A light sintered microcrystalline plate and sintering process thereof

By laying glass particles of different sizes in the refractory mold and adjusting the composition of the glass solution, the problems of thickness and weight of the microcrystalline plates are solved, and the high strength and low weight of the lightweight sintered microcrystalline plates are achieved, which is suitable for lightweight building materials. .

CN115745380BActive Publication Date: 2024-10-01SUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211345879.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-31
Publication Date
2024-10-01
Estimated Expiration
2042-10-31

AI Technical Summary

Technical Problem

The existing microcrystalline plates are thicker, resulting in increased weight and unable to meet the structural design requirements of lightweight and prefabricated buildings. At the same time, the thin plates affect the compressive strength and pose safety risks.

Method used

Using the steps of glass particle preparation, ball milling classification, distribution, sintering crystallization and cold processing, glass particles of different particle sizes are laid in different grooves of the refractory mold to form a reinforced structure and adjust the composition of the glass solution to achieve large-sized lightweight sintered micro-structures. Forming of crystal plates.

Benefits of technology

It significantly improves the load-bearing capacity and structural strength of the lightweight microcrystalline plate, reduces the shrinkage during the sintering process, ensures the light weight and high strength of the plate, and is suitable for lightweight building materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115745380B_ABST
    Figure CN115745380B_ABST
Patent Text Reader

Abstract

The invention relates to a lightweight sintered microcrystalline plate and a sintering process thereof, comprising the steps of glass particle preparation, ball milling classification, material distribution, sintering crystallization and cold processing; the material distribution comprises spreading the glass particles over a first groove and a second groove of a refractory mold, wherein the second groove is opened at the bottom of the first groove, the depth of the first groove is 5 mm-20 mm, the depth of the second groove is 3 mm-40 mm, and the particle size of the glass particles in the first groove is different from the particle size of the glass particles in the second groove. The beneficial effects of the present invention are as follows: by adjusting the glass solution to include 40% to 70% SiO2, 8% to 20% CaO, 4% to 12% MgO, 5% to 20% Al2O3 and 2% to 8% Na2O, and then quenching the glass solution with water, and sieving and distributing the glass particles obtained by the water quenching, the sintering forming of a large-sized lightweight sintered microcrystalline plate is achieved, and the shrinkage during the sintering process that makes it impossible for the glass particles to be reliably combined is prevented, the degree of combination between the reinforcement structure and the microcrystalline plate body is significantly enhanced, and the bearing capacity of the lightweight sintered microcrystalline plate is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of microcrystalline plate preparation, in particular to a lightweight sintered microcrystalline plate and a sintering process thereof. Background Art

[0002] Lightweight and prefabricated building design is one of the mainstream directions of current building development. Lightweight and prefabricated building design has outstanding significance for reducing resource and energy consumption in the preparation and processing of building materials. At present, in order to ensure the structural strength, the thickness of sintered microcrystalline panels is basically 18-30mm, and the density is 2.5-3.2g·cm-3, which is generally heavy; taking the 1200*800*20mm microcrystalline panel as an example, the weight of a single microcrystalline panel can reach 48-61.4kg, which not only greatly increases the load-bearing pressure on the building itself, but also cannot bear the structural design requirements of prefabricated buildings. At the same time, it restricts the transportation and installation efficiency of microcrystalline panels. Therefore, the lightweight design and processing of microcrystalline panels are particularly important. However, if the panel is too thin, it will affect the overall compressive strength and cause safety hazards.

[0003] Patent CN96114108.5 invented a method for preparing special-shaped microcrystalline glass plates by sintering. It adopts high-temperature molding, and uses the characteristics of microcrystalline glass blanks softening and deforming at high temperatures to press the blanks into shape at high temperatures with a mold. Patent CN200610043667.5 uses optimized glass particle size distribution to pave the material, compacts it with a roller, and uses SiO2 powder as an interlayer to prepare ultra-thin microcrystalline glass. It prepares ultra-thin microcrystalline glass panels with a molding thickness of about 2~5mm. Patent CN202010292506.X invented a method for preparing iron-selected tailings microcrystalline glass by sintering fumed slag. The mother blank is prepared by powder granulation and mold pressure molding, and then sintered into shape. Summary of the invention

[0004] In order to overcome at least some of the defects in the prior art, the embodiments of the present invention provide a lightweight sintered microcrystalline plate and a sintering process thereof, which have a simple structure and are easy to use.

