An organic long afterglow material and its preparation method and application
By doping aromatic organic compounds containing heteroatoms in the polymer matrix and melamine formaldehyde resin, the problems of low afterglow efficiency, short life and poor stability of polymer-based organic long afterglow materials are solved, and long life and quantum are achieved The organic long afterglow material with high yield and stable performance is suitable for the fields of anti-counterfeiting, data encryption and functional ink.
Patent Information
- Application Number
- CN202211293427.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-21
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-10-21
AI Technical Summary
The existing polymer-based organic long afterglow materials have problems with low afterglow efficiency, short lifetime and poor stability, due to the low intercoordinate crossover efficiency and low triplet excited state stability of the organic molecules used, as well as the selected polymerization. The material matrix has insufficient protective effect on guest molecules, resulting in unstable performance of the material in air and solvent atmosphere.
Using melamine formaldehyde resin as the main component, doping aromatic organic compounds containing heteroatoms as the guest component, improving inter-system crossing efficiency through n-π* transition and spin-orbit coupling, and forming through nitrogen and oxygen atoms Hydrogen bonding acts to isolate oxygen and water vapor and limit molecular movement, thereby improving the stability of triplet excitons and non-radiative transition rate.
It has achieved the long life, high quantum yield and good performance stability of organic long afterglow materials, and can effectively inhibit the penetration of solvent molecules at room temperature, and even soak in water, dilute hydrochloric acid, alkali and organic solvents for more than 7 days. It can still emit significantly, significantly improving the practicality of the material.
Smart Images

Figure SMS_2 
Figure SMS_3 
Figure SMS_5
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of materials, and in particular relates to an organic long afterglow material and a preparation method and application thereof. Background Art
[0002] Long afterglow materials can continue to emit light after the excitation source stops, which can effectively eliminate the influence of short-lived background light and greatly improve the signal-to-noise ratio of the luminescent signal. Therefore, this type of material has broad application prospects in the fields of anti-counterfeiting, emergency instructions, intelligent transportation, biological imaging, data encryption, etc., and has received widespread attention from the industry and scholars and has become a research hotspot. Traditional long afterglow materials are mainly inorganic components, which not only contain heavy metal elements such as rare earth metals or transition metals, but also have high preparation temperature and production costs, which greatly restricts their development and application. In contrast, organic materials have many advantages such as simple synthesis and modification, low production cost, flexibility and environmental friendliness. Therefore, in recent years, research on organic long afterglow materials has aroused widespread interest among scientific researchers.
[0003] At present, the strategies for achieving organic long afterglow luminescence at room temperature mainly include: 1. Providing a rigid environment for organic molecules through crystal engineering and forming special molecular aggregates; 2. Polymerizing organic molecules into polymers; 3. Using host-guest doping to incorporate organic molecules into a solid matrix that can isolate oxygen and restrict molecular motion, etc. Among them, the method of doping organic molecules (guests) into a polymer matrix (host) is simpler and faster, and the long afterglow luminescence properties of the material can be regulated by changing the chemical structure and doping concentration of organic molecules and the molecular weight of the polymer matrix. At the same time, the organic long afterglow material prepared by this method also has the advantages of good processing performance, flexibility, and easy large-scale production. However, this type of material generally has the problems of low afterglow efficiency and short life. This is related to the low intersystem crossing efficiency of the organic molecules used, the low stability of the triplet excited state, and the insufficient protection and restriction of the selected polymer matrix on the guest molecules. In addition, since most of the matrixes used are linear polymers with polar side groups, such as polylactic acid (PLA), polyvinyl alcohol (PVA), polymethyl methacrylate (PMMA), etc., the long afterglow performance of the material is greatly affected by water vapor and oxygen in the air, and the stability is poor. The above problems seriously restrict the practical application of polymer-based organic long afterglow materials. It can be seen that the design and preparation of polymer-based luminescent materials with high afterglow efficiency, long life and good stability at room temperature has important theoretical and practical significance for the development and application of organic long afterglow materials. Summary of the invention
[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the first aspect of the present invention provides an organic long afterglow material, which has the characteristics of long afterglow luminescence life, high efficiency and adjustable color.
[0005] The second aspect of the present invention provides a method for preparing the organic long afterglow material.
[0006] The third aspect of the present invention provides an organic long afterglow film comprising the organic long afterglow material.
[0007] The fourth aspect of the present invention provides a method for preparing the organic long afterglow film.
[0008] The fifth aspect of the present invention proposes an application of the organic long afterglow material or the organic long afterglow film.
[0009] According to a first aspect of the present invention, an organic long afterglow material is provided, comprising a host component and a guest component doped in the host component, wherein the host component comprises melamine formaldehyde resin, and the guest component comprises an aromatic organic compound containing heteroatoms.
[0010] In the present invention, the aromatic organic compound containing heteroatoms can undergo n-π* transition, has strong spin-orbit coupling, and has high intersystem crossing efficiency; at the same time, the melamine formaldehyde resin has a covalently cross-linked three-dimensional network structure and contains abundant nitrogen atoms and oxygen atoms, which can form strong hydrogen bonds with guest molecules, thereby effectively isolating oxygen and water vapor and restricting molecular motion, greatly improving the stability of triplet excitons of guest molecules and reducing their non-radiative transition rate. The synergistic effect of the host and the guest enables the prepared polymer-based luminescent material to produce organic long afterglow with long life, high quantum yield, and good performance stability.
