Methods, products, and applications for encapsulating multi-gas atomic chambers with irregularly arranged shapes.
By employing a high-sealing multi-gas atomic cell encapsulation method with irregularly arranged arrays, the problems of anodic bonding quality and buffer gas ratio in atomic cells are solved, achieving high-sealing and low-cost atomic cell fabrication suitable for quantum sensor devices.
Patent Information
- Application Number
- CN202211336426.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2042-10-28
AI Technical Summary
In the existing technology, the anodic bonding quality of the atomic gas chamber is not high, and the internal buffer gas filling ratio of the multi-part atomic gas chamber is inappropriate, making it difficult to achieve high sealing and effectively suppress linear temperature shift.
A high-sealing multi-gas atomic chamber encapsulation method using irregularly arranged arrays is employed. A mesh is formed on the surface of a silicon wafer through a non-uniform irregularly arranged array. Combined with silicon-glass anodic bonding and glass-silicon-glass anodic bonding, close-contact chemical bonds are formed by electrostatic attraction, and buffer gases of different proportions are filled in.
It achieves highly sealed atomic gas chamber encapsulation, enhances bonding quality, reduces manufacturing costs, is suitable for miniaturization and mass production, and is applicable to the field of quantum sensor devices.
Smart Images

Figure CN115744811B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of optical precision processing technology, and more specifically, relates to a method, product and application method for packaging multi-atom chambers with irregular arrangement, and a method, product and application method for packaging high-sealing multi-atom chambers with irregular arrangement array. Background Technology
[0002] Atomic gas cells, as important components of quantum sensor devices such as chip-based atomic clocks, atomic magnetometers, and gyroscopes, can be widely used in individual soldier operations, anti-jamming GPS positioning systems, network transmission synchronization encryption, and communication network synchronization. With the continuous development of modern technology, the demand for small size and low power consumption in quantum sensor devices is becoming increasingly strong. Atomic gas cells fabricated using MEMS micromachining technology greatly reduce the size of the physical system of quantum sensor devices and simplify the integration with other optical components.
[0003] In the fabrication of atomic gas cells, the arrangement of the cell mesh on the silicon wafer is crucial. Traditional MEMS gas cells have a uniformly distributed mesh on the silicon wafer. This arrangement results in almost uniform deformation and force on each mesh during bonding, failing to enhance anodic bonding quality. Furthermore, the atomic gas cell needs to be filled with a mixed buffer gas to suppress linear temperature shifts. Since frequency shifts in different directions are caused by buffer gas atoms or molecules with different shift coefficients, mixing easily polarizable and non-polarizable buffer gas atoms or molecules in a specific ratio plays a vital role in suppressing linear temperature shifts. For multi-part atomic gas cells, this invention proposes several different buffer gas filling ratios.
[0004] One of the most crucial steps in fabricating atomic gas cells is achieving a tight bond between the silicon wafer and the glass. The most widely used method for silicon-glass bonding is anodic bonding. During bonding, the silicon-glass is heated to 100-500°C, with the silicon wafer connected to the positive terminal of a power source and the glass connected to the negative terminal. Under a voltage of 200-1000V, the Na+ in the glass... +Drifting towards the negative terminal of the power supply, a depletion layer several micrometers wide is formed on the glass surface adjacent to the silicon wafer. This depletion layer carries a negative charge, creating a strong electrostatic attraction between the silicon wafer and the glass, resulting in a tight bond between them. Heating the anodic bonding equipment, heating the silicon wafer and glass, and applying voltage to both can promote the movement of ions in the glass and silicon wafer, creating an even stronger electrostatic attraction in the depletion layer. This leads to a chemical reaction at the tightly contacted silicon wafer-glass surface, forming strong chemical bonds, such as Si-O-Si bonds, achieving a highly sealed atomic gas chamber. Furthermore, the shape of the cathode also affects the bonding effect during bonding; commonly used electrodes include point contact electrodes and double parallel plate electrodes. Point contact electrodes do not create voids at the bonding interface, while double parallel plate electrodes have some porosity at the bonding interface. While double parallel plate electrodes have a higher bonding rate than point contact electrodes, their bonding efficiency for point charges is much lower. The cathode uses a cross-shaped graphite wire electrode for anodic bonding, which not only reduces the generation of voids at the bonding interface, but also improves the bonding rate compared to point electrode bonding.
[0005] To address the issues of low anodic bonding quality and the proportion of buffer gas filling inside the atomic gas chamber during the preparation process, a high-sealing multi-gas atomic gas chamber encapsulation method based on an irregularly arranged array is urgently needed to increase bonding strength and suppress linear temperature shift inside the atomic gas chamber. Summary of the Invention
[0006] To address the aforementioned deficiencies or improvement needs of existing technologies, this invention provides a method and product for high-sealing multi-gas atomic chamber encapsulation using an irregularly shaped array. This method, taking into account the characteristics of silicon wafers and their bonding process with glass, employs an irregularly shaped array. Compared to traditional atomic chamber fabrication methods, this non-uniform irregular array eliminates the need for fabricating mesh openings at the edges of the silicon wafer. Under voltage, Na+ ions in the glass react more readily with anions on the silicon wafer surface, forming a depletion layer several micrometers wide. This depletion layer carries a negative charge, while the silicon wafer carries a positive charge. A strong electrostatic attraction exists between the silicon wafer and the borosilicate glass, ensuring close contact and forming a highly sealed atomic chamber encapsulation. This method utilizes an array of multiple chamber mesh openings on a single silicon wafer, reducing fabrication costs and increasing atomic chamber density.
[0007] To achieve the above objectives, according to one aspect of the present invention, a method for packaging highly sealed multi-gas atomic chambers with irregularly arranged arrays is proposed, comprising the following steps: S1 determines the shape and size of the unit atomic gas cell based on the internal mesh of the atomic gas cell; S2 designs the arrangement of internal mesh holes on the silicon wafer based on the deformation during the silicon wafer heating and bonding process. S3 etches the silicon wafer according to the arrangement of the internal mesh holes; S4 involves performing silicon-glass anodic bonding between the silicon wafer obtained in step S3 and the top borosilicate glass to form two pre-bonded wafers. S5 If the atomic gas chamber is a single-chamber atomic gas chamber, then the alkali metal element is filled into the single-chamber light-atom interaction cavity mesh of the two-layer pre-bonded sheet; if the atomic gas chamber is a double-chamber atomic gas chamber, then the alkali metal release agent is filled into the double-chamber chemical reaction cavity mesh of the two-layer pre-bonded sheet. S6 involves performing glass-silicon-glass anodic bonding of the two pre-fabricated bonding sheets processed in step S5 and the bottom borosilicate glass sheet in a buffer gas atmosphere to form a three-layer sealed cavity bonding sheet. S7 According to the shape and size of the unit atomic gas chamber in step S1, the three-layer sealing cavity bonding sheet is diced and processed to obtain a unitized single-chamber atomic gas chamber or double-chamber atomic gas chamber. For a single-chamber atomic gas chamber, S8 heats the single-chamber atomic gas chamber to release alkali metal atoms in the alkali metal element; for a double-chamber atomic gas chamber, it is filled with an alkali metal releasing agent and heated to a certain temperature to release alkali metal atoms in the alkali metal releasing agent. S9 tests and screens the atomic gas chambers obtained in step S8.