[0005] The present invention relates to a sintering process of a microcrystalline plate, comprising the steps of glass particle preparation, ball milling classification, material distribution, sintering crystallization and cold processing;

[0006] The material distribution comprises the following steps: the glass particles are spread over the first groove and the second groove of the refractory mold, the second groove is opened at the bottom of the first groove, the depth of the first groove is 5mm-20mm, the depth of the second groove is 3mm-40mm, the particle size of the glass particles in the first groove is different from the particle size of the glass particles in the second groove, and the particle diameter of the particles in the first groove is generally larger than the diameter of the particles in the second groove;

[0007] The sintering crystallization includes the following steps: transferring the refractory mold covered with glass particles during the laying process to a sintering kiln, heating to 1000-1200°C at 8-12°C / min and keeping warm for 1-3 hours to complete sintering crystallization, forming a microcrystalline plate body in the first groove during the crystallization process, forming a reinforcing structure connected to the microcrystalline plate body in the second groove, cooling to 580-670°C at 4-8°C / min and keeping warm for 0.5-1 hour to remove internal residual stress, completing annealing, cooling at 6-10°C / min, and then cooling to room temperature and taking out of the kiln to obtain a lightweight microcrystalline glass slab.

[0008] Furthermore, the refractory mold includes a detachable first template and a second template, the first groove is opened on the upper surface of the first template and the first groove horizontally passes through the first template, and the second groove is opened on the upper surface of the second template.

[0009] Furthermore, the preparation of the glass particles includes the following steps: the raw materials are mixed and then sent into a glass melting furnace, melted at a temperature of 1400-1650°C and internal gas is removed to obtain a uniform glass solution, and the molten uniform glass liquid is discharged into water after clarification to obtain water-quenched glass particles.

[0010] Furthermore, the glass solution comprises 40% to 70% SiO2, 8% to 20% CaO, 4% to 12% MgO, 5% to 20% Al2O3 and 2% to 8% Na2O by weight.

[0011] Furthermore, the distribution includes the following steps: the second groove part in the refractory mold is evenly filled with glass particles larger than 16 meshes, and the first groove part is evenly filled with glass particles of 5-60 meshes, and the second grooves are distributed at the bottom of the first groove in parallel strips, I-shape, tic-tac-toe, cylindrical or square shapes.

[0012] Furthermore, the refractory mold is made of a refractory material that is resistant to high temperatures and has a small thermal expansion coefficient.

[0013] Furthermore, the refractory material is a spinel refractory board, a SiC refractory board, a mullite refractory board and a corundum refractory board.

[0014] Furthermore, the method includes placing the water-quenched glass particles into a ball mill for ball milling, and screening the milled glass materials.

[0015] The present invention also provides a lightweight sintered microcrystalline plate, which is prepared by a sintering process.

[0016] The beneficial effect of the present invention is that by adjusting the composition of the glass solution to include 40% to 70% SiO2, 8% to 20% CaO, 4% to 12% MgO, 5% to 20% Al2O3 and 2% to 8% Na2O, and then quenching the glass solution, the glass particles obtained by quenching are screened and distributed, thereby realizing the sintering molding of a large-sized lightweight sintered microcrystalline plate, preventing the glass particles from being unable to be reliably combined due to shrinkage during the sintering process, significantly strengthening the combination degree between the reinforcement structure and the microcrystalline plate body, and improving the bearing capacity of the lightweight sintered microcrystalline plate.

[0017] In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are specifically cited below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 This is a structural diagram of a refractory mold.

[0020] Figure 2 It is a structural schematic diagram of another structure of a refractory mold.

[0021] Figure 3 yes Figure 2 Schematic diagram of the cross-sectional structure.

[0022] Figure 4 The following is a performance comparison chart of the plates obtained in the embodiment and the comparative example. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1

[0024] Reference Figure 2 and Figure 3 In a preferred embodiment of the present invention, a sintering process of a microcrystalline plate includes glass particle preparation, ball milling classification, material distribution, sintering crystallization and cold working steps;

[0025] The spreading process includes the following steps: the glass particles are spread over the first groove and the second groove of the refractory mold, the second groove is opened at the bottom of the first groove, the depth of the first groove is 12 mm, the depth of the second groove is 20 mm, and the particle size of the glass particles in the first groove is different from the particle size of the glass particles in the second groove; in the actual implementation process, the refractory mold includes a detachable first template and a second template, the first groove is opened on the upper surface of the first template and is closed below the first groove, the second template includes a plurality of strip plates overlapped on the first template, the inner wall of the first template is provided with a positioning groove for overlapping the strip plates, the adjacent strip plates and the inner wall of the first template are jointly arranged to form the second groove, and the cross-sections of the first groove and the second groove are both rectangular.

