A thin gauge hot rolled steel and a preparation method thereof
Through chemical composition design and multi-mode rolling process, thin-gauge hot-rolled steel with high strength and low fluctuation is prepared, which solves the problems of poor pattern quality and large strength fluctuation in the existing technology, and achieves high strength and dimensional accuracy. combine.
Patent Information
- Application Number
- CN202211187560.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-28
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-09-28
AI Technical Summary
The pattern quality of thin-gauge hot-rolled steel in the existing technology is poor and the strength fluctuates greatly, making it difficult to meet the requirements for high strength and dimensional accuracy.
Through chemical composition design, the C-Si-Mn-Nb-Ti-Cr-B composition system is used, adding an appropriate amount of B element to improve hardenability, and relying on the solid solution strengthening of C, Mn, and Cr and the fine grain strengthening of Nb , controlling the metallographic structure to martensite, combined with multi-mode rolling process Process, including KR desulfurization, converter smelting, LF refining, VD refining, continuous casting, preheating, rough phosphorus removal, rough rolling, induction heating, fine phosphorus removal, finish rolling, laminar cooling and coiling, to prepare the yield strength> Thin gauge hot-rolled steel with a tensile strength of 900MPa and >1000MPa.
It achieves high strength, good shape, dimensional accuracy and low strength fluctuation of thin-gauge hot-rolled steel, with a thickness of up to 0.8-4.0mm, effectively solving the problems of poor pattern quality and large strength fluctuations.
Smart Images

Figure CN115747632B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel preparation, and in particular relates to a thin-gauge hot-rolled steel and a preparation method thereof. Background Art
[0002] In recent years, driven by factors such as "replacing cold with heat", reducing costs, energy conservation and emission reduction, shortening processes, and improving efficiency, headless rolling technology has gradually increased the production proportion of ultra-thin strip products. With the growing market demand for high-performance thin / ultra-thin hot-rolled strip steel, several thin slab continuous casting and rolling (ESP) production lines have been put into production in China, which can stably, reliably and accurately produce ordinary low-carbon ultra-thin plates and high-strength ultra-thin hot-rolled plate products. The difference between the multi-mode thin slab continuous casting and rolling production line and the conventional ESP production line is that the slab thickness is increased by 20-30mm compared with the ESP production line, and a roller-bottom tunnel furnace is added between the continuous casting machine outlet and the rough rolling. The tunnel furnace includes a fixed section and a moving section, and has the function of slab offline, which can realize single-slab, semi-headless and full-headless multi-mode rolling, and expand the product thickness range.
[0003] High-strength steel has become a new generation of environmentally friendly materials because it can achieve the goals of weight reduction, energy conservation and emission reduction while meeting safety and usage requirements. It is widely used in engineering machinery, automobile manufacturing, container manufacturing and other fields. The demand is increasing and the market prospects are good. 1000MPa-level high-strength steel has been widely used in automobile beams, frames and carriages, crane booms in the engineering machinery industry and container panels, replacing low-strength products and achieving reduced production. However, at present, the traditional hot rolling line produces thin-gauge 1000MPa high-strength steel with problems such as poor plate shape, large strength fluctuations, and poor dimensional accuracy control. Summary of the invention
[0004] The purpose of the present application is to provide a thin-gauge hot-rolled steel and a preparation method thereof, so as to solve the technical problems in the prior art that the thin-gauge hot-rolled steel has poor shape quality and large strength fluctuations.
[0005] An embodiment of the present invention provides a thin gauge hot-rolled steel, the chemical composition of the steel comprising, by mass percentage:
[0006] C: 0.15-0.25%, Si: ≤0.05%, Mn: 2.0-3.0%, Al: 0.02-0.35%, P: ≤0.010%, S: ≤
[0007] 0.005%, Nb: 0.01-0.10%, Ti: 0.010-0.030%, Cr: 0.1-0.5%, N: ≤0.004%, B: 0.0010-0.0025%, the balance is Fe and unavoidable impurities.
[0008] Optionally, the metallographic structure of the thin gauge hot rolled steel is martensite.
[0009] Based on the same inventive concept, an embodiment of the present invention further provides a method for preparing the thin-gauge hot-rolled steel as described above, comprising the following steps:
[0010] After KR desulfurization, converter smelting, LF refining and VD refining, molten steel meeting the chemical composition is obtained;
[0011] The molten steel is continuously cast to obtain a slab;
[0012] The slab is subjected to preheating, rough dephosphorization, rough rolling, induction heating, fine dephosphorization, fine rolling, laminar cooling, coiling and air cooling to obtain the thin gauge hot rolled steel;
[0013] in:
[0014] The finishing rolling is any one of single billet rolling, semi-endless rolling and full endless rolling;
[0015] The fine descaling is single removal of phosphorus or double removal of phosphorus;
[0016] When the finishing rolling is single-bill mode rolling, the finishing descaling is double dephosphorization;
[0017] When the finishing rolling is semi-endless mode rolling or full-endless mode rolling, the finishing dephosphorization is single dephosphorization.
[0018] Optionally, the end point temperature of the preheating is 1150-1200°C.
[0019] Optionally, the continuous casting pulling speed is 4.0-6.5 m / min, and the continuous casting slab thickness is 110-123 mm.
[0020] Optionally, the pressure of the rough phosphorus removal is ≥30 MPa, the pressure of the fine phosphorus removal is ≥30 MPa, and the distance between the nozzle of the fine phosphorus removal and the slab is 60-110 mm.
[0021] Optionally, the inlet temperature of the rough rolling is ≥1150°C, the outlet temperature of the rough rolling is 930-1000°C, and the number of passes of the rough rolling is 3.
[0022] Optionally, the end point temperature of the induction heating is 1050-1150°C.
[0023] Optionally, the cumulative deformation of the finishing rolling is 70-80%, the final rolling temperature of the finishing rolling is 820-880° C., and the number of finishing rolling passes is 5.
[0024] Optionally, the cooling rate of the laminar cooling is ≥30°C, and the coiling temperature is 250-400°C.