[0008] As a further preferred option, step S2 specifically includes the following steps: based on the properties of the silicon wafer, setting the heating conditions during the silicon wafer heating bonding process, as well as the shape of the edge sacrificial layer and the shape of the internal mesh during the bonding process, simulating the deformation during the silicon wafer heating bonding process, so as to obtain an internal mesh arrangement with the fewest edge sacrificial layers and the most internal meshes in the edge sacrificial layer.
[0009] As a further preferred option, it is also necessary to consider the amount of Na+ in the glass bonded to the silicon wafer during the bonding process. That is, the glass outside the edge sacrificial layer can provide more Na+ to react with the anions on the surface of the silicon wafer to form a depletion layer with a width of several micrometers on the glass surface. The depletion layer carries a negative charge, the silicon wafer carries a positive charge, and there is a large electrostatic attraction between the silicon wafer and the borosilicate glass, which makes the two in close contact.
[0010] As a further preferred embodiment, in step S3, the silicon wafer is etched according to the arrangement of the internal mesh. If the number of internal meshes in the unit atomic gas chamber is 1, a single-chamber atomic gas chamber is formed. If the number of internal meshes in the unit atomic gas chamber is 2, a double-chamber atomic gas chamber is formed, consisting of a light-atomic interaction chamber and a chemical reaction chamber.
[0011] As a further preferred option, before step S4, the following operation is required: A heater, a thermistor, and Au-Si pads connected to the heater and the thermistor are fabricated circumferentially at the top of the single-cavity gas chamber or the light-atom interaction cavity of the etched silicon wafer. The specific fabrication steps are as follows: S21 sequentially performs vapor deposition, homogenization and pre-baking, photolithography exposure, and development on the top surface of the silicon wafer, transferring the pattern on the mask with alignment marks to the top surface of the silicon wafer. S22 uses magnetron sputtering to sequentially deposit Ti and Pt on the top surface of a silicon wafer to prepare a heater and a thermistor. The magnetron sputtering of the Ti and Pt layers is performed by a stripping method. S23 sequentially performs vapor deposition, homogenization and pre-baking, photolithography exposure, and development on the top surface of the silicon wafer after step S22. The pattern on another mask with alignment marks is transferred to the top surface of the silicon wafer, and Au-Si pads are prepared by depositing Au using magnetron sputtering.
[0012] As a further preferred option, the following operations need to be performed before step S4: Shallow U-grooves are etched on the bottom surface of the top borosilicate glass to conform to the shape of the heater, thermistor, and Au-Si pads. Preferably, in step S4, the silicon wafer and the top borosilicate glass are optically aligned and mounted on a bonding tray, then fed into the bonding cavity for anodic bonding to form two pre-fabricated bonding sheets. During this process, the bonding vacuum degree is <1×10⁻⁶. - 5 mbar, bonding electrode voltage is 1000V, bonding pressure is 1000N, and the bonding surface is the top surface of the silicon wafer and one side of the shallow U-groove of the top borosilicate glass strip; Preferably, in step S6, two layers of pre-fabricated bonding sheets and a bottom borosilicate glass sheet are mounted on the bonding tray of the bonding machine through optical alignment. The two layers of pre-fabricated bonding sheets are connected to the bottom borosilicate glass sheet, which is connected to the top heating source. The top borosilicate glass sheet of the two layers of pre-fabricated bonding sheets is connected to the bottom heating source. Simultaneously, a thick gasket on the bonding tray forms a gap between the two layers of pre-fabricated bonding sheets and the bottom borosilicate glass sheet, allowing buffer gas to enter the light-atom interaction cavity or the light-atom interaction cavity and chemical reaction cavity. Both the top and bottom heating sources are heated to the bonding temperature. The bonding cavity inside the bonding machine is evacuated to a vacuum degree <1×10⁻⁶. -5After maintaining the vacuum for 30 minutes, a buffer gas is introduced and kept for a period of time to allow the buffer gas to diffuse into the light-atom interaction cavity or the light-atom interaction cavity and the chemical reaction cavity. The top heating source applies a pressure of 1000N to the bottom borosilicate glass sheet, and the bonding electrode voltage is 1000V to form a three-layer sealed cavity bonding sheet.
[0013] Preferably, before step S7, the following operations also need to be performed: A layer of Cr metal is sputtered onto the top borosilicate glass of the three-layer sealed cavity bonding sheet to enhance the adhesion between the surface of the top borosilicate glass and the seed layer metal Au. A seed layer of Au is electroplated onto the adhesion layer metal Cr as a raw material for preparing electrode leads and Au-Glass pads; The top borosilicate glass processed by the above steps is subjected to vapor deposition, homogenization and pre-baking, photolithography exposure and development to transfer the pattern on the mask with alignment marks to the surface of the top borosilicate glass, so as to pattern the electrode leads and Au-Glass pads. The patterned electrode leads and Au-Glass pads are etched to form the electrode leads and Au-Glass pads. The three-layer sealed cavity bonding sheet processed by the above steps is then annealed to achieve metal alloying of the electrode leads and Au-Glass pads.
[0014] As a further preferred embodiment, in step S6, the buffer gas includes an Ar-N2 mixed buffer gas, an Ar-CH4 mixed buffer gas, or a K gas mixed in a certain proportion. r -N2 mixed buffer gas or A r -N e Mixed buffer gas; Preferably, if the buffer gas is an Ar-N2 mixture, r(P) Ar / P N2 )=1.6, if it is an Ar-CH4 mixed buffer gas, r(P Ar / P CH4 )=1.8, if it is K r -N2 mixed buffer gas, r(P Kr / P N2 If ) = 0.9, then it is A r -N e Mixed buffer gas, r(P) Ar / P Ne )=0.8, where r is a proportional function.
[0015] According to another aspect of the present invention, a product is also provided, prepared by the method described above, comprising a top borosilicate glass layer, a silicon wafer, and a bottom borosilicate glass layer sequentially bonded together, wherein... The top borosilicate glass is provided with Au-Glass pads, electrode leads and pad lead contact holes. The Au-Glass pads are connected to the electrode leads. The pad lead contact holes penetrate the top borosilicate glass and are corresponding to the ends of the electrode leads. The silicon wafer is provided with a single-chamber light-atom interaction cavity, or a dual-chamber light-atom interaction cavity and a chemical reaction cavity connected in series. A heater and a thermistor are provided on the top circumferential direction of the light-atom interaction cavity. The heater and the thermistor are electrically connected to the Au-Si pads respectively. The Au-Si pads are provided with corresponding pad lead contact holes. The bottom borosilicate glass is used to encapsulate the bottom surface of the silicon wafer to form a sealed single or double chamber.