[0011] In some embodiments of the present invention, in the aromatic organic compound containing a heteroatom, the heteroatom is selected from at least one of B, N, O, P or S.
[0012] In some preferred embodiments of the present invention, the aromatic organic compound containing heteroatoms comprises a compound of formula I:
[0013] ;
[0014] Wherein, the dotted line represents connection or non-connection; the connection is a single bond connection or a 4- to 6-membered ring; R1 is selected from a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, a pyrene ring, a triphenylene ring or a perylene ring; R2 and R3 are independently selected from hydrogen, hydroxyl, a benzene ring, a pyridine ring, a pyrimidine ring, a triazine ring, an indole ring, a naphthalene ring, a phenanthrene ring, an anthracene ring, a fluorene ring, a silylene ring, a quinoline ring, an isoquinoline ring, a dithiophene ring, a difuran ring, a benzofuran ring, a benzothiophene ring, a dibenzofuran ring, a dibenzothiophene ring, a triphenylene ring, a carbazole ring, a phenylcarbazole ring, an azacarbazole ring, an azafluorene ring, an azasilylfluorene ring, an azadibenzofuran ring or an azadibenzothiophene ring; X is a heteroatom, and the heteroatom is selected from B, N, O, P or S.
[0015] The aromatic organic compound containing heteroatoms includes at least one of formula (1) to formula (13):
[0016]
[0017]
[0018] . According to the different chemical structures of the doped guest molecules, the afterglow color, afterglow quantum yield, afterglow lifetime and other properties of the organic long afterglow material can be regulated.
[0019] In some more preferred embodiments of the present invention, the doping includes physical doping.
[0020] In some more preferred embodiments of the present invention, the mass fraction of the guest molecule is 0.001% to 5%, and more preferably 0.1% to 1%.
[0021] According to a second aspect of the present invention, a method for preparing an organic long afterglow material is provided, comprising the following steps:
[0022] S1: adding melamine solid and formaldehyde aqueous solution to deionized water, adjusting the pH value of the solution with alkali, and heating to form a mixture solution;
[0023] S2: adding an organic solution of an aromatic organic compound containing heteroatoms to the mixed solution, heating for reaction, and then continuing to heat to evaporate the solvent to obtain the organic long afterglow material.
[0024] In some embodiments of the present invention, the mass concentration of the formaldehyde aqueous solution is 1% to 55%, preferably 30% to 40%, and more preferably 37%.
[0025] In some preferred embodiments of the present invention, the molar ratio of melamine to formaldehyde is 1:(1-5), more preferably 1:(2-3).
[0026] In some more preferred embodiments of the present invention, the base includes any one of diethylamine, triethylamine, triethanolamine, sodium hydroxide, potassium hydroxide or sodium carbonate, and triethanolamine is further preferred.
[0027] In some more preferred embodiments of the present invention, the organic solvent of the organic solution includes any one of methanol, ethanol, acetone, dimethyl sulfoxide, N,N-dimethylformamide, tetrahydrofuran or acetonitrile, and is more preferably tetrahydrofuran.
[0028] In some more preferred embodiments of the present invention, the pH value of the solution is 7.5-10, and more preferably 8-9.
[0029] In some more preferred embodiments of the present invention, in S1, the heating temperature is 80°C~120°C, and more preferably 90°C~100°C.
[0030] In some more preferred embodiments of the present invention, in S1, the heating time is 0.5h~3h; more preferably 2h~3h.
[0031] In some more preferred embodiments of the present invention, in S2, the temperature of the heating reaction is 60°C~100°C, and more preferably 80°C~90°C.
[0032] In some more preferred embodiments of the present invention, in S2, the heating reaction time is 1 h to 3 h.
[0033] In some more preferred embodiments of the present invention, in S2, the heating temperature is 100ºC~180ºC, and more preferably 120ºC~140ºC.
[0034] In some more preferred embodiments of the present invention, in S2, the heating time is 0.5h~2h.
[0035] According to a third aspect of the present invention, an organic long afterglow film is provided, comprising the organic long afterglow material.
[0036] According to a fourth aspect of the present invention, a method for preparing the organic long afterglow film is proposed, comprising the following steps: heating and pressing the organic long afterglow material to obtain the organic long afterglow film.
[0037] In some embodiments of the present invention, the heating and pressurizing time is 10 min to 15 min.
[0038] In some preferred embodiments of the present invention, the heating temperature is 100°C to 180°C, and more preferably 150°C to 170°C.
[0039] In some more preferred embodiments of the present invention, the pressurized pressure is 5MPa~30MPa, and more preferably 15MPa~19MPa.
[0040] According to a fifth aspect of the present invention, a use of the organic long afterglow material or the organic long afterglow film in data encryption and / or anti-counterfeiting and / or functional ink and / or road marking is proposed.
