithium, it is difficult to prepare, has poor stability in the air, and is more susceptible to water absorption.

[0009] In some embodiments of the present application, the particle size of the positive electrode additive is 100 nm-500 nm. In this case, the positive electrode additive can better balance faster decomposition and lithium release speed with better structural stability and preparation convenience.

[0010] In this application, Li x H 2-x There is no limitation on the preparation method of C2O4 material, and it can be prepared by substitution method or chemical in-situ synthesis method. When the substitution method is adopted, Li2C2O4 aqueous solution and low polarity solvent can be recrystallized to obtain Li x H 2- x C2O4 material. The low polarity solvent includes but is not limited to one or more of methanol, ethanol, propanol, acetone, ether, and ethylene glycol. When the chemical in-situ synthesis method is adopted, a soluble lithium salt can be added to water, and oxalic acid or a soluble oxalate can be added under stirring conditions to obtain Li x H 2-x C2O4 material. Wherein, the soluble lithium salt is selected from one or more of LiCl, LiOH, LiNO3 and Li2SO4, and the soluble oxalate is selected from one or more of K2C2O4, Na2C2O4 and the like.

[0011] The first aspect of this application mentions Li x H 2-x In C2O4 materials, part of Li is replaced by H. During the battery charging process, the H element is preferentially released to form vacancy defects, which is conducive to the low-voltage release of Li, reducing the decomposition and delithiation voltage of the material, and realizing Li x H 2-x The C2O4 material decomposes at a low voltage of no more than 4.6V. The active lithium produced by the decomposition can be used to replenish lithium to the negative electrode of the battery, avoiding irreversible structural changes in the positive electrode active materials of the battery under high charging voltage conditions, which is beneficial to improving the structural stability and cycle performance of the positive electrode active materials of the battery.

[0012] In a second aspect, the present application provides a positive electrode sheet, the positive electrode sheet comprising the positive electrode additive described in the first aspect of the present application. The method of introducing the positive electrode additive into the positive electrode sheet includes but is not limited to direct mixing method or coating method.

[0013] Specifically, in some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, and the positive electrode active material layer includes a positive electrode active material, the positive electrode additive, a conductive agent, and a binder. In this case, the positive electrode sheet can be obtained by directly mixing the positive electrode additive with the positive electrode active material, the conductive agent, and the binder to obtain a mixed slurry containing the positive electrode additive, and then coating and drying to obtain the positive electrode sheet.

[0014] In some other embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer and an additive layer sequentially arranged on the surface of the positive electrode current collector, wherein the additive layer contains the positive electrode additive, the conductive agent and the binder. At this time, a slurry containing the positive electrode additive, the conductive agent and the binder can be coated on the formed positive electrode active material layer, and the additive layer can be obtained after drying. It can also be understood that the positive electrode sheet provided in this embodiment of the present application is equivalent to the positive electrode sheet in the prior art plus the additive layer located on its surface.

[0015] Among them, the above-mentioned conductive agent and binder are conventional choices in the field of batteries. For example, the conductive agent may include but is not limited to at least one of carbon nanotubes, graphene, carbon black, graphite, etc. The binder may include but is not limited to one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl alcohol (PVA), styrene-butadiene rubber (SBR), polyacrylonitrile (PAN), polyimide (PI), polyacrylic acid (PAA), polyacrylate, polyolefin, sodium carboxymethyl cellulose (CMC) and sodium alginate, etc.

[0016] In the present application, the positive electrode active material includes but is not limited to at least one of lithium iron phosphate (LiFePO4), lithium manganese phosphate, lithium manganese iron phosphate, lithium vanadium phosphate, lithium cobalt phosphate, lithium cobalt oxide, lithium manganese oxide, lithium nickel manganese oxide, nickel cobalt manganese (NCM), nickel cobalt aluminum (NCA), etc.

[0017] Generally, the battery system LiFePO4 (charging cut-off voltage is about 3.8V) and NCM (charging cut-off voltage is about 4.35V). During the charging process of these battery systems, the Li x H 2-x The decomposition voltage of C2O4 material is low and it can decompose quickly with a very high degree of decomposition completion, thus avoiding the irreversible structural changes of the positive electrode active material under long-term high charging voltage conditions.