[0026] By arranging the second groove forming the reinforcement structure above the first groove, the pressure of the upper glass particles on the lower glass particles can be reduced, and the shrinkage amount can be significantly reduced during the glass crystallization shrinkage process, thereby improving the final crystallization quality.

[0027] The sintering crystallization includes the following steps: transferring the refractory mold covered with glass particles during the laying process to a sintering kiln, heating to 1000°C at 8°C / min and keeping warm for 1-3 hours to complete sintering crystallization, cooling to 580°C at 4°C / min and keeping warm for 0.5 hours to remove internal residual stress, completing annealing, cooling at 6°C / min, and then cooling to room temperature before taking out of the kiln to obtain a lightweight microcrystalline glass slab, and then obtaining a lightweight sintered microcrystalline board through cold working. The lightweight microcrystalline glass slab includes a reinforcing structure formed in the second groove and a microcrystalline board body formed in the first groove.

[0028] In the above embodiment, the preparation of the glass particles includes the following steps: the raw materials are mixed and then sent into a glass melting furnace, melted at a temperature of 1400°C and the internal gas is removed to obtain a uniform glass solution, and the molten uniform glass liquid is discharged into water after clarification to obtain water-quenched glass particles.

[0029] In the above embodiment, the glass solution includes 40% to 70% SiO2, 8% to 20% CaO, 4% to 12% MgO, 5% to 20% Al2O3 and 2% to 8% Na2O by weight.

[0030] In the above embodiment, the material distribution includes the following steps: the second groove part of the refractory mold is evenly covered with 20-mesh glass particles, and the first groove part is evenly covered with 30-mesh glass particles.

[0031] In the above embodiment, the refractory mold is made of a refractory material that is resistant to high temperatures and has a small thermal expansion coefficient.

[0032] In the above embodiments, the refractory material is a spinel refractory board, a SiC refractory board, a mullite refractory board and a corundum refractory board.

[0033] In the above embodiment, the method includes placing the water-quenched glass particles into a ball mill for ball milling, and screening the milled glass materials.

[0034] In the above embodiment, the second grooves are distributed at the bottom of the first groove in the shape of parallel strips, an I-shape, a well-shape, a cylinder or a grid. Example 2

[0035] Its main features are the same as those of Example 1, except that the depth of the first groove is 5 mm, and the depth of the second groove is 3 mm. Example 3

[0036] Its main features are the same as those of Example 1, except that the depth of the first groove is 5 mm, and the depth of the second groove is 20 mm. Example 4

[0037] Its main features are the same as those of Example 1, except that the depth of the first groove is 20 mm, and the depth of the second groove is 40 mm. Example 5

[0038] Its main features are the same as those of Example 1, except that the depth of the first groove is 12 mm, and the depth of the second groove is 3 mm. Example 6

[0039] Its main features are the same as those of Example 1, except that the depth of the first groove is 12 mm, and the depth of the second groove is 40 mm. Example 7

[0040] Its main features are the same as those of Example 1, except that the depth of the first groove is 20 mm, and the depth of the second groove is 3 mm.

[0041] Reference Figure 1 Indeed, in other embodiments, the refractory mold includes a detachable first template and a second template, the first groove is opened on the upper surface of the first template and the first groove horizontally passes through the first template, and the second groove is opened on the upper surface of the second template.

[0042] The present invention also provides a lightweight sintered microcrystalline plate, which is prepared by the sintering process of the microcrystalline plate in any of the above embodiments.

[0043] Comparative Example 1

[0044] Its main features are the same as those of Example 1, except that the refractory mold is a flat mold with a groove.

[0045] Comparative Example 2

[0046] Its main features are the same as those of Example 1, except that the second groove portion in the refractory mold is evenly covered with 30-mesh glass particles, and the first groove portion is evenly covered with 20-mesh glass particles. In other embodiments, attempts are also made to set the glass particles used in the first groove and the second groove to be consistent, and it is found that the glass particles in the first groove and the second groove will be clearly layered.