[0016] According to another aspect of the present invention, a method for using an atomic gas chamber is also provided. The atomic gas chamber is prepared by the method described above. During use, the atomic gas chamber is directly heated by a heater, and the heating temperature of the atomic gas chamber is controlled by the combined action of a thermistor and the heater.
[0017] In summary, compared with the prior art, the above-described technical solutions conceived by this invention mainly possess the following technical advantages: 1. The atomic gas chamber prepared by this invention is a sandwich-like structure, a highly sealed quantum sensor device formed by silicon-glass anodic bonding and glass-silicon-glass anodic bonding, filled with alkali metal or alkali metal releasing agent and multi-part buffer gas. The mesh of atomic gas chambers with different structures and shapes is formed on the surface of silicon wafer 2 in a certain array pattern, exhibiting a non-uniform irregular arrangement. The highly sealed multi-part atomic gas chamber is prepared through silicon-glass anodic bonding, glass-silicon-glass anodic bonding, and filling with multi-part buffer gas.
[0018] 2. In this invention, atomic gas cell meshes of different structures and shapes are arranged in a specific array on the surface of a silicon wafer, forming a non-uniform, irregularly shaped array. This arrangement results in greater deformation of the atomic gas cell meshes closest to the edge of the silicon wafer compared to other internal meshes during silicon-glass anodic bonding and glass-silicon-glass anodic bonding processes. At relatively high anodic bonding temperatures, the closely contacting silicon wafer and borosilicate glass undergo a chemical reaction, forming strong chemical bonds, such as Si-O-Si bonds, thus enhancing bonding quality. Furthermore, due to the silicon-glass anodic bonding process achieved at specific temperatures and voltages... During the process, the resistance increases further away from the center of the silicon wafer. Compared to the bonding quality at the center, the bonding quality is worse closer to the edge of the silicon wafer where it contacts the glass sheet. Compared to traditional atomic cell fabrication methods, the non-uniform irregular array eliminates the need for fabricating meshes at the edge of the silicon wafer surface. Under voltage, Na+ ions in the glass react more readily with anions on the silicon wafer surface, forming a depletion layer several micrometers wide on the glass surface. This depletion layer carries a negative charge, while the silicon wafer carries a positive charge. A strong electrostatic attraction exists between the silicon wafer and the borosilicate glass, ensuring close contact and forming a highly sealed atomic cell encapsulation. Arraying multiple cavity meshes on a single silicon wafer reduces fabrication costs and increases the density of atomic cells.
[0019] 3. The atomic gas cell meshes of the present invention with different shapes can meet the reaction requirements of light and atom interaction sites of different sizes and needs, such as to enhance or suppress specific signals.
[0020] 4. This invention fills the atomic gas chamber with two buffer gases of different properties, which can be a mixture of Ar-N2 buffer gas, Ar-CH4 buffer gas, or K gas in a certain proportion. r -N2 mixed buffer gas or A r -N e Mixed buffer gases. Based on the ideal gas law and the temperature shift formula caused by the buffer gas, the proportions of the mixed buffer gases can be obtained as follows: r(P) Ar / P N2 )=1.6, r(P Ar / P CH4 )=1.8, r(P Kr / P N2 )=0.9, r(P Ar / P Ne =0.8.
[0021] 5. The atomic gas cell prepared by this invention has the advantages of small size and miniaturization, and is easy to mass-produce in arrays. It is suitable for application in the field of quantum sensor devices such as atomic clocks, magnetometers, and MEMS gyroscopes.
[0022] 6. In this invention, the heater and thermistor in the gas chamber no longer exist as devices, but as components of the atomic gas chamber. This reduces the size and weight of the packaged device, making it easier to miniaturize and chip-scale the physical system. Furthermore, the heater and thermistor are directly located on the silicon-glass bonding surface of the atomic gas chamber, allowing direct heating of the gas chamber itself, reducing heat dissipation and saving the time required to reach the desired temperature. Moreover, the atomic gas chamber in this invention is glue-free, reducing laser loss during propagation and improving light transmission efficiency. Attached Figure Description
[0023] Figure 1 This is a flowchart of a high-sealing multi-gas atomic gas chamber encapsulation method with irregularly arranged arrays according to an embodiment of the present invention; Figure 2 This is a schematic diagram of the arrangement of internal mesh holes on a silicon wafer during the preparation of a high-sealing multi-gas atomic chamber with an irregularly arranged array, according to an embodiment of the present invention. Figure 3 This is a schematic diagram of the internal mesh structure involved in the dual-chamber atomic gas chamber; Figure 4 (a) is a schematic diagram of a modular single-chamber atomic gas chamber. Figure 4 (b) is a schematic diagram of the structure of the dual-chamber atomic gas chamber. Detailed Implementation
[0024] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention. Furthermore, the technical features involved in the various embodiments of this invention described below can be combined with each other as long as they do not conflict with each other.
[0025] like Figure 1 As shown in the figure, an embodiment of the present invention provides a highly sealed multi-gas atomic cell encapsulation method for irregularly arranged arrays, comprising the following steps: S1: Determine the shape and size of the unit atomic gas cell based on the internal mesh of the atomic gas cell. For example... Figure 3As shown, in one embodiment of the present invention, the atomic gas chamber mesh has various different shapes. For example, the shape of the single-chamber atomic gas chamber single-chamber light-atom interaction cavity mesh 3 includes, but is not limited to, triangles, squares, hexagons, octagons, dodecagons, circles, etc. The unitized dual-chamber atomic gas chamber includes a dual-chamber light-atom interaction cavity mesh 7, a dual-chamber chemical reaction cavity mesh 8, and a dual-chamber microchannel 9 on the top surface of the silicon wafer 2 for connecting the above two meshes. The shape of the dual-chamber light-atom interaction cavity mesh 7 includes, but is not limited to, triangles, squares, hexagons, etc. The shapes of the mesh 8 in the dual-chamber chemical reaction chamber include, but are not limited to, triangles, squares, hexagons, regular octagons, regular octagons, regular dodecagons, and circles. N tiny channels (1≤N≤5) connect the mesh 7 of the dual-chamber light-atom interaction chamber and the mesh 8 of the dual-chamber chemical reaction chamber, allowing the alkali metal vapor generated by the decomposition of the alkali metal releasing agent 10 filled inside the dual-chamber chemical reaction chamber under heating conditions to enter the dual-chamber light-atom interaction chamber. The different shapes of the atomic gas chamber meshes can meet the reaction requirements of light-atom interaction sites of different sizes and needs, such as enhancing or suppressing specific signals.