[0025] One or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0026] The thin-gauge hot-rolled steel provided in the embodiment of the present invention adopts a C-Si-Mn-Nb-Ti-Cr-B component system through chemical composition design, and improves the hardenability of the material by adding an appropriate amount of B element to obtain a martensitic structure. The strength of the material is ensured by solid solution strengthening of C, Mn, and Cr, and fine grain strengthening and organizational strengthening of Nb. The yield strength of the obtained thin-gauge hot-rolled steel is greater than 900MPa, the tensile strength is greater than 1000MPa, the elongation is greater than 8%, the transverse cold bending D=2a, 180° is qualified, and the thickness can reach 0.8-4.0mm, which can effectively solve the technical problems of poor quality of thin-gauge hot-rolled steel and large strength fluctuation in the prior art.
[0027] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0029] Figure 1 is a flow chart of a method provided by an embodiment of the present invention;
[0030] Figure 2 It is a metallographic structure diagram of thin-gauge hot-rolled steel provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0031] The present invention will be described in detail below in conjunction with specific implementations and examples, and the advantages and various effects of the present invention will be more clearly presented. It should be understood by those skilled in the art that these specific implementations and examples are used to illustrate the present invention, rather than to limit the present invention.
[0032] Throughout the specification, unless otherwise specifically stated, the terms used herein should be understood as meanings commonly used in the art. Therefore, unless otherwise defined, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. If there is a conflict, the present specification takes precedence. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. For example, room temperature can refer to a temperature within the range of 10 to 35°C.
[0033] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0034] The technical solution of the embodiment of the present application is to solve the above technical problems, and the overall idea is as follows:
[0035] According to a typical embodiment of the present invention, a thin gauge hot-rolled steel is provided, wherein the chemical composition of the steel comprises, by mass percentage:
[0036] C: 0.15-0.25%, Si: ≤0.05%, Mn: 2.0-3.0%, Al: 0.02-0.35%, P: ≤0.010%, S: ≤0.005%, Nb: 0.01-0.10%, Ti: 0.010-0.030%, Cr: 0.1-0.5%, N: ≤0.004%, B: 0.0010-0.0025%, the balance is Fe and unavoidable impurities.
[0037] The thin-gauge hot-rolled steel provided in the embodiment of the present invention adopts a C-Si-Mn-Nb-Ti-Cr-B component system through chemical composition design, and improves the hardenability of the material by adding an appropriate amount of B element to obtain a martensitic structure. The strength of the material is ensured by solid solution strengthening of C, Mn, and Cr, and fine grain strengthening and organizational strengthening of Nb. The yield strength of the obtained thin-gauge hot-rolled steel is greater than 900MPa, the tensile strength is greater than 1000MPa, the elongation is greater than 8%, the transverse cold bending D=2a, 180° is qualified, and the thickness can reach 0.8-4.0mm, which can effectively solve the technical problems of poor quality of thin-gauge hot-rolled steel and large strength fluctuation in the prior art.
[0038] The functions and limited ranges of the above main alloying elements are described in detail as follows:
[0039] C: C is the most important alloying element in steel and one of the most economical elements to improve strength. C atoms are limitedly dissolved in γ-Fe and expand the γ phase area, which has a great influence on the organization and performance, and plays a major role in controlling strength and hardness. It also forms carbonitrides with microalloying elements, which regulates the performance of steel in a wide range. When C>0.25%, banded structure is easily formed during slab smelting and rolling. Severe banded structure has an adverse effect on the cold forming performance and fatigue performance of the steel plate, and when C>0.25%, it is not conducive to welding performance; when C<0.15%, it will increase the difficulty of smelting. Therefore, the C content is controlled to be 0.15-0.25%.
[0040] Si: The Si element mainly affects the surface quality of hot-rolled strip, pickled steel plate and hot-dip galvanized strip. According to the Sanderin effect, when the Si content is controlled below 0.05%, the coating structure is basically unaffected by silicon, and a bright coating of normal thickness can be obtained. Therefore, the Si content is controlled to be ≤0.05%.
[0041] Mn: Mn and Fe can replace each other, and it is a substitutional solute atom in the iron-based solid solution, with good solid solution strengthening performance; manganese can also refine the grains and improve the strength. It is an austenite stabilizing element and expands the single austenite phase area; manganese can significantly reduce the temperature of γ→α transformation, so it can reduce the A1 point; in order to reduce the energy consumption of induction heating, the final temperature of the finishing rolling of thin slab continuous casting and rolling is generally controlled at 800-860℃. If the Mn content is low, the strip is easy to enter the two-phase region during the final rolling in this temperature range, and part of the austenite is transformed into ferrite structure, which reduces the strength of the strip. Therefore, in order to obtain a full martensitic structure, the Mn content is added to be more than 2.0%, ensuring that the strip is still in the complete austenite region during the final rolling at 800-860℃ to avoid the formation of ferrite structure; when the Mn content is greater than 3.0%, the production cost of the test steel will increase, so the Mn content is controlled to be 2.0-3.0%.
[0042] Al: Al is one of the effective deoxidizing elements and can form nitrides to refine grains. Al content > 0.35% will damage the toughness of the steel and the toughness of the heat affected zone of the weld will also deteriorate.
[0043] P, S and N: Too high P, S and N elements will have an adverse effect on the plasticity, toughness and fatigue properties of the material. If the N content is too high, it is easy to combine with the B element to form BN precipitates at high temperature, which consumes part of the B element and thus reduces the hardenability of the strip. It is impossible to obtain the entire martensitic structure, reducing the strength of the strip. Therefore, the P content is controlled to be ≤0.010%, the S content is ≤0.005%, and the N content is ≤0.004%.
[0044] Nb: Nb is one of the key strengthening elements in HSLA steel. It has multiple strengthening mechanisms such as solid solution strengthening and precipitation in the thermomechanical process. Solid solution Nb can significantly increase the dynamic recrystallization temperature of steel, thereby promoting the formation of deformation-induced precipitation through rolling in the non-recrystallized zone; Nb dispersed precipitates can strengthen the matrix by dragging dislocations and refine grains by pinning grain boundaries, thereby improving steel strength and toughness and plasticity; in addition, Nb can also ensure the refinement of weld structure and improve post-weld strength. Considering the cost factor, excessive Nb content will increase the production cost of the material, so the Nb content is controlled to 0.01-0.10%.
