A method for densifying EVA lamination in photovoltaic modules

By using uniform electric and magnetic fields to rearrange EVA film molecules during the photovoltaic module lamination process, combined with segmented lamination technology, the problems of uneven light transmittance and uneven adhesion caused by the disordered three-dimensional network structure were solved, achieving efficient production and high-quality finished products of photovoltaic modules.

CN115810695BActive Publication Date: 2026-11-10FUTURA NEW ENERGY TECH (JIANGSU) CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211631810.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-19
Publication Date
2026-11-10
Estimated Expiration
2042-12-19

AI Technical Summary

Technical Problem

In the existing photovoltaic module lamination process, the three-dimensional network structure formed by heating EVA material is disordered, resulting in uneven light transmittance and uneven adhesion, which affects the photoelectric conversion efficiency and strength of photovoltaic modules.

Method used

By using a uniform electric field and a uniform magnetic field to rearrange the ethylene and vinyl acetate copolymer molecules in the molten state of the EVA film, combined with a segmented lamination process, an ordered three-dimensional network structure is formed. Through multiple lamination and encapsulation by the left pre-lamination machine, the right pre-lamination machine, and the rear lamination machine, uniform adhesion between the EVA film and the glass and the battery cell assembly is ensured.

Benefits of technology

This achieves uniform light transmittance and consistent adhesion of photovoltaic modules, improving the photoelectric conversion efficiency and usage intensity of photovoltaic modules, while reducing production costs and increasing production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115810695B_ABST
    Figure CN115810695B_ABST
Patent Text Reader

Abstract

This invention relates to the field of photovoltaic cell technology, specifically to a method for densifying EVA lamination in photovoltaic modules. The invention first prepares an upper panel and a lower panel that mate with the front and back of the cell assembly. Then, using a fixing assembly, the upper panel, cell assembly, and lower panel are sequentially stacked and shaped. Next, they are laminated and encapsulated using a segmented lamination method. During the encapsulation process, varying electric and magnetic fields are used to control the orderly arrangement and uniform spatial distribution of the three-dimensional network structure formed by the molten EVA film, resulting in photovoltaic modules with uniform light transmittance and consistent adhesion throughout. This invention effectively solves the problems of low photoelectric conversion efficiency and low durability in existing photovoltaic module production technologies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photovoltaic cell technology, and more specifically to a method for densifying EVA lamination in photovoltaic modules. Background Technology

[0002] Photovoltaic modules are the core of a solar power generation system. Their function is to convert solar energy into electrical energy, which can be stored in batteries or used to power loads. Photovoltaic modules are usually made up of layers of backsheet, lower EVA, solar cells, upper EVA and tempered glass, which are then laminated together. The quality of the finished product directly determines the quality of the entire solar power generation system.

[0003] The photovoltaic module manufacturing process consists of the following steps: cell sorting, welding, stacking, lamination, trimming and framing, and wiring inspection. Among these, the lamination process is the key step. Currently, the lamination process generally involves placing the laid cells into a laminator, removing the air trapped between the layers of the module through vacuuming, then heating the EVA material (EVA is a copolymer of ethylene and vinyl acetate, with the molecular formula (C2H4)x.(C4H6O2)y) to melt it (resulting in a cross-linking reaction to form a three-dimensional network structure). This melts the EVA material and bonds it to the glass and backsheet on both sides of the cell, respectively. After cooling, the photovoltaic module is removed.

[0004] A photovoltaic module lamination process is disclosed in patent application number CN201611260868.0, comprising the following steps: ① Providing photovoltaic modules and a laminator for laminating the photovoltaic modules, the laminator being equipped with a heating plate and a self-heating plate on top of the photovoltaic modules; ② Setting lamination parameters on the laminator, and after the heating plate and self-heating plate reach the specified temperatures, placing the photovoltaic modules into the laminator and closing the lid; ③ Performing a vacuum operation between the layers of the photovoltaic modules; ④ Then pressurizing the upper chamber of the laminator, pressing the self-heating plate down to the top of the photovoltaic modules, with the self-heating plate and the heating plate simultaneously heating the photovoltaic modules; ⑤ After lamination, inflating the lower chamber of the laminator, evacuating the upper chamber, opening the lid, and removing the photovoltaic modules, thus completing the lamination process. This setup effectively controls the heating temperature of the photovoltaic modules at different stages, shortens the photovoltaic module lamination time, and improves production efficiency.