[0026] S2: The arrangement of internal mesh holes on the silicon wafer is designed based on the deformation during the silicon wafer heating bonding process. In the above method, atomic gas cell mesh holes of different structures and shapes on the silicon wafer surface are arranged in a specific array to form a non-uniform, irregularly shaped array. This arrangement results in greater deformation of the atomic gas cell mesh holes closest to the edge of the silicon wafer compared to other internal mesh holes during silicon-glass anodic bonding and glass-silicon-glass anodic bonding processes. At relatively high anodic bonding temperatures, the closely contacting silicon wafer and borosilicate glass undergo a chemical reaction, forming strong chemical bonds, such as Si-O-Si bonds, thus enhancing bonding quality. Furthermore, due to the achievement of silicon-glass anodic bonding at specific temperatures and voltages... During bonding, the resistance increases further away from the center of the silicon wafer. Compared to the bonding quality at the center, the bonding quality is worse closer to the edge of the silicon wafer where it contacts the glass sheet. Compared to traditional atomic cell fabrication methods, the non-uniform irregular array eliminates the need for fabricating meshes at the edges of the silicon wafer surface. Under voltage, Na+ ions in the glass react more readily with anions on the silicon wafer surface, forming a depletion layer several micrometers wide on the glass surface. This depletion layer carries a negative charge, while the silicon wafer carries a positive charge. A strong electrostatic attraction exists between the silicon wafer and the borosilicate glass, ensuring close contact and forming a highly sealed atomic cell encapsulation. Arraying multiple cavity meshes on a single silicon wafer reduces fabrication costs and increases the density of atomic cells.
[0027] Therefore, in this invention, the region with large heating deformation at the edge of the silicon wafer is designated as the edge sacrificial layer. The interior of the edge sacrificial layer contains internal mesh openings that meet the requirements. Based on the properties of the silicon wafer, the heating conditions during the silicon wafer heating bonding process, as well as the shape of the edge sacrificial layer and the shape of the internal mesh openings, are set. The deformation during the silicon wafer heating bonding process is simulated to obtain an internal mesh opening arrangement that minimizes the edge sacrificial layer and maximizes the number of internal mesh openings. Furthermore, the amount of Na+ in the glass bonded to the silicon wafer during the bonding process must be considered. Specifically, the glass outside the edge sacrificial layer must provide a greater amount of Na+ to react with the anions on the silicon wafer surface, forming a depletion layer several micrometers wide on the glass surface. The depletion layer carries a negative charge, while the silicon wafer carries a positive charge. A strong electrostatic attraction exists between the silicon wafer and the borosilicate glass, ensuring close contact between them. The method of this invention uses simulation software to simulate the deformation of silicon wafers during glass bonding, sets different non-uniform irregular array shapes of internal mesh structures, and calculates the amount of Na+ that the glass can replenish in the edge region of the silicon wafer outside the sacrificial layer, in order to seek the arrangement with the fewest edge sacrificial layers and the largest number of internal mesh openings that meet the requirements.
[0028] like Figure 2 As shown, based on the calculations above, generally speaking, the atomic gas chamber mesh is formed on the silicon wafer surface with an overall non-uniform irregular arrangement array. The array shape includes, but is not limited to, cross shape, square shape, regular hexagon shape, regular octagon shape, circle shape, star shape, etc. The attached figure only uses a single-chamber atomic gas chamber with circular mesh as an example for illustration. The single-chamber atomic gas chamber can also be replaced by a double-chamber atomic gas chamber, and the mesh shape can also be changed according to requirements.
[0029] After atomic gas cells of different structures and shapes are diced into units by a wafer dicing machine, they can be divided into two categories according to the number of internal pores: one category is the unitized single-chamber atomic gas cell, with an internal pore count of 1, such as... Figure 4 As shown in (a), this is a modular single-chamber atomic gas chamber; another type is a modular double-chamber atomic gas chamber with an internal mesh number of 2, as shown in (a). Figure 4 As shown in (b), a modularized dual-chamber atomic gas chamber. The modularized single-chamber atomic gas chamber, a single-chamber light-atomic interaction cavity, has mesh 3 with shapes including, but not limited to, triangles, squares, hexagons, octagons, dodecagons, circles, etc., such as... Figure 2As shown, the modular dual-chamber atomic gas chamber includes a dual-chamber light-atom interaction cavity mesh 7, a dual-chamber chemical reaction cavity mesh 8, and a dual-chamber microchannel 9 on the top surface of the silicon wafer 2 for connecting the two meshes. The shape of the dual-chamber light-atom interaction cavity mesh 7 includes, but is not limited to, triangles, squares, hexagons, octagons, dodecagons, and circles. The shape of the dual-chamber chemical reaction cavity mesh 8 includes, but is not limited to, triangles, squares, hexagons, octagons, dodecagons, and circles. There are N tiny channels, i.e., dual-chamber microchannels 9, between the dual-chamber light-atom interaction cavity mesh 7 and the dual-chamber chemical reaction cavity mesh 8 (1≤N≤5), allowing the alkali metal vapor generated by the decomposition of the alkali metal releasing agent 10 filled inside the dual-chamber chemical reaction cavity under heating conditions to enter the dual-chamber light-atom interaction cavity. The combination diagram of the dual-chamber light-atom interaction cavity mesh 7 and the dual-chamber chemical reaction cavity mesh 8 is shown in the figure. Figure 3 As shown.
[0030] S3: Etch the silicon wafer according to the arrangement of the internal mesh. In this step, the atomic gas chamber mesh is formed on the surface of silicon wafer 2 with a non-uniform irregular arrangement. During the formation of the mesh on silicon wafer 2, since the edge areas of the surface of silicon wafer 2 do not require the preparation of mesh, the present invention uses the DRIE deep reactive ion etching method to prepare the silicon through-hole mesh. In the process of forming the silicon through-hole mesh, the areas where no mesh preparation is required can also increase the substrate bonding area during deep silicon etching, thereby enhancing heat dissipation.
[0031] More specifically, the general steps for cleaning the surface of a silicon wafer using standard cleaning processes are as follows: First, the silicon wafer is immersed in acetone and alcohol and ultrasonically vibrated. The substrate surface is then rinsed with deionized water and dried with nitrogen gas to remove organic contaminants. The silicon wafer is then immersed and etched sequentially for 15 min, 10 min, and 10 min with standard cleaning solutions No. 3 (H2SO4 (98%): H2O2 (30%) = 3:1), No. 1 (NH4OH (28%): H2O2 (30%): H2O = 1:2:7), and No. 2 (HCl (37%): H2O2 (30%): H2O = 1:1:6) at 150°C, 10 min, and 10 min respectively to remove metal particles, metal, organic matter, moisture molecules, and other contaminants from the silicon wafer surface. Finally, the silicon wafer is etched with 5% HF for 5 s to remove the natural oxide layer on the silicon wafer surface.