[0045] Ti: Ti is a strong carbonitride-forming element. In the high temperature stage, Ti first combines with N to form TiN precipitation phase, which can consume N element, reduce the content of solid solution N, and improve the cleanliness of molten steel. On the other hand, since the formation stage of TiN precipitation phase is earlier than BN, the combination of B and N is avoided, and the consumption of N on solid solution B element is reduced, which ensures the hardenability of the strip. After the molten steel solidifies, fine TiN particles are precipitated. These fine TiN particles are very stable and can effectively prevent the growth of austenite grains, thereby refining the structure. In the welding process, Ti-containing second phase particles can prevent the growth of coarse grains in the welding process, refine the grains, and improve the welding performance of steel. At a higher Ti content, Ti combines with C to form TiC or Ti(C,N), which consumes part of the C element. A lower solid solution C content will reduce the strength of the strip. Therefore, the Ti content is controlled to be 0.010-0.030%.
[0046] Cr: Cr is a strong hardenability element, which plays a role of solid solution strengthening in the matrix. In order to obtain finer ferrite grains, an appropriate amount of Cr is added to improve the hardenability of the material and refine the grains. However, too much Cr will cause the welding performance of the material to deteriorate, so the Cr content is controlled to 0.1%-0.5%.
[0047] B: B is a strong hardenability element. The content of B in steel is very small (less than 50ppm). Its main function is to increase the hardenability of steel. Its effect is much greater than that of Cr, Mn and other alloying elements. The use of trace amounts of B can save a lot of alloying elements. However, B is extremely active in chemical properties and has a strong affinity with N and O. It can also form B with C. 4 C: Only B in the solid solution state has a beneficial effect on the hardenability of steel, while B in the form of a compound has no effect on the hardenability of steel. Therefore, the B content is controlled to be 0.0010-0.0025%.
[0048] As an optional implementation, the metallographic structure of the thin gauge hot rolled steel is martensite.
[0049] The reason for controlling the metallographic structure to be martensite is that the present invention is a 1000MPa tensile high-strength steel. In order to meet the mechanical properties, the material strength strengthening mechanism is organization strengthening. Martensite is a low-temperature phase transformation structure with excellent strength, so the structure is controlled to be martensite.
[0050] According to another typical embodiment of the present invention, there is provided a method for manufacturing the thin gauge hot rolled steel as provided above, comprising the following steps:
[0051] S1. After KR desulfurization, converter smelting, LF refining and VD refining, molten steel with the chemical composition is obtained.
[0052] S2. Continuously casting the molten steel to obtain a slab.
[0053] S3, subjecting the slab to preheating, rough dephosphorization, rough rolling, induction heating, fine dephosphorization, fine rolling, laminar cooling, coiling and air cooling to obtain the thin-gauge hot-rolled steel.
[0054] in:
[0055] The finishing rolling is any one of single billet mode rolling, semi-headless mode rolling and full headless mode rolling;
[0056] The fine descaling is single removal of phosphorus or double removal of phosphorus;
[0057] When the finishing rolling is single-bill mode rolling, the finishing descaling is double dephosphorization;
[0058] When the finishing rolling is semi-endless mode rolling or full endless mode rolling, the finishing rolling is single row phosphorus removal.
[0059] In the above steps: dephosphorization is performed twice before rough rolling and finish rolling to ensure the surface quality of the steel strip; the intermediate billet is induction heated before finish rolling to dissolve the carbonitrides of Nb and Ti formed during rough rolling; Nb is precipitated again in the finish rolling stage to refine the austenite grains and further refine the martensite grain size; an appropriate amount of B element is added to increase the hardenability of the steel strip so that the steel strip obtains a martensitic structure; laminar cooling is adopted after rolling, and the cooling rate and coiling temperature are adjusted according to different strip thicknesses to obtain a 1000MPa hot-rolled steel strip with uniform performance, good steel plate shape, high dimensional accuracy and small strength fluctuation.
[0060] It should be noted that single-bill rolling, semi-headless rolling and full headless rolling refer to: The three rolling modes are a definition of whether the billet is cut or not during the rolling process. Single-bill rolling means that the billet needs to be cut and one steel coil is produced after rolling. Semi-headless rolling means that the billet also needs to be cut, but the billet is longer, and generally one billet can produce several steel coils. Full headless rolling means that the billet does not need to be cut or not during the entire rolling process, but the strip is divided into coils after coiling.
[0061] Single-row descaling or double-row descaling refers to: the number of rows of descaling headers. The headers arranged in one row are called single-row descaling, and the headers arranged in two rows are called double-row descaling.
[0062] The reason for selecting the finishing descaling method by finishing rolling is that: the descaling method before finishing rolling is selected according to the rolling mode. When single billet is rolled, due to the fast rolling rate and the low finishing rolling entrance temperature during single billet mode rolling, the iron oxide scale has high viscosity and is not easy to remove, so double descaling is selected; for semi-headless and headless rolling, the rolling rate is slow, and the slab needs to be induction heated before finishing rolling to increase the temperature of the slab. After the temperature increases, the viscosity of the iron oxide scale decreases and it is easy to remove, so single descaling is selected.
[0063] As an optional implementation manner, the end temperature of the preheating is 1150-1200°C.
[0064] The reason for controlling the end temperature of preheating is that this temperature range can ensure the temperature of the slab entering the rolling mill, making the slab transition uniform; when the temperature is greater than 1200°C, it will cause energy waste, and when the temperature is less than 1150°C, it will cause rolling instability.
[0065] As an optional implementation manner, the continuous casting speed is 4.0-6.5 m / min, and the continuous casting slab thickness is 110-123 mm.
[0066] The reason for controlling the continuous casting pulling speed is that controlling the continuous casting pulling speed to 4.0-6.5m / min can ensure that the continuous casting matches the headless rolling production mode; when the pulling speed is greater than 6.5m / min, the adverse effect will be that 6.5m / min is the equipment operation limit, and too high a pulling speed will require equipment replacement, increasing costs. When the pulling speed is less than the minimum value of the endpoint of the range, the adverse effect will be that the pulling speed is too small, and the continuous casting and rolling production cannot be matched.
[0067] The reason for controlling the thickness of the continuous casting slab is that the slab thickness can be selected according to the thickness of the finished strip steel product. When the finished product thickness is ≤4.0mm, the ingot thickness can be selected as 110-115. When the finished strip steel product thickness is 5-12.0mm, the finished product thickness can be selected as 115-123mm. Increasing the ingot thickness mainly increases the total rolling reduction, which can refine the grains and thus improve the strength of the material.