[0047] In order to further illustrate the lightweight sintered microcrystalline plate prepared by the present invention, the performance of the lightweight sintered microcrystalline plate produced in the embodiment and the comparative example was tested. The test results are as follows: Figure 4 As shown: By comparing the embodiment and comparative example 1, it can be found that the lightweight structure enhanced microcrystalline board prepared by the refractory mold of the present invention can ensure that the lightweight structure enhanced microcrystalline board still has good structural strength while reducing the thickness and weight. By comparing the embodiment and comparative example 2, it can be found that the compressive strength of comparative example 2 is better than that of the embodiment, and the longitudinal flexural strength and the transverse flexural strength are both lower than those of the embodiment. Since the lightweight structure enhanced microcrystalline board as a building material has a low demand for compressive strength, the comprehensive performance of the lightweight structure enhanced microcrystalline board obtained in the embodiment is better than that of comparative example 2.

[0048] From a comprehensive comparison of Examples 1 to 7, it can be found that the comprehensive strength of the lightweight structure enhanced microcrystalline board obtained in Example 5 is the best. Although the lightweight structure enhanced microcrystalline board of Example 1 has the highest structural strength, its thickness is significantly greater than that of Example 5. Although the structural strength of the lightweight structure enhanced microcrystalline board obtained in Example 2 is relatively low, its weight is very low, and its longitudinal flexural strength and transverse flexural strength are comparable to those of the examples, and are more excellent in application in building materials.

[0049] The present invention uses specific embodiments to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.

Claims

1. A sintering process for a microcrystalline plate, characterized in that: It includes glass particle preparation, ball milling classification, material distribution, sintering crystallization and cold processing steps; The material distribution comprises the following steps: the glass particles are spread over the first groove and the second groove of the refractory mold, the second groove is opened at the bottom of the first groove, the depth of the first groove is 5mm-20mm, the depth of the second groove is 3mm-40mm, the particle size of the glass particles in the first groove is different from the particle size of the glass particles in the second groove, and the particle diameter of the particles in the first groove is generally larger than the diameter of the particles in the second groove; The sintering crystallization includes the following steps: transferring the refractory mold covered with glass particles during the laying process to a sintering kiln, heating to 1000-1200°C at 8-12°C / min and keeping warm for 1-3 hours to complete sintering crystallization, forming a microcrystalline plate body in the first groove during the crystallization process, forming a reinforcing structure connected to the microcrystalline plate body in the second groove, cooling to 580-670°C at 4-8°C / min and keeping warm for 0.5-1 hour to remove internal residual stress, completing annealing, cooling at 6-10°C / min, and then cooling to room temperature and taking out of the kiln to obtain a lightweight microcrystalline glass slab.

2. The sintering process of the microcrystalline plate according to claim 1, characterized in that: The refractory mold comprises a detachable first template and a second template, the first groove is opened on the upper surface of the first template and the first groove horizontally passes through the first template, and the second groove is opened on the upper surface of the second template.

3. The sintering process of the microcrystalline plate according to claim 1, characterized in that: The preparation of the glass particles comprises the following steps: mixing the raw materials and sending them into a glass melting furnace, melting them at a temperature of 1400-1650° C. and removing the internal gas to obtain a uniform glass solution, and then clarifying the uniform molten glass liquid and discharging it into water to obtain water-quenched glass particles.

4. The sintering process of the microcrystalline plate according to claim 3, characterized in that: The glass solution includes 40% to 70% SiO2, 8% to 20% CaO, 4% to 12% MgO, 5% to 20% Al2O3 and 2% to 8% Na2O by weight.

5. The sintering process of the microcrystalline plate according to claim 1, characterized in that: The material distribution includes the following steps: the second groove part in the refractory mold is evenly covered with glass particles larger than 16 meshes, and the first groove part is evenly covered with glass particles of 5-60 meshes, and the second grooves are distributed at the bottom of the first groove in parallel strips, I-shaped, well-shaped, cylindrical or square shapes.

6. The sintering process of the microcrystalline plate according to claim 1, characterized in that: The refractory mold is made of a refractory material that is resistant to high temperatures and has a small thermal expansion coefficient.

7. The sintering process of the microcrystalline plate according to claim 6, characterized in that: The refractory material is a spinel refractory board, a SiC refractory board, a mullite refractory board and a corundum refractory board.

8. The sintering process of the microcrystalline plate according to claim 1, characterized in that: The method comprises the steps of placing water-quenched glass particles into a ball mill for ball milling, and screening the ball-milled glass materials.