[0032] The general steps for preparing internal mesh (i.e., through-silicon vias) by DRIE deep silicon etching overlay are explained by performing front and back overlay on silicon wafers: (1) Vapor deposition: Hexamethyldisilazane (HMDS) is coated on the silicon wafer to change the surface state of the silicon wafer from hydrophilic to hydrophobic, thereby increasing the adhesion between the photoresist and the silicon wafer; (2) Spin coating and pre-baking: Photoresist is spin-coated on the surface of the silicon wafer in (1), and after completion, the silicon wafer is pre-baked to fully evaporate the solvent in the photoresist, reduce the film stress of the photoresist during high-speed rotation, and avoid photoresist delamination; (3) Photolithography exposure: The silicon wafer obtained in (2) is aligned with the photolithography machine, and the light emitted by the ultraviolet light source of the photolithography machine shines through the first mask 01 (Si-Topchannels) onto the photoresist on the top layer of the silicon wafer to activate the photosensitive components in the photoresist, thereby obtaining the internal mesh on the top surface of the silicon wafer. Basic shape; (4) Development and hardening: The silicon wafer exposed in (3) is soaked in the developer solution and developed. Oxygen plasma is used to bombard the surface of the silicon wafer to remove the residual photoresist on the surface. Then the silicon wafer is placed on the baking table for post-baking to remove the solvent remaining in the photoresist after development, and to improve the adhesion of the photoresist on the surface of the silicon wafer and its resistance to etching; (5) Front etching: C4F8 and SF6 gas in the DRIE deep reactive ion etching machine bombard the surface of the silicon wafer to transfer the pattern on the photoresist layer to the silicon wafer; (6) Back etching: Repeat steps (1)-(4). During photolithography exposure, the shape of the internal mesh of the bottom surface of the silicon wafer is defined by the second mask 02 (Si-Bottom) with alignment marks. The surface of the silicon wafer is etched by DRIE deep reactive ion etching until silicon through-holes are formed; (7) Standard cleaning: The surface of the silicon wafer is cleaned according to the standard cleaning process.
[0033] In one embodiment of the present invention, after this step, the following operation is also required: It should be explained that if the unit atomic gas chamber is a single-chamber atomic gas chamber, then the number of internal mesh openings in the unit atomic gas chamber is 1, thus forming a single-chamber atomic gas chamber. If the number of internal mesh openings in the unit atomic gas chamber is 2, then a double-chamber atomic gas chamber is formed, consisting of a light-atom interaction chamber and a chemical reaction chamber. A heater, a thermistor, and Au-Si pads connected to the heater and the thermistor are fabricated circumferentially on the top of the single-chamber or light-atom interaction chamber of the etched silicon wafer. The specific fabrication steps are as follows: S21 sequentially performs vapor deposition, homogenization and pre-baking, photolithography exposure, and development on the top surface of the silicon wafer, transferring the pattern on the mask with alignment marks to the top surface of the silicon wafer. S22 uses magnetron sputtering to sequentially deposit Ti and Pt on the top surface of a silicon wafer to prepare a heater and a thermistor. The magnetron sputtering of the Ti and Pt layers is performed by a stripping method. S23 sequentially performs vapor deposition, homogenization and pre-baking, photolithography exposure, and development on the top surface of the silicon wafer after step S22. The pattern on another mask with alignment marks is transferred to the top surface of the silicon wafer, and Au-Si pads are prepared by depositing Au using magnetron sputtering.
[0034] More specifically, the general steps for preparing heaters, thermistors, and Au-Si pads are explained: following steps (1)-(4) in the deep silicon etching process, vapor deposition, homogenization and pre-baking, photolithography exposure, and development are performed to transfer the pattern on the third mask 03 (Si-Ti-Pt) with alignment marks to the top surface of the silicon wafer. The heater and thermistor are prepared by sequentially depositing Ti and Pt using magnetron sputtering. The magnetron sputtering of the Ti layer and the Pt layer is performed by stripping. Similarly, following steps (1)-(4) in the deep silicon etching process, vapor deposition, homogenization and pre-baking, photolithography exposure, and development are performed to transfer the pattern on the fourth mask (Si-Au) with alignment marks to the top surface of the silicon wafer. The Au-Si pads are prepared by depositing Au using magnetron sputtering.
[0035] Among them, the pad lead contact hole can bring out the Au-Si pad on the silicon wafer surface to the top borosilicate glass surface to enable subsequent functions.
[0036] In addition, to accommodate the shapes of the heater, thermistor, and Au-Si pads and to prevent the glass or silicon wafer from being crushed during the bonding process, shallow U-grooves are etched on the bottom surface of the top borosilicate glass to fit the shapes of the heater, thermistor, and Au-Si pads.
[0037] S4: The silicon wafer 2 obtained in step S3 is bonded to the top borosilicate glass 1 with silicon-glass anode bonding to form two layers of pre-bonded wafers; In this step, the silicon-glass anodic bonding and glass-silicon-glass anodic bonding steps are as follows: pre-bonding cleaning → mechanical alignment of silicon wafer 2 and top borosilicate glass 1 and placement into the bonding cavity → vacuuming of the bonding machine → application of pressure → heating of the equipment, heating of the silicon wafer-glass substrate → application of voltage → cooling → bonding completion to form two pre-fabricated bonded sheets. The above anodic bonding steps, especially "application of pressure → heating of the equipment, heating of the silicon wafer-glass substrate → application of voltage," employ a method of applying pressure first, then heating the silicon-glass substrate, and finally applying voltage. This makes it less likely for the alkali metal filled in the vacuum, anhydrous, and oxygen-free environment to escape from the mesh, which is particularly important when preparing single-chamber atomic gas cells. Furthermore, this method can accelerate the ion migration rate in the silicon wafer and glass substrate, resulting in tighter Si-O bonds formed on the surfaces of the silicon wafer and glass substrate, enhancing the bonding quality of the atomic gas cell and increasing the overall reliability of the atomic gas cell.
[0038] In the above steps, the shape of the cathode during anodic bonding also affects the bonding effect. In this invention, a cross-shaped line electrode made of graphite is used for anodic bonding, which not only reduces the generation of voids at the bonding interface but also improves the bonding rate compared to point electrode bonding. Commonly used anodic bonding cathodes are generally point contact electrodes and double parallel plate electrodes. The bonding interface of a point contact electrode does not generate voids, while the bonding interface of a double parallel plate electrode has some pores. The bonding rate is higher than that of a point contact electrode, but the bonding efficiency of point charges is much lower than that of a double parallel plate electrode. Line electrode bonding combines the advantages of point contact electrodes and double parallel plate electrode bonding, ensuring both bonding quality and bonding rate.