[0068] As an optional implementation manner, the pressure of the rough phosphorus removal is ≥30 MPa, the pressure of the fine phosphorus removal is ≥30 MPa, and the distance between the nozzle of the fine phosphorus removal and the slab is 60-110 mm.
[0069] The reason for controlling the rough dephosphorization pressure is that within this pressure range, the iron oxide scale on the strip surface can be fully removed; when the descaling pressure is less than the minimum value of the endpoint of this range, the adverse effect will be that iron oxide scale will remain on the strip surface, which will affect the surface quality of the strip.
[0070] The reason for controlling the fine dephosphorization pressure is that within this pressure range, the iron oxide scale on the strip surface can be fully removed; when the descaling pressure is less than the minimum value of the endpoint of this range, the adverse effect will be the residual iron oxide scale on the strip surface, affecting the surface quality of the strip.
[0071] The reason for controlling the distance between the nozzle and the slab is that controlling the distance between the descaling nozzle for fine descaling and the continuous casting slab to be 60-110mm can ensure the descaling effect of the strip; when the distance value is greater than the maximum value of the endpoint of the range, the adverse effect will be that the distance is too large, resulting in poor effect of the descaling nozzle and the existence of an over-descaled area; when the distance value is less than the minimum value of the endpoint of the range, the adverse effect will be that the distance is too short, the descaling nozzle is poor, and there is an undescaled area.
[0072] As an optional implementation manner, the inlet temperature of the rough rolling is ≥1150°C, the outlet temperature of the rough rolling is 930-1000°C, and the number of passes of the rough rolling is 3.
[0073] The reason for controlling the above parameters is that: within this temperature range, the temperature of the slab entering the rolling mill can be guaranteed; when the temperature value is greater than the maximum value of the endpoint of the range, the adverse effect will be that the temperature is too high, which will cause energy waste; when the temperature value is less than the minimum value of the endpoint of the range, the adverse effect will be that the temperature is too low, which will cause unstable rolling.
[0074] The reason for controlling the rough rolling outlet temperature is that within this temperature range, the temperature of the slab entering the rolling mill can be guaranteed; when the temperature value is greater than the maximum value of the endpoint of the range, the adverse effect will be that the temperature is too high, which will cause energy waste; when the temperature value is less than the minimum value of the endpoint of the range, the adverse effect will be that the temperature is too low, which will cause rolling instability.
[0075] As an optional implementation, the end temperature of the induction heating is 1050-1150°C.
[0076] The reason for controlling the end temperature of induction heating is that the finishing rolling adopts 5-stand rolling, and the temperature drop during the finishing rolling process is large. In order to ensure the final rolling temperature at 820-880℃, the slab must be kept at a higher temperature before entering the finishing mill, so that the slab meets the final rolling temperature requirements after the finishing rolling. When semi-headless or headless rolling is adopted, the rolling rate is slow and the temperature drop during the finishing rolling process is large, so the required finishing rolling inlet temperature (induction heating end temperature) is high. When single billet rolling is adopted, the finishing rolling rate is fast, and the temperature drop during the finishing rolling process is small compared with semi-headless and headless rolling. Therefore, the required finishing rolling inlet temperature is low, but the finishing rolling inlet temperature must meet the requirement of >1050℃.
[0077] As an optional implementation manner, the cumulative deformation of the finishing rolling is 70-80%, the final rolling temperature of the finishing rolling is 820-880° C., and the number of finishing rolling passes is 5.
[0078] The reason for controlling the cumulative deformation is that within the deformation range, the grain structure can be refined and the strength and toughness of the product can be improved. When the cumulative deformation value is greater than the maximum value of the endpoint of the range, the adverse effect will be that the deformation is too large, which will cause the strength of the product to be too high. When the cumulative deformation value is less than the minimum value of the endpoint of the range, the adverse effect will be that the deformation is too low, which will cause the strength of the product to be insufficient.
[0079] The reason for controlling the final rolling temperature of finishing rolling is that within this temperature range, the final microstructure of the product can be guaranteed to be uniform; when the temperature value is greater than the maximum value of the endpoint of the range, the adverse effect will be that the temperature is too high, which will lead to unstable rolling; when the temperature value is less than the minimum value of the endpoint of the range, the adverse effect will be that the temperature is too low, which will cause finishing rolling in the two-phase region, and the resulting microstructure will be uneven.
[0080] As an optional implementation, the cooling rate of the laminar cooling is ≥30°C, and the coiling temperature is 250-400°C.
[0081] The reason for controlling the cooling rate of laminar cooling is that within the cooling rate range, the required metallographic structure and mechanical properties can be obtained; when the cooling rate value is greater than the maximum value of the endpoint of the range, the adverse effect will be that the cooling rate is too fast, different structures will be obtained, and the performance of the final product will be affected; when the cooling rate value is less than the minimum value of the endpoint of the range, the adverse effect will be that the cooling rate is too slow, different structures will be obtained, and the performance of the final product will be affected.
[0082] The reason for controlling the coiling temperature is that within this temperature range, the final structure of the product can be guaranteed to be uniform; when the temperature value is greater than the maximum value of the endpoint of the range, the adverse effect will be that the temperature is too high, different structures will be obtained, and the performance of the final product will be affected; when the temperature value is less than the minimum value of the endpoint of the range, the adverse effect will be that the temperature is too low, different structures will be obtained, and the performance of the final product will be affected.
[0083] The present application will be described in detail below with reference to embodiments, comparative examples and experimental data.
[0084] Example 1
[0085] A thin gauge hot rolled steel having the following chemical compositions by mass percentage:
[0086] C: 0.23%, Si: 0.021%, Mn: 2.86%, Al: 0.031%, P: 0.005%, S: 0.0015%, Nb: 0.033%, Ti: 0.015%, Cr: 0.30%, N: 0.0028%, B: 0.0015%, and the balance is Fe and inevitable impurities.
[0087] The metallographic structure of thin gauge hot rolled steel is martensite.
[0088] The thickness of thin gauge hot rolled steel is 0.8mm.
[0089] The method for preparing the thin hot-rolled steel comprises the following steps:
[0090] S1. After KR desulfurization, converter smelting, LF refining and VD refining, molten steel with chemical composition is obtained.
[0091] S2. Continuously cast the molten steel to obtain a slab.