[0018] In the embodiment of the present application, the mass of the positive electrode additive does not exceed 10% of the mass of the positive electrode active material. The specific amount of the positive electrode additive introduced into the positive electrode of the battery can be adjusted according to the irreversible consumption capacity of the solid electrolyte membrane (i.e., SEI membrane) of the battery system, so that the active lithium capacity provided by the positive electrode additive is equal to the irreversible consumption capacity of the battery.

[0019] The positive electrode sheet provided in the second aspect of the present application contains the above-mentioned positive electrode additive and can be used to provide a battery with high capacity, high energy density and long cycle life.

[0020] In a third aspect, the present application provides a lithium-ion battery, the lithium-ion battery comprising the positive electrode sheet described in the second aspect of the present application. In addition to the positive electrode sheet, the lithium-ion battery also comprises a negative electrode sheet, and a diaphragm and an electrolyte located between the positive electrode sheet and the negative electrode sheet.

[0021] The lithium-ion battery may have high energy density and long cycle life, which is conducive to its wide application. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 For the embodiment of this application, Li 1.7 H 0.3 X-ray diffraction spectra of C2O4 material and lithium oxalate.

[0023] Figure 2 The charge and discharge curves of the battery sample S3 of Example 3, the battery sample S4 of Example 4 and the battery sample DS1 of the control experiment 1 at a charge and discharge rate of 0.1C.

[0024] Figure 3 The charge and discharge curves of the battery sample S1 of Example 1, the battery sample S2 of Example 2, and the battery sample S3 of Example 3 at a charge and discharge rate of 0.1C. DETAILED DESCRIPTION

[0025] The embodiments of the present application are further described below in combination with multiple embodiments. It should be noted that the following are exemplary embodiments of the present invention, and it should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention, and these improvements and modifications are also considered to be within the scope of protection of the present invention.

[0026] Example 1

[0027] In order to measure the delithiation potential and delithiation capacity of the positive electrode additive S1, Li 1.9 H 0.1 C2O4 is used as the positive electrode material, acetylene black is used as the conductive agent, polyvinylidene fluoride (PVDF) is used as the binder, and N-methylpyrrolidone (NMP) is used as the solvent. The positive electrode material: acetylene black: PVDF: NMP are mixed evenly in a mass ratio of 85:10:5:50 to obtain a mixed slurry; the mixed slurry is coated on an aluminum foil current collector, vacuum dried in an oven at 120°C for 24 hours, and then pressed and rolled to make a positive electrode sheet.

[0028] A metallic lithium sheet was used as the negative electrode, a celgard 2400 polypropylene porous membrane was used as the separator, and a mixed solution of 1 mol / L LiPF6 of ethylene carbonate (EC) and dimethyl carbonate (DMC) (volume ratio = 1:1) was used as the electrolyte; the test battery was assembled in a glove box filled with argon to obtain a battery sample S1.

[0029] Example 2

[0030] Battery sample S2 was prepared by referring to the method in Example 1, except that the positive electrode material used was Li 1.9 H 0.1 C2O4 (particle size 1 μm).

[0031] Example 3

[0032] Battery sample S3 was prepared by referring to the method in Example 1, except that the positive electrode material used was Li 1.9 H 0.1 C2O4 (particle size 200nm).

[0033] Example 4

[0034] Battery sample S4 was prepared by referring to the method in Example 1, except that the positive electrode material used was Li 1.7 H 0.3 C2O4(200nm).

[0035] Example 5

[0036] Battery sample S5 was prepared by referring to the method in Example 1, except that the positive electrode material used was Li 1.2 H 0.3 C2O4(200nm).

[0037] Example 6

[0038] Battery sample S6 was prepared by referring to the method in Example 1, except that the positive electrode material used was Li 0.8 H 0.3 C2O4(200nm).

[0039] Example 7

[0040] A method for preparing a lithium battery comprises:

[0041] 1) The positive electrode sheet was prepared by referring to the method in Example 1, except that the positive electrode material used was a LiFePO4 active material and an additive Li in a mass ratio of 90:10. 1.7 H 0.3 C2O4 (particle size 200nm).

[0042] 2) Preparation of negative electrode sheet: using graphite as negative electrode active material, a mixture of styrene-butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC) as a binder, and water (H2O) as a solvent, and mixing them evenly in a mass ratio of graphite: SBR: CMC: H2O = 100: 3: 2: 50 to obtain a negative electrode slurry; coating the negative electrode slurry on copper foil, placing it in an oven at 90° C. to dry for 24 hours, and then pressing and rolling to make a negative electrode sheet.