[0005] However, the aforementioned comparative documents have obvious defects in actual operation: they cannot control the three-dimensional network structure formed by the cross-linking reaction of EVA material after heating (that is, the three-dimensional network structure formed by the cross-linking reaction of EVA material after heating is disordered).

[0006] This results in uneven light transmittance in the produced photovoltaic modules, which in turn affects the photoelectric conversion efficiency of the photovoltaic modules. In addition, this disordered three-dimensional network structure also leads to uneven adhesion between EVA, glass, and solar cells, which in turn affects the strength of the photovoltaic modules. Summary of the Invention

[0007] The purpose of this invention is to overcome the shortcomings of the prior art and solve the problems mentioned in the background art.

[0008] To achieve the above objectives, the present invention adopts the following technical solution: a method for densifying EVA lamination in photovoltaic modules, comprising the following steps: S1, Clean the glass surface and then inspect for defects; S2, the glass is divided into two parts. One part of the glass has an EVA film and a left mold plate laid flat on its inner side in sequence. The other part of the glass has an EVA film and a right mold plate laid flat on its inner side in sequence. Then the two parts of the glass are placed into the left pre-lamination machine and the right pre-lamination machine respectively for pre-treatment. The left pre-lamination machine and the right pre-lamination machine respectively bond the glass and the EVA film together to form the upper panel and the lower panel. S3, remove burrs from the edges of the top and bottom panels, and then inspect the top and bottom panels for defects; S4. The solar cells and the busbar are connected by welding to form a cell pack. Then the surface of the cell pack is cleaned and the cell pack is inspected for defects. S5, remove the left mold plate on the upper panel and the right mold plate on the lower panel, then the upper panel and the lower panel clamp the cell group and place it in the rear laminator for lamination, thereby bonding the upper panel, cell group and lower panel together to form a photovoltaic module; S6, remove burrs from the edges of the photovoltaic module, and then perform performance testing on the photovoltaic module; The cavities of the left pre-laminator, right pre-laminator, and rear laminator are also equipped with electrode plates and electromagnets. The electrode plates and electromagnets can generate uniform electric fields and uniform magnetic fields in six directions along the X, Y, and Z axes. At the same time, the directions of the uniform electric field and the uniform magnetic field are perpendicular to each other, and at the same time, the uniform electric field and the uniform magnetic field each have only one direction. Furthermore, the directions of the uniform electric field and the uniform magnetic field change with time. During the pretreatment in S2 and the lamination process in S5, the uniform electric field attracts and rearranges the ethylene and vinyl acetate copolymer molecules in the molten EVA film, thereby increasing the macromolecular structure aligned along the electric field direction. At the same time, the polar molecules in the molten EVA film are also affected by the uniform magnetic field during their movement and change direction, thereby reducing or even eliminating the network irregular cross-linked structure of the ethylene and vinyl acetate copolymer molecules in the EVA film.

[0009] Furthermore, processes S1 to S6 are all completed in a fully automated workshop with constant temperature, humidity, and dust-free conditions.

[0010] Furthermore, in S1 and S4, the glass and battery cell assembly are cleaned using dry ice cleaning, and a negative pressure suction device is simultaneously used to remove impurities and debris during the dry ice cleaning process.

[0011] Furthermore, in S1, S3, and S4, the defect detection employs machine vision technology.

[0012] Furthermore, in S2, the inner surfaces of the left mold plate and the right mold plate are coated with a non-stick layer, and the embossed shapes of the left mold plate and the right mold plate are the same as the shapes of the top and bottom of the battery cell assembly in S4, respectively.