[0041] The beneficial effects of the present invention are:
[0042] The organic long afterglow material of the present invention has the characteristics of long afterglow luminescence life, high efficiency and adjustable color. At the same time, it can effectively inhibit the penetration of solvent molecules at room temperature, and can still produce significant long afterglow luminescence even if it is immersed in water, dilute hydrochloric acid, alkali solution and organic solvent for more than 7 days, which can solve the problem that the long afterglow luminescence performance of the current polymer-based long afterglow material is unstable in the air and in the solvent atmosphere. Therefore, the material has strong practicality in the fields of anti-counterfeiting, data encryption, functional ink, road marking and the like. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:
[0044] Figure 1 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (1) in the embodiment of the present invention is shown in FIG.
[0045] Figure 2 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (2) in the embodiment of the present invention is shown in FIG.
[0046] Figure 3 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (3) in the embodiment of the present invention is shown in FIG.
[0047] Figure 4 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (4) in the embodiment of the present invention is shown in FIG.
[0048] Figure 5 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (5) in the embodiment of the present invention is shown in FIG.
[0049] Figure 6 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (6) in the embodiment of the present invention is shown in FIG.
[0050] Figure 7 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (7) in the embodiment of the present invention is shown in FIG.
[0051] Figure 8 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (8) in the embodiment of the present invention is shown in FIG.
[0052] Fig. 9 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (9) in the embodiment of the present invention is shown in FIG.
[0053] Fig.10 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (10) in the embodiment of the present invention is shown in FIG.
[0054] Fig.11 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (11) in the embodiment of the present invention is shown in FIG.
[0055] Fig.12 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (12) in the embodiment of the present invention is shown in FIG.
[0056] Fig.13 The hydrogen nuclear magnetic resonance spectrum of the compound of formula (13) in the embodiment of the present invention is shown in FIG.
[0057] Fig.14 This is a demonstration of the application of the organic long afterglow material of Example 8 in Example 15 of the present invention in anti-counterfeiting and / or information encryption.
[0058] Fig.15 Pictures of the solid powders of the compounds of formula (1) to (13) in Examples 1 to 13 of the present invention under ultraviolet light and after the ultraviolet light is turned off.
[0059] Fig.16 This is a steady-state luminescence spectrum of the solid powder of the compound of formula (1) to (13) in Examples 1 to 13 of the present invention.
[0060] Fig.17 The luminescence decay curves of the solid powders of the compounds of formula (1) to (13) in Examples 1 to 13 of the present invention and the lifetime values obtained by fitting are shown.
[0061] Fig.18 These are the steady-state luminescence spectra and afterglow luminescence spectra of the organic long afterglow materials in Examples 1 to 13 of the present invention.
[0062] Fig.19 The afterglow luminescence attenuation curve diagram of the organic long afterglow material in Examples 1 to 13 of the present invention and the afterglow luminescence lifetime value obtained by fitting are shown.
[0063] Fig. 20 This is a diagram of the afterglow luminescence phenomenon of the organic long afterglow material in Examples 1 to 13 of the present invention.
[0064] Fig.21 These are long afterglow luminescence images of the organic long afterglow material in Example 6 of the present invention after being immersed in different solvents for 14 days.
[0065] Fig. 22 This is a diagram of the organic long afterglow luminescence of the materials prepared in Comparative Examples 1 to 3. DETAILED DESCRIPTION
[0066] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0067] Figure 1 to Figure 13 It is the hydrogen nuclear magnetic resonance spectrum of the compounds of formula (1) to formula (13) in the embodiments of the present invention.
[0068] Example 1
[0069] This embodiment prepares an organic long afterglow material, which is a melamine formaldehyde resin-based organic long afterglow material doped with a compound of formula (1). The specific process is as follows:
[0070] S1: Weigh 2 mg of the compound of formula (1) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (1) with a concentration of 1 mg / mL;
[0071] S2: Add 256 mg of melamine and 2.14 mL of 37% formaldehyde aqueous solution into 0.1 mL of deionized water, then add triethanolamine to adjust the pH value of the solution to 8-9, and heat at 95 °C for 2 hours to form a clear mixed solution.
[0072] S3: Add the organic solution of the compound of formula (1) to the mixed solution, and then heat it at 85°C for 2 hours, then increase the temperature to 130°C and continue heating for 1 hour. After the solvent is evaporated, a melamine formaldehyde resin-based organic long afterglow material doped with formula (1) is obtained.
[0073] Example 2
[0074] This embodiment prepares an organic long afterglow material, which is a melamine formaldehyde resin-based organic long afterglow material doped with a compound of formula (2). The specific process is as follows:
[0075] S1: Weigh 1 mg of the compound of formula (2) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (2) with a concentration of 0.5 mg / mL;
[0076] S2: Add 0.138 mg of melamine and 1.06 mL of 37% formaldehyde aqueous solution into 0.1 mL of deionized water, then add triethanolamine to adjust the pH value of the solution to 8-9, and heat at 95 °C for 2 hours to form a clear mixed solution.
[0077] S3: Add the organic solution of the compound of formula (2) to the mixed solution, and then heat it at 85°C for 2 hours, then increase the temperature to 130°C and continue heating for 1 hour. After the solvent is evaporated, a melamine formaldehyde resin-based organic long afterglow material doped with formula (2) is obtained.