[0039] In one embodiment, when the anodic bonding temperature is around 300°C, the thermal expansion coefficients of the borosilicate glass and the silicon wafer are well matched and consistent at this temperature. In particular, the thermal expansion coefficients of Pyrex 7740 glass and the silicon wafer are very well matched and consistent, resulting in uniform internal stress distribution and a high-quality sealing of the three-layer glass-silicon-glass anodic bonding sealed wafer. The top and bottom borosilicate glass types that can be used to fabricate this quantum sensor device include, but are not limited to, the following: Pyrex 7740, BF33, Corning 7070, soda lime 0080, potassium soda lead 0120, and aluminosilicate 1720.
[0040] More specifically, the silicon wafer and the top borosilicate glass are optically aligned and mounted on a bonding tray, then fed into the bonding cavity for anodic bonding to form two pre-fabricated bonding sheets. During this process, the bonding vacuum is <1×10-5mbar, the bonding electrode voltage is 1000V, the bonding pressure is 1000N, and the bonding surfaces are the top surface of the silicon wafer and the side of the top borosilicate glass with a shallow U-groove.
[0041] S5: If the atomic gas chamber is a single-chamber atomic gas chamber, then the alkali metal element is filled into the single-chamber light-atom interaction cavity mesh of the two-layer pre-bonded sheet. If the atomic gas chamber is a double-chamber atomic gas chamber, then the alkali metal release agent is filled into the double-chamber chemical reaction cavity mesh of the two-layer pre-bonded sheet.
[0042] In the above steps, the silicon wafer is etched according to the arrangement of the internal mesh. If the internal mesh of the unit atomic gas chamber is 1, a single-cavity gas chamber is formed. If the internal mesh of the unit atomic gas chamber is 2, a double-cavity gas chamber is formed, consisting of a light-atomic interaction cavity and a chemical reaction cavity.
[0043] S6: The two pre-fabricated bonding sheets processed in step S5 and the bottom borosilicate glass sheet 6 are subjected to glass-silicon-glass anodic bonding in a buffer gas atmosphere to form a three-layer sealed cavity bonding sheet.
[0044] More specifically, two layers of pre-fabricated bonding sheets and a bottom borosilicate glass sheet are mounted on the bonding tray of the bonding machine through optical alignment. The two pre-fabricated bonding sheets are connected to the bottom borosilicate glass sheet, which is connected to the top heating source. The top borosilicate glass sheet of the two pre-fabricated bonding sheets is connected to the bottom heating source. Simultaneously, a thick gasket on the bonding tray creates a gap between the two pre-fabricated bonding sheets and the bottom borosilicate glass sheet, allowing buffer gas to enter the light-atom interaction cavity or the light-atom interaction cavity and chemical reaction cavity. Both the top and bottom heating sources are heated to the bonding temperature. The bonding cavity inside the bonding machine is evacuated to a vacuum level <1×10⁻⁶. -5 After maintaining the vacuum for 30 minutes, a buffer gas is introduced and kept for a period of time to allow the buffer gas to diffuse into the light-atom interaction cavity or the light-atom interaction cavity and the chemical reaction cavity. The top heating source applies a pressure of 1000N to the bottom borosilicate glass sheet, and the bonding electrode voltage is 1000V to form a three-layer sealed cavity bonding sheet.
[0045] Furthermore, the atomic gas chamber needs to be filled with a mixed buffer gas to suppress linear temperature shifts. Since frequency shifts in different directions are caused by buffer gas atoms or molecules with different shift coefficients, mixing easily polarizable and non-polarizable buffer gas atoms or molecules in a certain proportion plays a crucial role in suppressing linear temperature shifts. For multi-part atomic gas chambers, this invention proposes filling the chamber with two buffer gases of different properties mixed in a certain proportion, such as: Ar-N2 mixed buffer gas, Ar-CH4 mixed buffer gas, Kr-N2 mixed buffer gas, or Ar-Ne mixed buffer gas. The proportions of the mixed buffer gases are as follows: r(P) Ar / P N2 )=1.6, r(P Ar / PCH4 )=1.8, r(P Kr / P N2 )=0.9, r(P Ar / P Ne = 0.8. Where r(x / y) is a proportional function, which is the ratio of x to y.
[0046] S7: Based on the shape and size of the unit atomic gas chamber in step S1, dicing and machining a three-layer sealing cavity bonding sheet to obtain a unitized single-chamber atomic gas chamber or a double-chamber atomic gas chamber; Prior to this, the following operations are required: A Cr adhesion layer is sputtered onto the top borosilicate glass of the three-layer sealed cavity bonding sheet to enhance the adhesion between the top borosilicate glass surface and the seed layer Au; the seed layer Au is electroplated onto the Cr adhesion layer as the raw material for preparing the electrode leads and Au-Glass pads; the top borosilicate glass treated in the above steps undergoes vapor deposition, homogenization and pre-baking, photolithography exposure, and development to transfer the pattern on the mask with alignment marks to the surface of the top borosilicate glass, thus patterning the electrode leads and Au-Glass pads; the patterned electrode leads and Au-Glass pads are etched to form the electrode leads and Au-Glass pads; the three-layer sealed cavity bonding sheet treated in the above steps is annealed to achieve metal alloying of the electrode leads and Au-Glass pads.
[0047] S8: For a single-chamber atomic gas chamber, the single-chamber atomic gas chamber is heated to release alkali metal atoms in the alkali metal element. For a double-chamber atomic gas chamber, its interior is filled with an alkali metal releasing agent and heated to a certain temperature to release alkali metal atoms in the alkali metal releasing agent.
[0048] In this step, a laser is used to irradiate the alkali metal releasing agent inside the atomic gas chamber to release alkali metal atoms from the alkali metal releasing agent. The unitized atomic gas chambers are then tested and screened to obtain unitized atomic gas chambers whose performance meets the standards.
[0049] S9: Test and screen the atomic gas chambers obtained in step S8.
[0050] The above method for testing and screening modular MEMS atomic gas chambers includes obtaining the absorption spectra of alkali metal atoms corresponding to the MEMS atomic gas chambers on a constructed optical platform. For example, to test the absorption spectrum corresponding to rubidium (Rb) atoms, a 795nm laser is required, and to test the absorption spectrum corresponding to cesium (Cs) atoms, an 852nm laser is required. Furthermore, this invention directly heats the alkali metal releasing agent within the gas chamber using a heater, and simultaneously irradiates it with a laser to obtain the absorption spectra of the alkali metal atoms corresponding to the atomic gas chambers. Further, this invention connects the thermistor and heater to a controller to form a PID closed-loop control, ensuring that the heating temperature of the gas chamber remains consistent with the desired heating temperature under the action of the thermistor and heater.