[0013] Furthermore, in S2 and S5, during the stacking of glass and the left mold plate, the stacking of glass and the right mold plate, and the stacking of the upper panel and the lower panel, a detachable fixing component is used for shaping. The fixing component includes four shaping frames and two elastic bands. The shaping frame consists of a main telescopic rod, a secondary telescopic rod, a right-angle arm, and a vacuum suction cup. The two right-angle arms are arranged in parallel and connected in the middle by the main telescopic rod. Two secondary telescopic rods are symmetrically distributed on both sides of the main telescopic rod, and the two ends of the two secondary telescopic rods are respectively connected to the corresponding right-angle arms. The ends of the right-angle arms are provided with inward-facing vacuum suction cups. The outer wall of the fixing rod of the main telescopic rod is provided with a guide groove block that cooperates with the elastic band. In S2, when the glass and the left mold plate are stacked, a first robotic arm extends from each of the four top corners of the glass. Each first robotic arm holds a shaping frame. The first robotic arm holds the shaping frame close to the glass, so that the two vacuum suction cups at the lower end of the shaping frame are respectively attached to the two adjacent side walls of the glass, and the two vacuum suction cups at the upper end of the shaping frame are respectively attached to the two adjacent side walls of the left mold plate. Then the first robotic arm retracts. Then a second robotic arm extends from the top of the glass. The second robotic arm opens the elastic band and puts it on the guide groove block. Then the second robotic arm retracts. In S2, when the glass and the right mold plate are stacked, a first robotic arm extends from each of the four top corners of the glass. Each first robotic arm holds a shaping frame. The first robotic arm holds the shaping frame close to the glass, so that the two vacuum suction cups at the lower end of the shaping frame are respectively attached to the two adjacent side walls of the glass, and the two vacuum suction cups at the upper end of the shaping frame are respectively attached to the two adjacent side walls of the right mold plate. Then the first robotic arm retracts. Then a second robotic arm extends from the top of the glass. The second robotic arm opens the elastic band and puts it on the guide groove block. Then the second robotic arm retracts. In S5, when the upper and lower panels are stacked, a first robotic arm extends from each of the four corners of the lower panel. Each first robotic arm holds a shaping frame. The first robotic arm holds the shaping frame close to the lower panel, so that the two vacuum suction cups at the lower end of the shaping frame are respectively attached to the two adjacent side walls of the lower panel, and the two vacuum suction cups at the upper end of the shaping frame are respectively attached to the two adjacent side walls of the upper panel. Then the first robotic arm retracts. Then a second robotic arm extends from the top of the lower panel. The second robotic arm opens the elastic band and puts it on the guide groove block. Then the second robotic arm retracts.

[0014] Furthermore, both the main telescopic rod and the auxiliary telescopic rod are composed of a movable rod with a fixed rod sliding at each end. The ends of the movable rod and the bottom of the groove of the fixed rod are provided with permanent magnets. The permanent magnets are all unipolar magnets made of Helbeck array. Adjacent permanent magnets on the same movable rod central axis repel each other. The elastic band is embedded with a full-length temperature memory alloy wire. When the temperature rises, the full-length temperature memory alloy wire will deform and drive the circumference of the elastic band to shorten.

[0015] Furthermore, the process of manufacturing the upper panel using the left pre-laminator is as follows: Step 1, firstly, the left pre-laminator closes its cavity and evacuates it, then the internal temperature is raised to 135-145°C, then the upper chamber is pressurized and inflated to perform a first lamination and encapsulation of the glass and EVA film, then the lower chamber is evacuated, and then the upper chamber is evacuated until the silicone plate is reset; Step 2, firstly, the left pre-laminator is directly evacuated, then the upper chamber is pressurized and inflated to perform a second lamination and encapsulation of the glass and EVA film, then the lower chamber is evacuated, and then the upper chamber is evacuated to reset the silicone plate. After inflating, the cover is opened, and finally the upper panel is removed from the left pre-laminator and cooled to room temperature; The process of manufacturing the upper panel using the right pre-laminator is as follows: Step 3: First, the right pre-laminator closes its cavity and is evacuated. Then, the internal temperature is raised to 135-145°C. Then, the upper chamber is pressurized and inflated to perform a first lamination and encapsulation of the glass and EVA film. Then, the lower chamber is evacuated, and then the upper chamber is evacuated until the silicone plate is reset. Step 4: First, the right pre-laminator is directly evacuated. Then, the upper chamber is pressurized and inflated to perform a second lamination and encapsulation of the glass and EVA film. Then, the lower chamber is evacuated, and then the upper chamber is evacuated to reset the silicone plate. After inflating, the cover is opened. Finally, the lower panel is removed from the right pre-laminator and cooled to room temperature. The process of manufacturing photovoltaic modules using the post-lamination laminator is as follows: Step 5, firstly, the post-lamination laminator closes its cavity and evacuates the vacuum, then the internal temperature is raised to 135-145 ℃, then the upper chamber is pressurized and inflated to perform a first lamination and encapsulation of the upper and lower panels, then the lower chamber is evacuated, and then the upper chamber is evacuated until the silicone plate is reset; Step 6, firstly, the post-lamination laminator directly evacuates the vacuum, then the upper chamber is pressurized and inflated to perform a second lamination and encapsulation of the upper and lower panels, then the lower chamber is evacuated, and then the upper chamber is evacuated to reset the silicone plate. After inflating the lower chamber, the cover is opened, and finally the photovoltaic module is removed from the left pre-lamination laminator and cooled to room temperature.