[0078] Example 3
[0079] This embodiment prepares an organic long afterglow material, which is a melamine formaldehyde resin-based organic long afterglow material doped with a compound of formula (3). The specific process is as follows:
[0080] S1: Under argon atmosphere, 9-bromophenanthrene (1.00 g, 3.88 mmol), aniline (0.56 g, 6.01 mmol), 2-dicyclohexylphospho-2′,4′,6′-triisopropylbiphenyl (0.08 g, 0.17 mmol), sodium tert-butoxide (1.86 g, 19.97 mmol) were added to a 250 mL three-necked flask, followed by the addition of 20 mL toluene solvent. After bubbling argon for 40 minutes, Pd2(dba3) catalyst was added, the temperature was raised to 110°C and refluxed for 30 hours, and then cooled to room temperature. The toluene solvent was then removed by a rotary evaporator, and the crude product was separated by column chromatography using dichloromethane / petroleum ether (2:3, V / V) as the mobile phase and 200-300 mesh silica gel powder. The product was then recrystallized using dichloromethane as a good solvent and n-hexane as a poor solvent, and vacuum dried to obtain a white solid powder of the compound of formula (3), with a mass of 0.75 g and a yield of 71.95%.
[0081]
[0082] S2: Weigh 10 mg of the compound of formula (3) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (3) with a concentration of 5 mg / mL;
[0083] S3: Add 1440 mg of melamine and 10.5 mL of 37% formaldehyde aqueous solution into 0.5 mL of deionized water, then add triethanolamine to adjust the pH value of the solution to 8-9, and heat at 95 °C for 1 hour to form a clear mixed solution.
[0084] S4: Add the organic solution of the compound of formula (3) to the mixed solution, then heat at 85°C for 2 hours, then increase the temperature to 130°C and continue heating for 1 hour. After the solvent is evaporated, a melamine formaldehyde resin-based organic long afterglow material doped with formula (3) is obtained.
[0085] Example 4
[0086] This embodiment prepares an organic long afterglow material, which is a melamine formaldehyde resin-based organic long afterglow material doped with a compound of formula (4). The specific process is as follows:
[0087] S1: Under argon atmosphere, 50 mL of dichloromethane was added to a 250 mL three-necked flask. After bubbling argon for 40 minutes, phenylboronic acid (0.49 g, 5.26 mmol), Cu(OAc)2·H2O (80.00 mg, 0.36 mmol) and powdered 4 Å molecular sieves (3.0 g) were added to the 250 mL three-necked flask and stirred at room temperature for 5 minutes. Then, 1-aminopyrene (0.87 g, 3.53 mmol) and triethylamine (0.81 g, 8.00 mmol) were added. After reacting at room temperature for 24 hours, dichloromethane was removed by rotary evaporator, and the crude product was separated by column chromatography using dichloromethane / petroleum ether (2:1, V / V) as mobile phase and 200-300 mesh silica gel powder. The product was recrystallized using dichloromethane as good solvent and n-hexane as poor solvent, and vacuum dried to obtain a white solid powder of the compound of formula (3), with a mass of 0.54 g and a yield of 52.06%.
[0088]
[0089] S2: Weigh 1 mg of the compound of formula (4) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (4) with a concentration of 1 mg / mL;
[0090] S3: Add 150 mg of melamine and 1.04 mL of 37% formaldehyde aqueous solution into 0.1 mL of deionized water, then add triethanolamine to adjust the pH value of the solution to 8-9, and heat at 95 °C for 1 hour to form a clear mixed solution.
[0091] S4: Add the organic solution of the compound of formula (4) to the mixed solution, then heat at 85°C for 2 hours, then heat to 130°C and continue heating for 1 hour. After the solvent is evaporated, a melamine formaldehyde resin-based organic long afterglow material doped with formula (4) is obtained.
[0092] Example 5
[0093] This embodiment prepares an organic long afterglow material, which is a melamine formaldehyde resin-based organic long afterglow material doped with a compound of formula (5). The specific process is as follows:
[0094] S1: Under argon atmosphere, bromotriphenylene (0.50 g, 1.62 mmol), aniline (0.23 g, 2.46 mmol), 2-dicyclohexylphosphine-2′,4′,6′-triisopropylbiphenyl (80 mg, 0.17 mmol), sodium tert-butoxide (0.78 g, 8.12 mmol) were placed in a 250 mL three-necked flask, followed by 20 mL of toluene solvent. After bubbling argon for 40 minutes, tris(dibenzylideneacetone)dipalladium catalyst was added, and the temperature was raised to 110°C for reflux reaction for 30 hours. The toluene solvent was then removed by a rotary evaporator, and the crude product was separated by column chromatography using dichloromethane / petroleum ether (3:7, V / V) as the mobile phase and 200-300 mesh silica gel powder. The product was then recrystallized using dichloromethane as a good solvent and n-hexane as a poor solvent, and vacuum dried to obtain a white solid powder of the compound of formula (3), with a mass of 0.31 g and a yield of 59.03%.