[0092] S3. The slab is subjected to preheating, rough dephosphorization, rough rolling, induction heating, fine dephosphorization, fine rolling, laminar cooling, coiling and air cooling to obtain thin-gauge hot-rolled steel.
[0093] in:
[0094] Finish rolling is full headless rolling;
[0095] Fine descaling is for the sole purpose of removing phosphorus;
[0096] The end temperature of preheating is 1200°C;
[0097] The casting speed is 4.9 m / min, and the thickness of the slab is 110 mm.
[0098] The pressure of rough phosphorus removal is 35MPa, the pressure of fine phosphorus removal is 37MPa, and the distance between the nozzle of fine phosphorus removal and the slab is 60mm;
[0099] The inlet temperature of rough rolling is 1130°C, the outlet temperature of rough rolling is 930°C, and the number of rough rolling passes is 3;
[0100] The end point temperature of induction heating is 1100°C;
[0101] The cumulative deformation of the finishing rolling is 80%, the final rolling temperature of the finishing rolling is 840°C, and the number of passes of the finishing rolling is 5;
[0102] The cooling rate of the laminar cooling was 35°C / s, and the coiling temperature was 350°C.
[0103] Example 2
[0104] A thin gauge hot rolled steel having the following chemical compositions by mass percentage:
[0105] C: 0.21%, Si: 0.033%, Mn: 2.26%, Al: 0.025%, P: 0.006%, S: 0.0040%, Nb: 0.025%, Ti: 0.025%, Cr: 0.25%, N: 0.0032%, B: 0.0024%, and the balance is Fe and inevitable impurities.
[0106] The metallographic structure of thin gauge hot rolled steel is martensite.
[0107] The thickness of thin gauge hot rolled steel is 1.0mm.
[0108] The method for preparing the thin hot-rolled steel comprises the following steps:
[0109] S1. After KR desulfurization, converter smelting, LF refining and VD refining, molten steel with chemical composition is obtained.
[0110] S2. Continuously cast the molten steel to obtain a slab.
[0111] S3. The slab is subjected to preheating, rough dephosphorization, rough rolling, induction heating, fine dephosphorization, fine rolling, laminar cooling, coiling and air cooling to obtain thin-gauge hot-rolled steel.
[0112] in:
[0113] Finish rolling is full headless rolling;
[0114] Fine descaling is for the sole purpose of removing phosphorus;
[0115] The end temperature of preheating is 1200°C;
[0116] The casting speed is 4.9 m / min, and the thickness of the slab is 110 mm.
[0117] The pressure of rough phosphorus removal is 35MPa, the pressure of fine phosphorus removal is 37MPa, and the distance between the nozzle of fine phosphorus removal and the slab is 65mm;
[0118] The inlet temperature of rough rolling is 1140°C, the outlet temperature of rough rolling is 940°C, and the number of rough rolling passes is 3;
[0119] The end point temperature of induction heating is 1100°C;
[0120] The cumulative deformation of the finishing rolling is 80%, the final rolling temperature of the finishing rolling is 840°C, and the number of passes of the finishing rolling is 5;
[0121] The cooling rate of the laminar cooling was 35°C / s, and the coiling temperature was 330°C.
[0122] Example 3
[0123] A thin gauge hot rolled steel having the following chemical compositions by mass percentage:
[0124] C: 0.19%, Si: 0.031%, Mn: 2.05%, Al: 0.040%, P: 0.007%, S: 0.0030%, Nb: 0.030%, Ti: 0.019%, Cr: 0.38%, N: 0.0030%, B: 0.0020%, and the balance is Fe and inevitable impurities.
[0125] The metallographic structure of thin gauge hot rolled steel is martensite.
[0126] The thickness of thin gauge hot rolled steel is 1.2mm.
[0127] The method for preparing the thin hot-rolled steel comprises the following steps:
[0128] S1. After KR desulfurization, converter smelting, LF refining and VD refining, molten steel with chemical composition is obtained.
[0129] S2. Continuously cast the molten steel to obtain a slab.
[0130] S3. The slab is subjected to preheating, rough dephosphorization, rough rolling, induction heating, fine dephosphorization, fine rolling, laminar cooling, coiling and air cooling to obtain thin-gauge hot-rolled steel.
[0131] in:
[0132] Finish rolling is full headless rolling;
[0133] Fine descaling is for the sole purpose of removing phosphorus;
[0134] The end temperature of preheating is 1200°C;
[0135] The casting speed is 5.0 m / min, and the thickness of the slab is 110 mm.
[0136] The pressure of rough phosphorus removal is 35MPa, the pressure of fine phosphorus removal is 37MPa, and the distance between the nozzle of fine phosphorus removal and the slab is 65mm;
[0137] The inlet temperature of rough rolling is 1150℃, the outlet temperature of rough rolling is 940℃, and the number of rough rolling passes is 3;
[0138] The end point temperature of induction heating is 1120°C;
[0139] The cumulative deformation of the finishing rolling is 78%, the final rolling temperature of the finishing rolling is 840°C, and the number of finishing rolling passes is 5;
[0140] The cooling rate of the laminar cooling was 38°C / s, and the coiling temperature was 330°C.
[0141] Example 4
[0142] A thin gauge hot rolled steel having the following chemical compositions by mass percentage:
[0143] C: 0.21%, Si: 0.035%, Mn: 2.80%, Al: 0.032%, P: 0.009%, S: 0.0050%, Nb: 0.028%, Ti: 0.023%, Cr: 0.42%, N: 0.0029%, B: 0.0018%, and the balance is Fe and inevitable impurities.
[0144] The metallographic structure of thin gauge hot rolled steel is martensite.
[0145] Thin gauge hot rolled steel has a thickness of 1.5mm.
[0146] The method for preparing the thin hot-rolled steel comprises the following steps:
[0147] S1. After KR desulfurization, converter smelting, LF refining and VD refining, molten steel with chemical composition is obtained.
[0148] S2. Continuously cast the molten steel to obtain a slab.
[0149] S3. The slab is subjected to preheating, rough dephosphorization, rough rolling, induction heating, fine dephosphorization, fine rolling, laminar cooling, coiling and air cooling to obtain thin-gauge hot-rolled steel.