[0043] 3) Using Celgard 2400 polypropylene porous membrane as the separator and a mixed solution of 1 mol / L LiPF6 in ethylene carbonate (EC) and dimethyl carbonate (DMC) (volume ratio = 1:1) as the electrolyte; in a glove box filled with argon, assemble the above-mentioned positive electrode sheet and negative electrode sheet to obtain a battery, which is recorded as battery sample S7.

[0044] Example 8

[0045] The substrate layer positive electrode sheet is prepared by referring to the method in Example 1, except that the positive electrode material used is LiFePO4; according to the mass ratio of Li 1.7 H 0.3 C2O4 (particle size 200nm): acetylene black: PVDF: NMP = 85:10:5:50 are mixed evenly and coated on the substrate layer positive electrode sheet. After drying, an additive layer is formed on the substrate layer positive electrode sheet to obtain a composite positive electrode sheet; wherein Li 1.7 H 0.3 The mass of C2O4 is 1 / 9 of the mass of LiFePO4. Referring to the method described in Example 4, the above composite sheet was used as the positive electrode sheet to make a battery sample S8.

[0046] In addition, in order to highlight the beneficial effects of the technical solution of the present application, the following control experiments are also provided.

[0047] Control experiment 1

[0048] The battery sample DS1 was manufactured by referring to the method in Example 1, except that the positive electrode material used was Li2C2O4 (particle size was 200 nm).

[0049] Control experiment 2

[0050] The battery sample DS2 was manufactured by referring to the method in Example 7, except that the positive electrode material used was LiFePO4.

[0051] Experimental results analysis

[0052] 1. X-ray diffraction and structure refinement analysis

[0053] For Li in Example 4 1.7 H 0.3The C2O4 material and the Li2C2O4 material in Comparative Example 1 were subjected to phase analysis using an X-ray diffraction (XRD) device. The obtained XRD spectra are shown in Figure 1 The XRD test conditions are as follows: tube voltage 40 kV, tube current 20 mA, Cu Kα line, λ=0.154056 nm, graphite monochromator, step width 0.02°, dwell time 0.2 s.

[0054] right Figure 1 The XRD spectra in the figure are combined with XRD data and crystal structure knowledge to refine the structures of the two, analyze their different atomic proportions, and obtain the results shown in Table 1.

[0055] Table 1

[0056] Sample name C1 O2 O3 Li4 <![CDATA[Li 1.7 H 0.3 C2O4]]> 1 1 1 0.85 <![CDATA[Li2C2O4]]> 1 1 1 0.99

[0057] From Table 1, we can see that the atomic occupancy of C1, O2, and O3 in both are 1, which is not replaced. The difference lies in the atomic occupancy of Li4. The atomic occupancy of Li4 ​​in Li2C2O4 is 0.99, which is close to 1, which is a normal deviation, corresponding to x = 2, while Li 1.7 H 0.3 The Li4 atom occupancy of C2O4 is 0.85, which corresponds to x=1.7 after conversion, indicating that some atoms are replaced. Therefore, combined with the XRD spectrum and structure refinement results, compared with the comparative sample Li2C2O4, Li 1.7 H 0.3 The crystal structure of C2O4 has not changed, but part of the Li has been replaced by H atoms, which leads to differences in the decomposition characteristics of the two when used as positive electrode additives.

[0058] 2. Li x H 2-x C2O4 material decomposition performance test

[0059] The charge-discharge specific capacity test used in this experiment is carried out on a charge-discharge tester. The battery is set to a charging state (i.e., positive electrode delithiation), the charging current density is 0.1C, and the charge is stopped when the cut-off voltage is 4.6V or 4.8V, and the battery's first charge specific capacity and first delithiation specific capacity are calculated.

[0060] First charge specific capacity (mAh / g) = first charge capacity / mass of active material

[0061] First delithiation specific capacity (mAh / g) = first delithiation capacity / mass of active material.