[0016] Furthermore, the uniform electric field and uniform magnetic field change direction every 0.02 to 5 seconds.

[0017] Compared with the prior art, the advantages and positive effects of the present invention are as follows: This invention first produces an upper panel and a lower panel that match the shapes of the front and back of the battery cell assembly. Then, the upper panel, battery cell assembly, and lower panel are stacked and shaped sequentially using a fixing component. The assembly is then laminated and encapsulated in a segmented manner. During the encapsulation process, changing electric and magnetic fields are used to control the orderly arrangement and uniform spatial distribution of the three-dimensional network structure formed by the molten EVA film, thereby ensuring that the produced photovoltaic module has uniform light transmittance and consistent adhesion throughout. Attached Figure Description

[0018] Figure 1 This is a visual diagram of the photovoltaic module constructed by stacking the upper panel, battery cell group, and lower panel of the present invention. Figure 2 This is a perspective view of the inner sides of the left and right mold plates of the present invention; Figure 3 This is a perspective view of the inner sides of the upper and lower panels of the present invention; Figure 4 This is a frontal view of the battery pack of the present invention from the side view. Figure 5 This is a perspective view of the auxiliary telescopic rod of the present invention after partial cross-section; Figure 6 For the present invention Figure 1 Enlarged view of region A in the middle; The labels in the diagram represent: 1 - Photovoltaic module; 2 - Left mold plate; 3 - Right mold plate; 4 - Top panel; 5 - Bottom panel; 6 - Cell assembly; 7 - Fixed rod; 8 - Movable rod; 9 - Permanent magnet; 10 - Vacuum chuck; 11 - Main telescopic rod; 12 - Guide slot block; 13 - Elastic band; 14 - Secondary telescopic rod; 15 - Right angle arm. Detailed Implementation

[0019] To better understand the above-mentioned objectives, features, and advantages of the present invention, the present invention will be further described below in conjunction with the accompanying drawings and embodiments. It should be noted that, unless otherwise specified, the embodiments and features described in these embodiments can be combined with each other.

[0020] Numerous specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways than those described herein, and therefore the invention is not limited to the specific embodiments disclosed in the following specification.

[0021] This embodiment describes a method for densifying EVA lamination in photovoltaic modules, referring to... Figure 1-6 Includes the following steps: S1. Clean the glass surface and then inspect for defects.

[0022] S2, the glass is divided into two parts. One part of the glass has EVA film and left mold plate 2 laid flat on its inner side in sequence. The other part of the glass has EVA film and right mold plate 3 laid flat on its inner side in sequence. Then the two parts of the glass are placed into the left pre-lamination machine and the right pre-lamination machine respectively for pre-treatment. The left pre-lamination machine and the right pre-lamination machine respectively bond the glass and EVA film together to form the upper panel 4 and the lower panel 5.

[0023] S3, remove burrs from the edges of the upper panel 4 and the lower panel 5, and then perform defect detection on the upper panel 4 and the lower panel 5.

[0024] S4, the solar cells and the busbar are connected by welding to form a cell group 6, then the surface of the cell group 6 is cleaned, and then the cell group 6 is inspected for defects.

[0025] S5, remove the left mold plate 2 on the upper panel 4 and the right mold plate 3 on the lower panel 5, then the upper panel 4 and the lower panel 5 clamp the cell group 6 and place it in the rear laminator for lamination, thereby bonding the upper panel 4, the cell group 6 and the lower panel 5 together to form the photovoltaic module 1.

[0026] S6, remove the burrs on the edge of photovoltaic module 1, and then perform performance testing on photovoltaic module 1.