[0051] This invention relates to a high-sealing multi-gas atomic chamber packaging method based on an irregularly arranged array. Different structures and shapes of atomic chamber meshes on the silicon wafer surface are arranged in a specific array to form a non-uniform, irregularly arranged array. The mesh array shapes include, but are not limited to, cross-shaped, square, hexagonal, octagonal, circular, and star-shaped. Based on the number of meshes, the gas chambers are divided into single-chamber gas chambers and double-chamber gas chambers. The shape of a single mesh in a single-chamber or double-chamber gas chamber includes, but is not limited to, triangles, squares, hexagons, octagons, dodecagons, and circles. From the perspective of the array shape, this arrangement results in greater deformation of the atomic gas cell mesh closest to the edge of the silicon wafer compared to other internal meshes during silicon-glass anodic bonding and glass-silicon-glass anodic bonding. At relatively high anodic bonding temperatures, the closely contacting silicon wafer and the borosilicate glass surface undergo a chemical reaction, forming strong chemical bonds, such as Si-O-Si bonds, thus enhancing bonding quality. Compared to traditional atomic gas cell fabrication methods, this non-uniform irregular array eliminates the need for fabricating meshes at the edge of the silicon wafer surface. Under high voltage, the Na in the glass... + It can react more easily with anions on the surface of more silicon wafers, forming a depletion layer several micrometers wide on the glass surface. The depletion layer carries a negative charge, while the silicon wafer carries a positive charge. There is a strong electrostatic attraction between the silicon wafer and the borosilicate glass, allowing their surfaces to make close contact to form a highly sealed atomic chamber encapsulation. During encapsulation, the anode bonding cathode uses a cross-shaped graphite wire electrode for anode bonding, which not only reduces the generation of bonding interface voids but also improves the bonding rate compared to point electrode bonding. To suppress the linear temperature shift inside the atomic chamber, the atomic chamber needs to be filled with a mixture of easily polarizable buffer gas atoms or molecules and non-polarizable buffer gas atoms or molecules to form a highly sealed, multi-gas atomic chamber. The atomic chamber prepared by this encapsulation method can achieve the goals of miniaturization and micro-miniaturization with small volume and low power consumption.
[0052] The atomic gas cell prepared by the method provided in this invention has the advantages of small size and miniaturization, and is easy to mass-produce in arrays. It is suitable for application in quantum sensor devices such as atomic clocks, magnetometers, and MEMS gyroscopes.
[0053] That is, the present invention also provides a product prepared by the above method, comprising a top layer of borosilicate glass, a silicon wafer, and a bottom layer of borosilicate glass bonded sequentially, wherein, The top borosilicate glass is provided with Au-Glass pads, electrode leads and pad lead contact holes. The Au-Glass pads are connected to the electrode leads. The pad lead contact holes penetrate the top borosilicate glass and are corresponding to the ends of the electrode leads. The silicon wafer is provided with a single-chamber light-atom interaction cavity, or a dual-chamber light-atom interaction cavity and a chemical reaction cavity connected in series. A heater and a thermistor are provided circumferentially at the top of the light-atom interaction cavity. The heater and the thermistor are electrically connected to the Au-Si pads respectively. The Au-Si pads are correspondingly provided with pad lead contact holes. The bottom borosilicate glass is used to encapsulate the bottom surface of the silicon wafer to form a sealed single or double chamber.
[0054] Furthermore, a shallow U-groove is provided on the side of the top borosilicate glass bonded to the silicon wafer to accommodate the heater, the thermistor, and the Au-Si pad. The heater is formed by sequentially depositing Ti, Pt, and Au.
[0055] Furthermore, an alkali metal releasing agent is placed within the chemical reaction chamber. This alkali metal releasing agent can release alkali metal atoms when heated to a certain temperature.
[0056] This invention also provides a method for using the above-mentioned product: During use, the atomic gas chamber is directly heated by a heater, and the heating temperature of the atomic gas chamber is controlled by the combined action of a thermistor and the heater. The heater and the thermistor are directly located on the silicon-glass bonded surface of the atomic gas chamber, enabling direct heating of the chamber itself, reducing heat dissipation, and saving the time required to reach the desired temperature.
[0057] Those skilled in the art will readily understand that the above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for encapsulating highly sealed multi-gas atomic chambers with irregularly arranged arrays, characterized in that, Includes the following steps: S1 determines the shape and size of the unit atomic gas cell based on the internal mesh of the atomic gas cell; S2 designs the arrangement of internal mesh holes on the silicon wafer based on the deformation during the silicon wafer heating and bonding process. S3 etches the silicon wafer according to the arrangement of the internal mesh holes; S4 involves performing silicon-glass anodic bonding between the silicon wafer obtained in step S3 and the top borosilicate glass to form two pre-bonded wafers. S5 If the atomic gas chamber is a single-chamber atomic gas chamber, then the alkali metal element is filled into the light-atom interaction cavity mesh of the single-chamber of the two-layer pre-bonded sheet. If the atomic gas chamber is a double-chamber atomic gas chamber, then the alkali metal release agent is filled into the chemical reaction cavity mesh of the double-chamber of the two-layer pre-bonded sheet. S6 involves performing glass-silicon-glass anodic bonding on the two pre-fabricated bonding sheets and the bottom borosilicate glass sheet after step S5 in a multi-gas buffer gas atmosphere to form a three-layer sealed cavity bonding sheet. S7 According to the shape and size of the unit atomic gas chamber in step S1, the three-layer sealing cavity bonding sheet is diced and processed to obtain a unitized single-chamber atomic gas chamber or double-chamber atomic gas chamber. For a single-chamber atomic gas chamber, S8 heats the single-chamber atomic gas chamber to release alkali metal atoms in the alkali metal element; for a double-chamber atomic gas chamber, it is filled with an alkali metal releasing agent and heated to a certain temperature to release alkali metal atoms in the alkali metal releasing agent. S9 tests and screens the atomic gas chambers obtained in step S8; step S2 specifically includes the following steps: based on the properties of silicon wafers, sets the heating conditions during the silicon wafer heating bonding process, as well as the shape of the edge sacrificial layer and the shape of the internal mesh during the bonding process, and simulates the deformation during the silicon wafer heating bonding process to obtain an internal mesh arrangement with the fewest edge sacrificial layers and the most internal meshes in the edge sacrificial layer.
2. The method for encapsulating a highly sealed multi-gas atomic chamber with an irregularly arranged array according to claim 1, characterized in that, It is also necessary to consider the amount of Na+ in the glass bonded to the silicon wafer during the bonding process. That is, the glass outside the edge sacrificial layer can provide more Na+ to react with the anions on the surface of the silicon wafer to form a depletion layer with a width of a few micrometers on the glass surface. The depletion layer carries a negative charge, the silicon wafer carries a positive charge, and there is a large electrostatic attraction between the silicon wafer and the borosilicate glass, which makes the two come into close contact.