[0150] in:
[0151] Finish rolling is full headless rolling;
[0152] Fine descaling is for the sole purpose of removing phosphorus;
[0153] The end temperature of preheating is 1200°C;
[0154] The casting speed is 5.2 m / min, and the thickness of the slab is 110 mm.
[0155] The pressure of rough phosphorus removal is 35MPa, the pressure of fine phosphorus removal is 37MPa, and the distance between the nozzle of fine phosphorus removal and the slab is 68mm;
[0156] The inlet temperature of rough rolling is 1160℃, the outlet temperature of rough rolling is 935℃, and the number of rough rolling passes is 3;
[0157] The end point temperature of induction heating is 1120°C;
[0158] The cumulative deformation of the finishing rolling is 78%, the final rolling temperature of the finishing rolling is 820°C, and the number of finishing rolling passes is 5;
[0159] The cooling rate of the laminar cooling was 40°C, and the coiling temperature was 300°C.
[0160] Example 5
[0161] A thin gauge hot rolled steel having the following chemical compositions by mass percentage:
[0162] C: 0.16%, Si: 0.038%, Mn: 2.43%, Al: 0.043%, P: 0.005%, S: 0.0020%, Nb: 0.013%, Ti: 0.028%, Cr: 0.38%, N: 0.0022%, B: 0.0017%, and the balance is Fe and inevitable impurities.
[0163] The metallographic structure of thin gauge hot rolled steel is martensite.
[0164] The thickness of thin gauge hot rolled steel is 2.0mm.
[0165] The method for preparing the thin hot-rolled steel comprises the following steps:
[0166] S1. After KR desulfurization, converter smelting, LF refining and VD refining, molten steel with chemical composition is obtained.
[0167] S2. Continuously cast the molten steel to obtain a slab.
[0168] S3. The slab is subjected to preheating, rough dephosphorization, rough rolling, induction heating, fine dephosphorization, fine rolling, laminar cooling, coiling and air cooling to obtain thin-gauge hot-rolled steel.
[0169] in:
[0170] Finish rolling is full headless rolling;
[0171] Fine descaling is for the sole purpose of removing phosphorus;
[0172] The end temperature of preheating is 1180℃;
[0173] The casting speed is 5.5 m / min, and the thickness of the slab is 110 mm.
[0174] The pressure of rough phosphorus removal is 35MPa, the pressure of fine phosphorus removal is 38MPa, and the distance between the nozzle of fine phosphorus removal and the slab is 70mm;
[0175] The inlet temperature of rough rolling is 1150℃, the outlet temperature of rough rolling is 942℃, and the number of rough rolling passes is 3;
[0176] The end point temperature of induction heating is 1140°C;
[0177] The cumulative deformation of the finishing rolling is 75%, the final rolling temperature of the finishing rolling is 820°C, and the number of passes of the finishing rolling is 5;
[0178] The cooling rate of the laminar cooling was 45°C, and the coiling temperature was 280°C.
[0179] Example 6
[0180] A thin gauge hot rolled steel having the following chemical compositions by mass percentage:
[0181] C: 0.24%, Si: 0.042%, Mn: 2.50%, Al: 0.034%, P: 0.009%, S: 0.0050%, Nb: 0.038%, Ti: 0.013%, Cr: 0.33%, N: 0.0025%, B: 0.0025%, and the balance is Fe and inevitable impurities.
[0182] The metallographic structure of thin gauge hot rolled steel is martensite.
[0183] The thickness of thin gauge hot rolled steel is 3.0mm.
[0184] The method for preparing the thin hot-rolled steel comprises the following steps:
[0185] S1. After KR desulfurization, converter smelting, LF refining and VD refining, molten steel with chemical composition is obtained.
[0186] S2. Continuously cast the molten steel to obtain a slab.
[0187] S3. The slab is subjected to preheating, rough dephosphorization, rough rolling, induction heating, fine dephosphorization, fine rolling, laminar cooling, coiling and air cooling to obtain thin-gauge hot-rolled steel.
[0188] in:
[0189] Finish rolling is full headless rolling;
[0190] Fine descaling is for the sole purpose of removing phosphorus;
[0191] The end temperature of preheating is 1180℃;
[0192] The casting speed is 6.0 m / min, and the thickness of the slab is 110 mm.
[0193] The pressure of rough phosphorus removal is 36MPa, the pressure of fine phosphorus removal is 38MPa, and the distance between the nozzle of fine phosphorus removal and the slab is 75mm;
[0194] The inlet temperature of rough rolling is 1130°C, the outlet temperature of rough rolling is 933°C, and the number of rough rolling passes is 3;
[0195] The end point temperature of induction heating is 1140°C;
[0196] The cumulative deformation of the finishing rolling is 75%, the final rolling temperature of the finishing rolling is 800°C, and the number of passes of the finishing rolling is 5;
[0197] The cooling rate of the laminar cooling was 45°C, and the coiling temperature was 250°C.
[0198] Example 7
[0199] A thin gauge hot rolled steel having the following chemical compositions by mass percentage:
[0200] C: 0.23%, Si: 0.021%, Mn: 2.45%, Al: 0.024%, P: 0.006%, S: 0.0019%, Nb: 0.028%, Ti: 0.027%, Cr: 0.45%, N: 0.0030%, B: 0.0022%, and the balance is Fe and inevitable impurities.
[0201] The metallographic structure of thin gauge hot rolled steel is martensite.
[0202] The thickness of thin gauge hot rolled steel is 4.0mm.
[0203] The method for preparing the thin hot-rolled steel comprises the following steps:
[0204] S1. After KR desulfurization, converter smelting, LF refining and VD refining, molten steel with chemical composition is obtained.
[0205] S2. Continuously cast the molten steel to obtain a slab.
[0206] S3. The slab is subjected to preheating, rough dephosphorization, rough rolling, induction heating, fine dephosphorization, fine rolling, laminar cooling, coiling and air cooling to obtain thin-gauge hot-rolled steel.
[0207] in:
[0208] Finish rolling is semi-endless rolling;
[0209] Fine descaling is for the sole purpose of removing phosphorus;
[0210] The end temperature of preheating is 1150℃;
[0211] The casting speed is 4.5 m / min, and the thickness of the slab is 110 mm.