[0027] It is worth noting that: The processes S1 to S6 are all completed in a fully automated workshop with constant temperature, humidity and dust-free environment. This is to ensure that there is no contamination from impurities (including external dust, human hair, etc.) during the production of photovoltaic module 1, thereby ensuring the production quality of photovoltaic module 1, while also improving the production efficiency of photovoltaic module 1 and reducing production costs.

[0028] It is worth noting that: In S1 and S4, the glass and cell assembly 6 are cleaned using dry ice. (The principle of dry ice cleaning is to accelerate dry ice particles with compressed air and spray them onto the surface of the object to be cleaned. Due to the extremely low temperature of dry ice (-78℃), the adhering material is quickly frozen and made brittle. At the same time, the dry ice penetrates into the gaps between the object surface and the adhering material. Utilizing the principle that the dry ice itself absorbs heat and vaporizes, its volume expands, causing a micro-explosion inside the adhering material, thereby peeling off the adhering material from the surface of the object to be cleaned. The entire process is a physical change of dry ice and will not damage the cleaning surface or the precision of the object to be cleaned. No secondary pollutants are generated during the cleaning process, and dry ice does not contain water and is non-conductive.) Furthermore, a negative pressure suction device is simultaneously used during the dry ice cleaning process to remove impurities and debris in a timely manner. This is to ensure the cleanliness of the surfaces of the glass, left mold plate 2, right mold plate 3, and cell assembly 6, and to avoid affecting the product quality of photovoltaic module 1 due to impurities on their surfaces.

[0029] It is worth noting that: In S1, S3, and S4, defect detection employs machine vision technology (typically using the working principle of online image scanning with an industrial CCD camera; that is, during high-speed production on the production line, a high-brightness LED industrial linear focusing light source of a specific wavelength is used to illuminate the product surface (for opaque thin film products, the principle of reflection detection is used), while the industrial CCD camera scans and acquires product images of the illuminated area in real time; the system processes the thin film images acquired by the camera using MVI image software algorithms for defect identification. Because the image images of defects differ from those of normal products in grayscale, the system can accurately detect product defects; at the same time, based on the image features of various defects collected in advance and recorded in the defect database, online detection, classification, and subsequent handling of defects are achieved). This is because some common surface defects such as dirt spots, streaks, damage, edge cracks, wrinkles, dark spots, bright spots, edge damage, black spots, hair, and insects have diameters between 0.01mm and 2mm, which the human eye cannot accurately and promptly identify.

[0030] It is worth noting that: In S2, the inner surfaces of the left mold plate 2 and the right mold plate 3 are coated with a non-stick layer (this is to prevent the upper panel 4 from sticking to the left mold plate 2 and the lower panel 5 from sticking to the right mold plate 3 and being unable to be demolded), and the embossed shapes of the left mold plate 2 and the right mold plate 3 are the same as the shapes of the upper and lower parts of the battery cell pack 6 in S4.

[0031] The significance of producing the upper panel 4 and the lower panel 5 in this process is to ensure the stability of the stacking of the upper panel 4, the cell group 6 and the lower panel 5 in the subsequent S5, and at the same time, to suppress the displacement of the busbar and the cell group 6 relative to the glass during the lamination process of the photovoltaic module 1.

[0032] It is worth noting that: In S2 and S5, during the stacking of glass and left mold plate 2, glass and right mold plate 3, and upper panel 4 and lower panel 5, detachable fixing components are used for shaping. The fixing components include four shaping frames and two elastic bands 13. The shaping frame consists of a main telescopic rod 11, a secondary telescopic rod 14, a right-angle arm 15, and a vacuum suction cup 10. The two right-angle arms 15 are arranged in parallel and connected in the middle by the main telescopic rod 11. Two secondary telescopic rods 14 are symmetrically distributed on both sides of the main telescopic rod 11, and the two ends of the two secondary telescopic rods 14 are respectively connected to the corresponding right-angle arms 15. The ends of the right-angle arms 15 are provided with inward-facing vacuum suction cups 10. The outer wall of the fixing rod 7 of the main telescopic rod 11 is provided with a guide groove block 12 that cooperates with the elastic band 13.