[0062] Among them, in the absence of Li x H 2-xIn the battery containing C2O4 (battery DS1, DS2), the first charge specific capacity is equal to the first lithium de-ion specific capacity; x H 2-x In the C2O4 batteries (batteries S1, S2, S3, S4, S5, S6, S7, and S8), the first charge specific capacity includes the capacity contributed by Li and H removal, and the first lithium removal specific capacity includes the capacity contributed by Li removal. H removal can reduce the decomposition voltage but does not participate in lithium replenishment at the negative electrode.

[0063] After the first lithium removal is completed, each battery is set to a discharge state (i.e., positive electrode lithium insertion), the discharge current density is 0.1C, and the discharge ends when the cut-off voltage is 3V, and the first discharge specific capacity is calculated. Among them, the first discharge specific capacity (mAh / g) = first discharge capacity / mass of active material.

[0064] (1) Li with different atomic proportions x H 2-x Comparison of C2O4 decomposition performance

[0065] Figure 2 The charge and discharge curves of battery samples S3, S4, and DS1 at a charge and discharge rate of 0.1C are shown in Table 2.

[0066] Table 2

[0067]

[0068] The theoretical specific capacity of lithium oxalate is 526.0 mAh / g. The first charge mass specific capacity of DS1 battery-Li2C2O4 at a charge cut-off voltage of 4.8 V is 340.2 mAh / g, which indicates a decomposition rate of 64.7%. As shown in Table 2, it only produces a decomposition capacity of 29.7 mAh at a voltage of 4.6 V, and the decomposition rate is only 5.6%. In this application, Li2C2O4 with x=1.9 is used. x H 2-x The first charge specific capacity of the S3 battery of C2O4 at a charge cut-off voltage of 4.6V is 469.7mAh / g, and the Li 1.9 H 0.1 The decomposition rate of C2O4 reached 89.3%; using Li x = 1.7 x H 2-x The first charge specific capacity of the S4 battery of C2O4 at a charge cut-off voltage of 4.6V is 498.1mAh / g, and the Li 1.7 H 0.3 The decomposition rate of C2O4 reached 94.7%; using Li x = 1.2 x H 2-x The first charge specific capacity of the S5 battery of C2O4 at a charge cut-off voltage of 4.6V is 510.1mAh / g, and the Li1.9 H 0.1 The decomposition rate of C2O4 reached 96.9%; using Li x = 0.8 x H 2-x The first charge specific capacity of the S6 battery of C2O4 is 519.4mAh / g, and the Li 1.9 H 0.1 The decomposition rate of C2O4 is 98.7%. x H 2-x The decomposition rate of C2O4 is significantly higher than that of Li2C2O4, and the available initial lithium removal capacity is also significantly higher than that of Li2C2O4. x H 2-x The charging decomposition voltage platform of C2O4 is also significantly reduced, specifically, the platform voltage is from high to low DS1-4.7V>S3-4.55V>S4-4.47V>S5-4.43V>S6-4.38V. It should be noted that the charging cut-off voltages of DS1 and S3-S6 are different, mainly for testing the Li x H 2-x Charging decomposition voltage platform of C2O4 material.

[0069] The above results show that when part of the Li in lithium oxalate is replaced by H, the resulting Li x H 2-x The decomposition voltage of C2O4 material is reduced, and the lower first charge decomposition voltage platform enables the material to decompose without exceeding the voltage limit of many positive electrode active materials. It can be used as a lithium supplement material to increase the actual available active lithium capacity.

[0070] The above test results show that at a charging cut-off voltage of 4.6V, battery samples S3, S4, S5 and S6 have higher lithium removal capacity than DS1 sample, indicating that the Li x H 2-x C2O4 material can provide more active lithium to the negative electrode than Li2C2O4. In addition, Li x H 2-x When C2O4 is used as an additive, the lithium removal capacity of batteries S3 and S4 is higher than that of S5 and S6, but the decomposition voltage is also slightly higher than the latter. Therefore, under the premise of taking into account low decomposition voltage and high lithium removal capacity, batteries of different systems can choose Li x H 2-x The C2O4 additive avoids the adverse effects of high charging voltage on the structure of the positive electrode active material that may cause the additive to decompose, improves the stability and cycle performance of the battery, and enables the additive to provide a higher lithium removal capacity.