[0095]
[0096] S2: Weigh 2 mg of the compound of formula (5) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (5) with a concentration of 4 mg / mL;
[0097] S3: Add 266 mg of melamine and 2.13 mL of 37% formaldehyde aqueous solution into 0.2 mL of deionized water, then add triethanolamine to adjust the pH value of the solution to 8-9, and heat at 95 °C for 1 hour to form a clear mixed solution.
[0098] S4: Add the organic solution of the compound of formula (5) to the mixed solution, and then heat it at 85°C for 2 hours, then increase the temperature to 130°C and continue heating for 1 hour. After the solvent is evaporated, a melamine formaldehyde resin-based organic long afterglow material doped with formula (5) is obtained.
[0099] Example 6
[0100] This embodiment prepares an organic long afterglow material, which is a melamine formaldehyde resin-based organic long afterglow material doped with a compound of formula (6). The specific process is as follows:
[0101] S1: Weigh 1 mg of the compound of formula (6) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (6) with a concentration of 1 mg / mL;
[0102] S2: Add 144 mg of melamine and 1.05 mL of 37% formaldehyde aqueous solution into 0.3 mL of deionized water, then add triethanolamine to adjust the pH value of the solution to 8-9, and heat at 95 °C for 1 hour to form a clear mixed solution.
[0103] S3: Add the organic solution of the compound of formula (6) to the mixed solution, then heat at 85°C for 2 hours, then heat to 130°C and continue heating for 1 hour. After the solvent is evaporated, a melamine formaldehyde resin-based organic long afterglow material doped with formula (6) is obtained.
[0104] Example 7
[0105] This embodiment prepares an organic long afterglow material, which is a melamine formaldehyde resin-based organic long afterglow material doped with a compound of formula (7). The specific process is as follows:
[0106] S1: Weigh 5 mg of the compound of formula (7) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (7) with a concentration of 5 mg / mL;
[0107] S2: Add 640 mg of melamine and 5.35 mL of 37% formaldehyde aqueous solution into 1 mL of deionized water, then add triethanolamine to adjust the pH value of the solution to 8-9, and heat at 95 °C for 1 hour to form a clear mixed solution.
[0108] S3: Add the organic solution of the compound of formula (7) to the mixed solution, then heat at 85°C for 2 hours, then increase the temperature to 130°C and continue heating for 1 hour. After the solvent is evaporated, a melamine formaldehyde resin-based organic long afterglow material doped with formula (7) is obtained.
[0109] Example 8
[0110] This embodiment prepares an organic long afterglow material, which is a melamine formaldehyde resin-based organic long afterglow material doped with a compound of formula (8). The specific process is as follows:
[0111] S1: Weigh 4 mg of the compound of formula (8) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (8) with a concentration of 2 mg / mL;
[0112] S2: Add 600 mg of melamine and 4.17 mL of 37% formaldehyde aqueous solution into 0.2 mL of deionized water, then add triethanolamine to adjust the pH value of the solution to 8-9, and heat at 95 °C for 1 hour to form a clear mixed solution.
[0113] S3: Add the organic solution of the compound of formula (8) to the mixed solution, then heat at 85°C for 2 hours, then increase the temperature to 130°C and continue heating for 1 hour. After the solvent is evaporated, a melamine formaldehyde resin-based organic long afterglow material doped with formula (8) is obtained.
[0114] Example 9
[0115] This embodiment prepares an organic long afterglow material, which is a melamine formaldehyde resin-based organic long afterglow material doped with a compound of formula (9). The specific process is as follows:
[0116] S1: Weigh 2 mg of the compound of formula (9) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (9) with a concentration of 1 mg / mL;
[0117] S2: Add 288 mg of melamine and 2.10 mL of 37% formaldehyde aqueous solution into 0.5 mL of deionized water, then add triethanolamine to adjust the pH value of the solution to 8-9, and heat at 95 °C for 1 hour to form a clear mixed solution.
[0118] S3: Add the organic solution of the compound of formula (9) to the mixed solution, then heat at 85°C for 2 hours, then heat to 130°C and continue heating for 1 hour. After the solvent is evaporated, a melamine formaldehyde resin-based organic long afterglow material doped with formula (9) is obtained.
[0119] Example 10
[0120] This embodiment prepares an organic long afterglow material, which is a melamine formaldehyde resin-based organic long afterglow material doped with a compound of formula (10). The specific process is as follows:
[0121] S1: Weigh 1 mg of the compound of formula (10) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (10) with a concentration of 0.5 mg / mL;
[0122] S2: Add 133 mg of melamine and 1.06 mL of 37% formaldehyde aqueous solution into 0.8 mL of deionized water, then add triethanolamine to adjust the pH value of the solution to 8-9, and heat at 95 °C for 1 hour to form a clear mixed solution.
[0123] S3: Add the organic solution of the compound of formula (10) to the mixed solution, then heat at 85°C for 2 hours, then increase the temperature to 130°C and continue heating for 1 hour. After the solvent is evaporated, a melamine formaldehyde resin-based organic long afterglow material doped with formula (10) is obtained.