[0033] Both the main telescopic rod 11 and the auxiliary telescopic rod 14 consist of a movable rod 8 with a fixed rod 7 slidingly connected to each end. Permanent magnets 9 are provided at the ends of both ends of the movable rod 8 and at the bottom of the grooves of the fixed rods 7. These permanent magnets 9 are unipolar magnets made using a Hellbeck array, and adjacent permanent magnets 9 on the same central axis of the movable rod 8 repel each other. This ensures that during the extension and retraction of the main telescopic rod 11 and the auxiliary telescopic rod 14, the length of the fixed rods 7 at both ends of the movable rod 8 is the same, thus ensuring that the left mold plate 2 can be pressed down parallel to the glass (or the right mold plate 3 can be pressed down parallel to the glass) (or the upper panel 4 can be pressed down parallel to the lower panel 5).

[0034] The elastic band 13 is internally embedded with a full-length temperature memory alloy wire. When the temperature rises, the full-length temperature memory alloy wire deforms and causes the circumference of the elastic band 13 to shorten. The reason for this design is that the upper panel 4 (or lower panel 5) (or photovoltaic module 1) needs to undergo high temperature and vacuum during the lamination process. In a vacuum environment, the vacuum suction cup 10 will fail. Therefore, in order to ensure that the fixing component can still play a shaping role, the elastic band 13 needs to be able to shrink in a high-temperature environment, so that the fixing component can continue to play a shaping role for the upper panel 4 (or lower panel 5) (or photovoltaic module 1).

[0035] In summary, the function of the fixing components is to prevent the workpiece from shifting during the lamination process.

[0036] The specific application steps of the fixed component in S2 and S5 are as follows: In S2, when the glass and the left mold plate 2 are stacked, a first robotic arm extends from each of the four top corners of the glass. Each first robotic arm holds a shaping frame. The first robotic arm holds the shaping frame close to the glass, so that the two vacuum suction cups 10 at the lower end of the shaping frame are respectively attached to the two adjacent side walls of the glass, and the two vacuum suction cups 10 at the upper end of the shaping frame are respectively attached to the two adjacent side walls of the left mold plate 2. Then the first robotic arm retracts, and then a second robotic arm extends from the top of the glass. The second robotic arm opens the elastic band 13 and puts it on the guide groove block 12. Then the second robotic arm retracts.

[0037] In S2, when the glass and the right mold plate 3 are stacked, a first robotic arm extends from each of the four top corners of the glass. Each first robotic arm holds a shaping frame. The first robotic arm holds the shaping frame close to the glass, so that the two vacuum suction cups 10 at the lower end of the shaping frame are respectively attached to the two adjacent side walls of the glass, and the two vacuum suction cups 10 at the upper end of the shaping frame are respectively attached to the two adjacent side walls of the right mold plate 3. Then the first robotic arm retracts, and then a second robotic arm extends from the top of the glass. The second robotic arm opens the elastic band 13 and puts it on the guide groove block 12. Then the second robotic arm retracts.

[0038] In S5, when the upper panel 4 and the lower panel 5 are stacked, a first robotic arm extends from each of the four corners of the lower panel 5. Each first robotic arm holds a shaping frame. The first robotic arm holds the shaping frame close to the lower panel 5, so that the two vacuum suction cups 10 at the lower end of the shaping frame are respectively attached to the two adjacent side walls of the lower panel 5, and the two vacuum suction cups 10 at the upper end of the shaping frame are respectively attached to the two adjacent side walls of the upper panel 4. Then the first robotic arm retracts. Then the second robotic arm extends from the top of the lower panel 5. The second robotic arm opens the elastic band 13 and puts it on the guide groove block 12. Then the second robotic arm retracts.

[0039] It is worth noting that: Electrode plates and electromagnets are also installed in the cavities of the left pre-laminator, right pre-laminator, and rear laminator. The electrode plates and electromagnets can generate uniform electric fields and uniform magnetic fields in six directions along the positive and negative X, Y, and Z axes in the cavity. At the same time, the directions of the uniform electric field and the uniform magnetic field are perpendicular, and at the same time, the uniform electric field and the uniform magnetic field have only one direction. The uniform electric field and the uniform magnetic field change direction every 0.02 to 5 seconds.