[0071] (2)Li x H 2-x Comparison of decomposition performance of C2O4 materials with different particle sizes

[0072] Figure 3 The charge and discharge curves of battery samples S1, S2 and S3 at a charge and discharge rate of 0.1C are shown in Table 3. Table 3 summarizes the electrochemical performance parameters such as the first charge specific capacity, first discharge specific capacity and decomposition platform voltage of battery samples S1, S2 and S3 at a charge and discharge rate of 0.1C.

[0073] Table 3

[0074]

[0075] The additives in the S1, S2 and S3 battery samples are all Li 1.9 H 0.1 C2O4, the difference between the three lies in the different particle sizes of the additives: S1-5μm micron, S2-1μm micron, S3-200nm nanometer. The decomposition specific capacity of the nano-level S3 additive material is 469.7mAh / g, which is 42.1mAh / g higher than the additive with a particle size of 1μm and 86.6mAh / g higher than the additive with a particle size of 5μm. The corresponding first delithiation specific capacity of the actual available active lithium is also significantly higher than that of S1 and S2. In terms of the charge decomposition voltage platform, Li with a particle size of 200nm x H 2-x The charging voltage platform of C2O4 material is also significantly lower than that of micron-sized large-particle materials. Therefore, particle size can affect the x H 2-x Decomposition properties of C2O4 materials such as decomposition voltage and decomposition capacity.

[0076] 3. Li x H 2-x Lithium replenishment performance test of C2O4 material

[0077] The charge and discharge regime of batteries S7, S8 and DS2 is a charge cut-off voltage of 4.6 V and a discharge cut-off voltage of 2.00 V. The first charge and discharge capacities of batteries S4, S5 and DS2 are listed in Table 4.

[0078] Table 4

[0079] Battery ID First charge capacity (mAh) First discharge capacity (mAh) S7 1269.6 1083.1 S8 1180.8 1077.4 DS2 1082.1 952.2

[0080] The results in Table 4 show that the positive electrode active material LiFePO4 of DS2 battery has a charging capacity of 1082.1 mAh, SEI film formation consumes about 12% of active lithium, and discharge can embed 952.2 mAh; while the positive electrode introduces the additive Li 1.7 H 0.3C2O4 batteries S7 and S8, due to Li 1.7 H 0.3 C2O4 decomposes during charging to provide active lithium. The discharge capacity of batteries S7 and S8 is basically the same as the charging capacity of DS2, which shows that Li 1.7 H 0.3 The active lithium provided by the decomposition of C2O4 during the charging process can meet the consumption of SEI film, replenish sufficient active lithium, and enable sufficient active lithium to be discharged and embedded back into LiFePO4. x H 2-x C2O4 material can replenish the active lithium consumed by the negative electrode SEI film, thereby significantly improving the capacity of the battery.

[0081] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.

Claims

1. A positive electrode lithium supplement, characterized in that: The general formula of the positive electrode lithium supplement is Li x H 2-x C2O4, where the value range of x is: 1.2≤x≤1.

9.

2. The positive electrode lithium supplement according to claim 1, characterized in that The particle size of the positive electrode lithium supplement agent is 50nm-20μm.

3. The positive electrode lithium supplement according to claim 2, characterized in that: The particle size of the positive electrode lithium supplement agent is 100nm-500nm.

4. A positive electrode sheet, characterized in that: The positive electrode sheet contains the positive electrode lithium supplement agent according to any one of claims 1 to 3.

5. The positive electrode sheet according to claim 4, characterized in that: The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector, wherein the positive electrode active material layer includes a positive electrode active material, the positive electrode lithium supplement, a conductive agent and a binder.

6. The positive electrode sheet according to claim 4, characterized in that: The positive electrode sheet comprises a positive electrode current collector and a positive electrode active material layer and an additive layer sequentially arranged on the positive electrode current collector, wherein the additive layer contains the positive electrode lithium supplement, a conductive agent and a binder.

7. The positive electrode sheet according to claim 5 or 6, characterized in that: The mass of the positive electrode lithium supplement does not exceed 10% of the mass of the positive electrode active material.

8. A lithium ion battery, characterized in that: The lithium-ion battery comprises the positive electrode sheet as described in any one of claims 4 to 7.

Citation Information

Patent Citations

  • Preparing method for high-purity lithium oxalate

    CN105859542A

  • Cathode for lithium-sulfur battery, and lithium-sulfur battery comprising same

    CN110800136A

  • Preparation method of pole piece and cylindrical battery

    CN111900490A