[0124] Embodiment 11
[0125] This embodiment prepares an organic long afterglow material, which is a melamine formaldehyde resin-based organic long afterglow material doped with a compound of formula (11). The specific process is as follows:
[0126] S1: Weigh 1 mg of the compound of formula (11) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (11) with a concentration of 0.5 mg / mL;
[0127] S2: Add 128 mg of melamine and 1.07 mL of 37% formaldehyde aqueous solution into 0.1 mL of deionized water, then add triethanolamine to adjust the pH value of the solution to 8-9, and heat at 95 °C for 1 hour to form a clear mixed solution.
[0128] S3: Add the organic solution of the compound of formula (11) to the mixed solution, then heat at 85°C for 2 hours, then increase the temperature to 130°C and continue heating for 1 hour. After the solvent is evaporated, a melamine formaldehyde resin-based organic long afterglow material doped with formula (11) is obtained.
[0129] Example 12
[0130] This embodiment prepares an organic long afterglow material, which is a melamine formaldehyde resin-based organic long afterglow material doped with a compound of formula (12). The specific process is as follows:
[0131] S1: Weigh 3 mg of the compound of formula (12) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (12) with a concentration of 0.5 mg / mL;
[0132] S2: Add 414 mg of melamine and 3.19 mL of 37% formaldehyde aqueous solution into 1.2 mL of deionized water, then add triethanolamine to adjust the pH value of the solution to 8-9, and heat at 95 °C for 1 hour to form a clear mixed solution.
[0133] S3: Add the organic solution of the compound of formula (12) to the mixed solution, then heat at 85°C for 2 hours, then increase the temperature to 130°C and continue heating for 1 hour. After the solvent is evaporated, a melamine formaldehyde resin-based organic long afterglow material doped with formula (12) is obtained.
[0134] Example 13
[0135] This embodiment prepares an organic long afterglow material, which is a melamine formaldehyde resin-based organic long afterglow material doped with a compound of formula (13). The specific process is as follows:
[0136] S1: Weigh 1 mg of the compound of formula (13) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (13) with a concentration of 1 mg / mL;
[0137] S2: Add 138 mg of melamine and 1.05 mL of 37% formaldehyde aqueous solution into 0.5 mL of deionized water, then add triethanolamine to adjust the pH value of the solution to 8-9, and heat at 95 °C for 1 hour to form a clear mixed solution.
[0138] S3: Add the organic solution of the compound of formula (13) to the mixed solution, then heat at 85°C for 2 hours, then increase the temperature to 130°C and continue heating for 1 hour. After the solvent is evaporated, a melamine formaldehyde resin-based organic long afterglow material doped with formula (13) is obtained.
[0139] Embodiment 14
[0140] This embodiment has an organic long afterglow film, and the specific process is as follows:
[0141] The organic long afterglow material prepared in Example 1 was heated and pressurized at 150°C and 18MPa for 10 min using a hot press to prepare a translucent plastic film.
[0142] The organic long afterglow material prepared in Example 2 was heated and pressurized at 150°C and 16MPa for 10 minutes using a hot press to prepare a translucent plastic film.
[0143] The organic long afterglow material prepared in Example 3 was heated and pressurized at 150°C and 16MPa for 10 minutes using a hot press to prepare a translucent plastic film.
[0144] The organic long afterglow material prepared in Example 4 was heated and pressurized at 150°C and 16MPa for 10 min using a hot press to prepare a translucent plastic film.
[0145] The organic long afterglow material prepared in Example 5 was heated and pressurized at 150°C and 16MPa for 10 min using a hot press to prepare a translucent plastic film.
[0146] The organic long afterglow material prepared in Example 6 was heated and pressurized at 150°C and 16MPa for 10 min using a hot press to prepare a translucent plastic film.
[0147] The organic long afterglow material prepared in Example 7 was heated and pressurized at 150°C and 16MPa for 10 min using a hot press to prepare a translucent plastic film.
[0148] The organic long afterglow material prepared in Example 8 was heated and pressurized at 150°C and 16MPa for 10 min using a hot press to prepare a translucent plastic film.
[0149] The organic long afterglow material prepared in Example 9 was heated and pressurized at 150°C and 16MPa for 10 min using a hot press to prepare a translucent plastic film.
[0150] The organic long afterglow material prepared in Example 10 was heated and pressurized at 150°C and 16MPa for 10 minutes using a hot press to prepare a translucent plastic film.
[0151] The organic long afterglow material prepared in Example 11 was heated and pressurized at 150°C and 16MPa for 10 minutes using a hot press to prepare a translucent plastic film.
[0152] The organic long afterglow material prepared in Example 12 was heated and pressurized at 150°C and 16MPa for 10 minutes using a hot press to prepare a translucent plastic film.
[0153] The organic long afterglow material prepared in Example 13 was heated and pressurized at 150°C and 16MPa for 10 minutes using a hot press to prepare a translucent plastic film.
[0154] Embodiment 15
[0155] This embodiment provides the use of the melamine formaldehyde resin-based organic long afterglow material doped with the compound of formula (8) for anti-counterfeiting and information encryption. The organic long afterglow material in Example 8 is prepared into an anti-counterfeiting pattern by screen printing for anti-counterfeiting and information encryption. The specific process is as follows:
[0156] S1: Weigh 4 mg of the compound of formula (8) and dissolve it in tetrahydrofuran to prepare an organic solution of the compound of formula (8) with a concentration of 2 mg / mL;
[0157] S2: Add 600 mg of melamine and 4.17 mL of 37% formaldehyde aqueous solution into 0.2 mL of deionized water, then add triethanolamine to adjust the pH value of the solution to 8-9, and heat at 95 °C for 1 hour to form a clear mixed solution.