[0212] The pressure of rough phosphorus removal is 36MPa, the pressure of fine phosphorus removal is 37MPa, and the distance between the nozzle of fine phosphorus removal and the slab is 80mm;
[0213] The inlet temperature of rough rolling is 1100°C, the outlet temperature of rough rolling is 970°C, and the number of rough rolling passes is 3;
[0214] The end point temperature of induction heating is 1060°C;
[0215] The cumulative deformation of the finishing rolling is 70%, the final rolling temperature of the finishing rolling is 860°C, and the number of passes of the finishing rolling is 5;
[0216] The cooling rate of the laminar cooling was 45°C, and the coiling temperature was 280°C.
[0217] Comparative Example 1
[0218] A thin gauge hot rolled steel having the following chemical compositions by mass percentage:
[0219] C: 0.07%, Si: 0.20%, Mn: 1.8%, Al: 0.024%, P: 0.006%, S: 0.0019%, Mo: 0.28%, Ti: 0.09%, N: 0.0030%, and the balance is Fe and inevitable impurities.
[0220] The metallographic structure of thin gauge hot rolled steel is ferrite.
[0221] The thickness of thin gauge hot rolled steel is 2.0mm.
[0222] The method for preparing the thin hot-rolled steel comprises the following steps:
[0223] S1. After KR desulfurization, converter smelting, LF refining and VD refining, molten steel with chemical composition is obtained.
[0224] S2. Continuously cast the molten steel to obtain a slab.
[0225] S3. The slab is subjected to preheating, rough descaling, rough rolling, fine descaling, fine rolling, laminar cooling, coiling and air cooling to obtain thin-gauge hot-rolled steel.
[0226] in:
[0227] Finish rolling is single billet rolling;
[0228] Fine descaling is double descaling;
[0229] The end temperature of preheating is 1250℃;
[0230] The casting speed is 0.8m / min, and the thickness of the slab is 240mm.
[0231] The pressure of rough descaling is 22MPa, the pressure of fine descaling is 22MPa, and the distance between the nozzle of fine descaling and the slab is 110mm;
[0232] The inlet temperature of rough rolling is 1100°C, the outlet temperature of rough rolling is 970°C, and the number of rough rolling passes is 3;
[0233] Finishing rolling inlet temperature 1090℃;
[0234] The cumulative deformation of the finishing rolling is 70%, the final rolling temperature of the finishing rolling is 880°C, and the number of passes of the finishing rolling is 7;
[0235] The cooling rate of the laminar cooling was 20°C / s, and the coiling temperature was 650°C.
[0236] Comparative Example 2
[0237] A thin gauge hot rolled steel having the following chemical compositions by mass percentage:
[0238] C: 0.15%, Si: 0.20%, Mn: 1.8%, Al: 0.024%, P: 0.006%, S: 0.0019%, Ti: 0.09%, Cr: 0.30%, N: 0.0030%, and the balance is Fe and inevitable impurities.
[0239] The metallographic structure of thin gauge hot rolled steel is martensite.
[0240] The thickness of thin gauge hot rolled steel is 3.0mm.
[0241] The method for preparing the thin hot-rolled steel comprises the following steps:
[0242] S1. After KR desulfurization, converter smelting, LF refining and VD refining, molten steel with chemical composition is obtained.
[0243] S2. Continuously cast the molten steel to obtain a slab.
[0244] S3. The slab is subjected to preheating, rough descaling, rough rolling, fine descaling, fine rolling, laminar cooling, coiling and air cooling to obtain thin-gauge hot-rolled steel.
[0245] in:
[0246] Finish rolling is single billet rolling;
[0247] Fine descaling is double descaling;
[0248] The end temperature of preheating is 1250℃;
[0249] The casting speed is 0.8m / min, and the thickness of the slab is 240mm.
[0250] The pressure of rough descaling is 22MPa, the pressure of fine descaling is 22MPa, and the distance between the nozzle of fine descaling and the slab is 110mm;
[0251] The inlet temperature of rough rolling is 1100°C, the outlet temperature of rough rolling is 970°C, and the number of rough rolling passes is 3;
[0252] Finishing rolling inlet temperature 1090℃;
[0253] The cumulative deformation of the finishing rolling is 88%, the final rolling temperature of the finishing rolling is 880°C, and the number of finishing rolling passes is 7;
[0254] The cooling rate of the laminar cooling was 30°C / s, and the coiling temperature was 350°C.
[0255] Comparative Example 3
[0256] A thin gauge hot rolled steel having the following chemical compositions by mass percentage:
[0257] C: 0.20%, Si: 0.20%, Mn: 1.2%, Al: 0.024%, P: 0.006%, S: 0.0019%, Ti: 0.025%, Cr: 0.30%, N: 0.0030%, B: 0.0030%, and the balance is Fe and inevitable impurities.
[0258] The metallographic structure of thin gauge hot rolled steel is bainite.
[0259] The thickness of thin gauge hot rolled steel is 3.0mm.
[0260] The method for preparing the thin hot-rolled steel comprises the following steps:
[0261] S1. After KR desulfurization, converter smelting, LF refining and VD refining, molten steel with chemical composition is obtained.
[0262] S2. Continuously cast the molten steel to obtain a slab.
[0263] S3. The slab is subjected to preheating, rough descaling, rough rolling, fine descaling, fine rolling, laminar cooling, coiling and air cooling to obtain thin-gauge hot-rolled steel.
[0264] in:
[0265] Finish rolling is single billet rolling;
[0266] Fine descaling is double descaling;
[0267] The end temperature of preheating is 1250℃;
[0268] The casting speed is 0.8m / min, and the thickness of the slab is 240mm.
[0269] The pressure of rough descaling is 22MPa, the pressure of fine descaling is 22MPa, and the distance between the nozzle of fine descaling and the slab is 110mm;
[0270] The inlet temperature of rough rolling is 1100°C, the outlet temperature of rough rolling is 970°C, and the number of rough rolling passes is 3;
[0271] Finishing rolling inlet temperature 1090℃;
[0272] The cumulative deformation of the finishing rolling is 88%, the final rolling temperature of the finishing rolling is 880°C, and the number of finishing rolling passes is 7;
[0273] The cooling rate of the laminar cooling was 30°C / s, and the coiling temperature was 550°C.
[0274] Experimental example
[0275] The performance of the thin-gauge hot-rolled steel provided in Examples 1-7 and Comparative Examples 1-3 was tested, and the specific results are shown in Table 1.