3. The method for encapsulating a highly sealed multi-gas atomic chamber with an irregularly arranged array according to claim 1, characterized in that, In step S3, the silicon wafer is etched according to the arrangement of the internal mesh. If the number of internal meshes in the unit atomic gas chamber is 1, a single-chamber atomic gas chamber is formed. If the number of internal meshes in the unit atomic gas chamber is 2, a double-chamber atomic gas chamber is formed, consisting of a light-atomic interaction chamber and a chemical reaction chamber.
4. The method for encapsulating a highly sealed multi-gas atomic chamber with an irregularly arranged array according to claim 1, characterized in that, Before step S4, the following operations are required: A heater, a thermistor, and Au-Si pads connected to the heater and the thermistor are fabricated circumferentially on the top of the single-chamber atomic gas chamber of the etched silicon wafer. The specific fabrication steps are as follows: S31 sequentially performs vapor deposition, homogenization and pre-baking, photolithography exposure, and development on the top surface of the silicon wafer, transferring the pattern on the mask with alignment marks to the top surface of the silicon wafer. S32 uses magnetron sputtering to sequentially deposit Ti and Pt on the top surface of a silicon wafer to prepare a heater and a thermistor. The magnetron sputtering of the Ti and Pt layers is performed by a stripping method. S33 sequentially performs vapor deposition, homogenization and pre-baking, photolithography exposure, and development on the top surface of the silicon wafer after step S32. The pattern on another mask with alignment marks is transferred to the top surface of the silicon wafer, and Au-Si pads are prepared by depositing Au using magnetron sputtering.
5. The method for encapsulating a highly sealed multi-gas atomic chamber with an irregularly arranged array according to claim 4, characterized in that, After step S32 and before step S4, the following operations also need to be performed: Shallow U-grooves are etched on the bottom surface of the top borosilicate glass to conform to the shape of the heater, thermistor, and Au-Si pads.
6. The method for encapsulating a highly sealed multi-gas atomic gas chamber with an irregularly arranged array according to claim 5, characterized in that, In step S4, the silicon wafer and the top borosilicate glass are optically aligned and mounted on a bonding tray, then fed into the bonding cavity for anodic bonding to form two pre-fabricated bonding layers. During this process, the bonding vacuum degree is <1×10⁻⁶. -5 mbar, bonding electrode voltage is 1000V, bonding pressure is 1000N, and the bonding surface is the top surface of the silicon wafer and one side of the shallow U-groove of the top borosilicate glass strip.
7. The method for encapsulating a highly sealed multi-gas atomic gas chamber with an irregularly arranged array according to claim 6, characterized in that, In step S6, two layers of pre-fabricated bonding sheets and a bottom borosilicate glass sheet are optically aligned and mounted on the bonding tray of the bonding machine. The two pre-fabricated bonding sheets are connected to the bottom borosilicate glass sheet, which is connected to the top heating source. The top borosilicate glass sheet of the two pre-fabricated bonding sheets is connected to the bottom heating source. Simultaneously, a thick gasket on the bonding tray creates a gap between the two pre-fabricated bonding sheets and the bottom borosilicate glass sheet, allowing buffer gas to enter the light-atom interaction cavity or the light-atom interaction cavity and chemical reaction cavity. Both the top and bottom heating sources are heated to the bonding temperature. The bonding cavity inside the bonding machine is evacuated to a vacuum level <1×10⁻⁶. -5 After maintaining the vacuum for 30 minutes, a buffer gas is introduced and kept for a period of time to allow the buffer gas to diffuse into the light-atom interaction cavity or the light-atom interaction cavity and the chemical reaction cavity. The top heating source applies a pressure of 1000N to the bottom borosilicate glass sheet, and the bonding electrode voltage is 1000V to form a three-layer sealed cavity bonding sheet.
8. The method for encapsulating a highly sealed multi-gas atomic chamber with an irregularly arranged array according to claim 1, characterized in that, Before step S7, the following operations must be performed: A layer of Cr metal is sputtered onto the top borosilicate glass of the S61 three-layer sealed cavity bonding sheet to enhance the adhesion between the surface of the top borosilicate glass and the seed layer metal Au. S62 uses Au seed layer metal electroplated on the adhesion layer metal Cr as the raw material for preparing electrode leads and Au-Glass pads. S63 performs vapor deposition, homogenization and pre-baking, photolithography exposure and development on the top borosilicate glass after the above step S62, so as to transfer the pattern on the mask with alignment marks to the surface of the top borosilicate glass, thereby patterning the electrode leads and Au-Glass pads. S64 etches the patterned electrode leads and Au-Glass pads to form the electrode leads and Au-Glass pads. S65 performs annealing on the three-layer sealed cavity bonding sheet processed in step S64 above to achieve metal alloying of the electrode leads and Au-Glass pads.
9. The method for encapsulating a highly sealed multi-gas atomic gas chamber with an irregularly arranged array according to claim 1, characterized in that, In step S6, the buffer gas includes an Ar-N2 mixed buffer gas, an Ar-CH4 mixed buffer gas, or a K gas mixed in a certain proportion. r -N2 mixed buffer gas or A r -N e Mixed buffer gas; If it is an Ar-N2 mixed buffer gas, r(P) Ar / P N2 )=1.6, if it is an Ar-CH4 mixed buffer gas, r(P Ar / P CH4 )=1.8, if it is K r -N2 mixed buffer gas, r(P Kr / P N2 If ) = 0.9, then it is A r -N e Mixed buffer gas, r(P) Ar / P Ne )=0.8, where r is a proportional function.
10. An atomic gas chamber, characterized in that, It is prepared by the method described in any one of claims 1-6.
11. The atomic gas chamber according to claim 10, characterized in that, This includes a top layer of borosilicate glass, a silicon wafer, and a bottom layer of borosilicate glass bonded sequentially. The top borosilicate glass is provided with Au-Glass pads, electrode leads and pad lead contact holes. The Au-Glass pads are connected to the electrode leads. The pad lead contact holes penetrate the top borosilicate glass and are corresponding to the ends of the electrode leads. The silicon wafer is provided with a single-chamber light-atom interaction cavity, or a dual-chamber light-atom interaction cavity and a chemical reaction cavity connected in series. A heater and a thermistor are provided on the top circumferential direction of the light-atom interaction cavity. The heater and the thermistor are electrically connected to the Au-Si pads respectively. The Au-Si pads are provided with corresponding pad lead contact holes. The bottom borosilicate glass is used to encapsulate the bottom surface of the silicon wafer to form a sealed single or double chamber.
12. A method of using an atomic gas chamber, characterized in that, The atomic gas chamber as described in claim 11 is used in which the atomic gas chamber is directly heated by a heater during use, and the heating temperature of the atomic gas chamber is controlled by the combined action of a thermistor and the heater.
Citation Information
Patent Citations
Wafer level chip size atomic vapor chamber encapsulating method
CN104555905A
Wafer-level atomic gas chamber processing method and device based on MEMS technology
CN114477074A