[0158] S3: Add the organic solution of the compound of formula (8) in S1 to the mixed solution in S2, and then use it as ink to print a two-dimensional code pattern that can identify the information "South China Normal University" on A4 white paper by screen printing. Since the obtained pattern is relatively transparent and the strong deep blue fluorescence of A4 paper is similar to the steady-state luminescence of the polymer material, the two-dimensional code presented under the irradiation of fluorescent lamps and ultraviolet lamps cannot be recognized. Only the two-dimensional code presented by the long afterglow emitted by the material after turning off the ultraviolet lamp can be recognized, thereby achieving the effect of anti-counterfeiting and information encryption. The results are shown in FIG. Fig.14 shown.
[0159] from Fig.14 It can be seen that the organic long afterglow material of the present invention can be applied to the fields of anti-counterfeiting, information encryption, functional ink, road marking, etc.
[0160] Comparative Example 1
[0161] This comparative example prepares an organic light-emitting material. The difference from Example 4 is that the compound of molecular formula (4) is doped into bisphenol A diglycidyl ether type epoxy resin. The specific process is as follows:
[0162] The compound of formula (4) (1.00 mg), bisphenol A diglycidyl ether (1.00 g) and 1,3-propylenediamine were placed in a 1.5 mL transparent sample tube. The mixture was ultrasonicated at room temperature until it became clear and transparent, injected into a mold, and cured at 90° C. for 2 hours to obtain an epoxy polymer-based organic light-emitting material doped with formula (4).
[0163] Comparative Example 2
[0164] This comparative example prepares an organic light-emitting material. The difference from Example 4 is that the compound of molecular formula (4) is doped into polyvinyl alcohol. The specific process is as follows:
[0165] 1.00 mg of the compound of formula (4) and 200 μl of dimethyl sulfoxide were placed in a 1.5 mL transparent sample tube, and then 1.00 g of a 50 mg / ml polyvinyl alcohol aqueous solution was added. The mixture was ultrasonicated at room temperature until it became clear and transparent, injected into a mold, and cured at 90°C for 4 hours to obtain a polyvinyl alcohol-based organic light-emitting material doped with formula (4).
[0166] Comparative Example 3
[0167] This comparative example prepares an organic light-emitting material. The difference from Example 4 is that the compound of molecular formula (4) is doped into polymethyl methacrylate. The specific process is as follows:
[0168] The compound of formula (4) (1.00 mg) and 200 μl of dimethyl sulfoxide were placed in a 1.5 mL transparent sample tube, and then 1 ml of a 100 mg / ml tetrahydrofuran solution of polymethyl methacrylate was added. The mixture was ultrasonicated at room temperature until it became clear and transparent, injected into a mold, and cured at 100°C for 5 hours to obtain a polymethyl methacrylate organic light-emitting material doped with formula (4).
[0169] Test example
[0170] This test example tests the optical properties of the solid powder (microcrystal) of the compound of formula (1) to formula (13) in Examples 1 to 13, the organic long afterglow material in Examples 1 to 13, and the organic light-emitting material in Comparative Examples 1 to 3. The main properties of the target material such as afterglow luminescence spectrum, afterglow quantum yield, afterglow lifetime, and the stability of afterglow performance are investigated. All tests were performed on an Edinburgh FLS980 steady-state transient fluorescence spectrometer with an integrating sphere. The results are shown in the figure. Figure 15~Figure 22 , as shown in Table 1.
[0171] Fig.15 The following are pictures of the solid powders of the compounds of formula (1) to (13) in Examples 1 to 13 under ultraviolet light and after the ultraviolet light is turned off.
[0172] Fig.16 The steady-state luminescence spectra of the solid powders of the compounds of formula (1) to (13) in Examples 1 to 13 are shown.
[0173] Fig.17 The luminescence decay curves of the solid powders of the compounds of formula (1) to (13) in Examples 1 to 13 and the lifetime values obtained by fitting are shown.
[0174] Fig.18 These are the steady-state luminescence spectra and afterglow luminescence spectra of the organic long afterglow materials in Examples 1 to 13.
[0175] Fig.19 The afterglow luminescence attenuation curve diagram of the organic long afterglow material in Example 1 to Example 13 and the afterglow luminescence lifetime value obtained by fitting.
[0176] Fig. 20 This is a diagram of the afterglow luminescence phenomenon of the organic long afterglow material in Examples 1 to 13.
[0177] Fig.21 This is a long afterglow luminescence image of the organic long afterglow material in Example 6 after being immersed in common solvents or solutions such as toluene, dichloromethane, tetrahydrofuran, N,N-dimethylformamide, acetonitrile, ethyl acetate, n-hexane, water, hydrochloric acid solution, acetic acid solution, sodium hydroxide solution, etc. for 14 days.
[0178] Fig. 22 This is a diagram of the organic long afterglow luminescence of the materials prepared in Comparative Examples 1 to 3.