[0276] The processing method is:
[0277] Yield strength: in accordance with GB / T 228.1-2010 Tensile test of metallic materials Part 1: Room temperature test method;
[0278] Tensile strength: in accordance with GB / T 228.1-2010 Tensile test for metallic materials Part 1: Room temperature test method;
[0279] Elongation: According to GB / T 228.1-2010 Tensile test of metallic materials Part 1: Room temperature test method;
[0280] Transverse cold bending: in accordance with GB / T 228.1-2010 Tensile tests on metallic materials Part 1: Room temperature test methods.
[0281] Table 1
[0282] Yield strength(MPa) Tensile strength(MPa) Elongation(%) Horizontal cold bending Example 1 981 1071 9 qualified Example 2 931 1050 10 qualified Example 3 951 1033 9.5 qualified Example 4 975 1076 11.5 qualified Example 5 923 1106 10.5 qualified Example 6 943 1133 11.5 qualified Example 7 967 1093 12.5 qualified Comparative Example 1 785 863 15.2 qualified Comparative Example 2 638 792 17.8 qualified Comparative Example 3 587 724 19.0 qualified
[0283] Table 1 Detailed analysis:
[0284] Yield strength refers to the yield limit of steel when it yields, that is, the stress that resists slight plastic deformation. The higher the yield strength, the greater the yield limit of steel when it yields.
[0285] Tensile strength refers to the maximum stress value that steel can withstand before it breaks. The greater the tensile strength, the higher the maximum stress value of the filament.
[0286] Elongation refers to the percentage of the total deformation ΔL of the gauge section after the steel is tensile fractured to the original gauge length L. The higher the elongation, the stronger the tensile resistance of the steel.
[0287] Transverse cold bending refers to the degree of bending that steel can withstand at room temperature. The greater the transverse cold bending, the greater the degree of bending that the steel can withstand.
[0288] From the data of Examples 1-7, it can be seen that:
[0289] The present invention adopts a multi-mode thin slab continuous casting and rolling production line. By adjusting the chemical composition of the steel and improving the continuous casting and rolling processes, the steel yield strength can be obtained to be greater than 900Mpa, the tensile strength is greater than 1000Mpa MPa, the elongation is greater than 8%, the transverse cold bending D=2a, 180° is qualified, and the steel plate shape is good, the dimensional accuracy is high, the strength fluctuation is small, and the steel plate thickness can be controlled within 0.8-4.0mm.
[0290] Explanation of the attached figure:
[0291] Figure 2 The metallographic structure diagram of the thin gauge hot-rolled steel provided in the embodiment of the present application is Figure 2 It can be seen that the structure is martensite.
[0292] Finally, it should be noted that the terms "comprises," "includes," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements that are inherent to such process, method, article, or apparatus.
[0293] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0294] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A thin gauge hot rolled steel, characterized in that: The chemical composition of the steel includes by mass percentage: C: 0.15-0.25%, Si: ≤0.05%, Mn: 2.0-3.0%, Al: 0.02-0.35%, P: ≤0.010%, S: ≤0.005%, Nb: 0.01-0.10%, Ti: 0.010-0.030%, Cr: 0.1-0.5%, N: ≤0.004%, B: 0.0010-0.0025%, the balance is Fe and inevitable impurities; the metallographic structure of the thin gauge hot-rolled steel is martensite, the metallographic structure of the thin gauge hot-rolled steel is martensite, the yield strength is greater than 900MPa, the tensile strength is greater than 1000MPa, the elongation is greater than 8%, the transverse cold bending D=2a, 180° is qualified, and the thickness can reach 0.8-4.0mm. The preparation method of the thin gauge hot-rolled steel consists of the following steps: After KR desulfurization, converter smelting, LF refining and VD refining, molten steel meeting the chemical composition is obtained; The molten steel is continuously cast to obtain a slab; The slab is subjected to preheating, rough dephosphorization, rough rolling, induction heating, fine dephosphorization, fine rolling, laminar cooling, coiling and air cooling to obtain the thin gauge hot rolled steel; Wherein: the distance between the nozzle for fine dephosphorization and the slab is 60-110 mm, the coiling temperature is 250-400°C, the final rolling temperature of the fine rolling is 820-880°C, and the cooling rate of the laminar cooling is ≥30°C.
2. A method for preparing thin gauge hot rolled steel as claimed in claim 1, characterized in that: It consists of the following steps: After KR desulfurization, converter smelting, LF refining and VD refining, molten steel meeting the chemical composition is obtained; The molten steel is continuously cast to obtain a slab; The slab is subjected to preheating, rough dephosphorization, rough rolling, induction heating, fine dephosphorization, fine rolling, laminar cooling, coiling and air cooling to obtain the thin gauge hot rolled steel; in: The finishing rolling is any one of single billet rolling, semi-endless rolling and full endless rolling; The fine descaling is single removal of phosphorus or double removal of phosphorus; When the finishing rolling is single-bill mode rolling, the finishing descaling is double dephosphorization; When the finishing rolling is semi-endless mode rolling or full-endless mode rolling, the finishing dephosphorization is single dephosphorization.
3. The method for preparing thin-gauge hot-rolled steel according to claim 2, characterized in that: The end point temperature of the preheating is 1150-1200°C.
4. The method for preparing thin-gauge hot-rolled steel according to claim 2, characterized in that: The continuous casting speed is 4.0-6.5 m / min, and the continuous casting slab thickness is 110-123 mm.
5. The method for preparing thin gauge hot rolled steel according to claim 2, characterized in that: The pressure of the rough phosphorus removal is ≥30MPa, and the pressure of the fine phosphorus removal is ≥30MPa.
6. The method for preparing thin gauge hot rolled steel according to claim 2, characterized in that: The inlet temperature of the rough rolling is ≥1150°C, the outlet temperature of the rough rolling is 930-1000°C, and the number of passes of the rough rolling is 3.
7. The method for preparing thin-gauge hot-rolled steel according to claim 2, characterized in that: The end point temperature of the induction heating is 1050-1150°C.
8. The method for preparing thin gauge hot rolled steel according to claim 2, characterized in that: The cumulative deformation of the finish rolling is 70-80%, and the number of passes of the finish rolling is 5.
Citation Information
Patent Citations
1500MPa-grade hot forming steel and preparation method thereof
CN114012056A