[0179] Table 1 Test results of photophysical properties of organic long afterglow materials in Examples 1 to 13
[0180]
[0181] from Figure 15~Figure 17It can be seen that at room temperature, pure compounds of formula (1) to (13) did not produce long afterglow after being excited by ultraviolet light. Pure guest materials only emit instantaneous fluorescence in the solid state and have no afterglow properties. They need to be doped into the host material to produce long afterglow.
[0182] From Table 1, Figure 18~Figure 20 It can be seen that the organic long afterglow materials of the present invention all have long afterglow luminescence characteristics, and their afterglow lifetime can reach up to 3.148 s at room temperature in air, and the highest efficiency can reach 16.95%. At the same time, the wavelength, lifetime and efficiency of their long afterglow luminescence can be adjusted by changing the doped guest molecules.
[0183] from Fig.21 It can be seen that the organic long afterglow material of the present invention can be placed in air at room temperature for 14 days, or in toluene, dichloromethane, tetrahydrofuran, N , N -After being immersed in common organic solvents such as dimethylformamide for 14 days, it can still maintain excellent long afterglow luminescence performance.
[0184] contrast Fig. 20 and Fig. 22 It can be seen that the compound of formula (4) cannot produce long organic afterglow when doped in other polymers as a guest molecule, but can produce excellent long afterglow luminescence properties when doped in melamine formaldehyde resin, indicating that the organic long afterglow property of the organic long afterglow material of the present invention is produced after the aromatic organic compound containing heteroatoms and melamine formaldehyde resin are combined with each other.
[0185] In summary, in the embodiments of the present invention, the prepared polymer luminescent material can emit afterglow with long lifetime, high quantum yield and good stability in air at room temperature by physical doping with the aromatic organic compound containing heteroatoms (1) to (13) as the guest and melamine formaldehyde resin as the host. By changing the doped aromatic organic compound containing heteroatoms, the wavelength, lifetime and quantum yield of the long afterglow luminescence of the melamine formaldehyde resin-based long afterglow material can be regulated. By utilizing the unique long afterglow luminescence properties of the prepared material, functions such as anti-counterfeiting and information encryption can also be realized. It can be seen that the prepared melamine formaldehyde resin-based material doped with the aromatic organic compound containing heteroatoms has the advantages of long afterglow luminescence lifetime, high quantum yield, good performance stability, and the wavelength can be adjusted by the guest molecular structure, and can be used in the fields of anti-counterfeiting, information encryption, functional inks and road signs.
[0186] The above is a detailed description of the embodiments of the present invention, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. An organic long afterglow material, characterized in that: It comprises a main component and a guest component doped in the main component, wherein the main component comprises melamine formaldehyde resin, and the guest component comprises an aromatic organic compound containing heteroatoms; the mass fraction of the guest molecule is 0.1% to 1%; The aromatic organic compound containing heteroatoms includes compounds of formula I: ; Wherein, the dotted line represents connection or non-connection; the connection is a single bond connection; R1 is selected from a benzene ring, a naphthalene ring, a phenanthrene ring, a pyrene ring, and a triphenylene ring; R2 and R3 are independently selected from hydrogen, hydroxyl, a benzene ring, a naphthalene ring, a benzofuran ring, a benzothiophene ring, a dibenzofuran ring, a dibenzothiophene ring, a triphenylene ring, a carbazole ring, a phenylcarbazole ring, and an azacarbazole ring; X is a heteroatom, and the heteroatom is selected from B or N.
2. The organic long afterglow material according to claim 1, characterized in that: The aromatic organic compound containing heteroatoms includes at least one of formula (1) to formula (13): 。 3. The organic long afterglow material according to claim 1, characterized in that: The doping includes physical doping.
4. A method for preparing the organic long afterglow material according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1: adding melamine solid and formaldehyde aqueous solution to deionized water, adjusting the pH value of the solution with alkali, and heating to form a mixture solution; S2: adding the organic solution of the aromatic organic compound containing heteroatoms as claimed in any one of claims 1 to 3 to the mixed solution, heating for reaction, and then continuing to heat to evaporate the solvent to obtain the organic long afterglow material.
5. The method for preparing the organic long afterglow material according to claim 4, characterized in that: The molar ratio of melamine to formaldehyde is 1:(1-5).
6. An organic long afterglow film, comprising the organic long afterglow material according to any one of claims 1 to 3.
7. A method for preparing an organic long afterglow film as claimed in claim 6, comprising the following steps: The organic long afterglow material is heated and pressed to obtain an organic long afterglow film.
8. Use of the organic long afterglow material according to any one of claims 1 to 3 or the organic long afterglow film according to claim 6 in data encryption and / or anti-counterfeiting and / or functional ink and / or road marking.
Citation Information
Patent Citations
Environmental protection type organic coumarin-base photoluminescence anti-counterfeiting pigment, environmental protection type organic coumarin-base photoluminescence anti-counterfeiting ink,and preparation methods thereof
CN103666457A
Platelike effect pigments with a melamine formaldehyde resin coating
US20050204958A1
Thermally activated delayed fluorescence organic light emitting diode having host matrix polarity co-doping
US20180277766A1