[0040] The process of manufacturing the upper panel 4 using the left pre-lamination press is as follows: Step 1: First, the left pre-lamination machine closes the cavity and evacuates the vacuum. Then, the internal temperature is raised to 135-145°C. Next, the upper chamber is filled with gas and pressurized to perform a first lamination and encapsulation of the glass and EVA film. Then, the lower chamber is evacuated, and then the upper chamber is evacuated until the silicone plate is reset.

[0041] Step 2: First, the left pre-lamination press is directly evacuated. Then, the upper chamber is filled with gas and pressurized to perform secondary lamination and encapsulation of the glass and EVA film. Then, the lower chamber is evacuated. Then, the upper chamber is evacuated to reset the silicone plate. After filling with gas, the cover is opened. Finally, the upper panel 4 is removed from the left pre-lamination press and cooled to room temperature.

[0042] The process of manufacturing the upper panel 4 using the right pre-lamination press is as follows: Step 3: First, the right pre-lamination machine closes the cavity and evacuates the vacuum. Then, the internal temperature is raised to 135-145°C. Then, the upper chamber is filled with gas and pressurized to perform a first lamination and encapsulation of the glass and EVA film. Then, the lower chamber is evacuated, and then the upper chamber is evacuated until the silicone plate is reset.

[0043] Step 4: First, the right pre-lamination press is directly evacuated. Then, the upper chamber is filled with gas and pressurized to perform secondary lamination and sealing of the glass and EVA film. Then, the lower chamber is evacuated. Then, the upper chamber is evacuated to reset the silicone plate. After filling with gas, the cover is opened. Finally, the lower panel 5 is removed from the right pre-lamination press and cooled to room temperature.

[0044] The process of manufacturing photovoltaic module 1 using a post-lamination press is as follows: Step 5: First, the laminator closes the cavity and evacuates the vacuum. Then, the internal temperature is raised to 135-145°C. Then, the upper chamber is filled with gas and pressurized to perform a lamination and sealing of the upper panel 4 and the lower panel 5. Then, the lower chamber is evacuated, and then the upper chamber is evacuated until the silicone plate is reset.

[0045] Step 6: First, the rear laminator is directly evacuated. Then, the upper chamber is filled with gas and pressurized to perform secondary lamination and encapsulation of the upper panel 4 and the lower panel 5. Then, the lower chamber is evacuated. Then, the upper chamber is evacuated to reset the silicone plate. After filling with gas, the cover is opened. Finally, the photovoltaic module 1 is removed from the left pre-laminator and cooled to room temperature.

[0046] In summary: During the primary lamination encapsulation processes in Steps 1, 3, and 5, and the secondary lamination encapsulation processes in Steps 2, 4, and 6, a uniform electric field attracts and rearranges the ethylene and vinyl acetate copolymer molecules in the molten EVA film, thereby increasing the macromolecular structure aligned along the electric field direction. Simultaneously, the polar molecules in the molten EVA film are also subjected to a uniform magnetic field during their movement, causing them to change direction. This reduces or even eliminates the irregular cross-linked network structure of the ethylene and vinyl acetate copolymer molecules in the EVA film, resulting in a uniform distribution and regular shape of polar molecules in space. Consequently, there is sufficient and uniform contact and consistent adhesion between the EVA film and the glass, between EVA films, and between the EVA film and the battery cell assembly 6.

[0047] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any other way. Any person skilled in the art may make changes or modifications to the above-disclosed technical content to create equivalent embodiments for application in other fields. However, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the protection scope of the present invention.

Claims

1. A method for densifying EVA lamination in photovoltaic modules, characterized in that: Includes the following steps: S1, Clean the glass surface and then inspect for defects; S2, divide the glass into two parts. One part of the glass is covered with EVA film and left mold plate (2) on its inner side in sequence. The other part of the glass is covered with EVA film and right mold plate (3) on its inner side in sequence. Then, the two parts of the glass are placed into the left pre-lamination machine and the right pre-lamination machine for pre-treatment. The left pre-lamination machine and the right pre-lamination machine bond the glass and EVA film together to form the upper panel (4) and the lower panel (5). S3, remove the burrs from the edges of the upper panel (4) and the lower panel (5), and then perform defect detection on the upper panel (4) and the lower panel (5); S4, the solar cells and the busbar are connected by welding to form a cell pack (6), then the surface of the cell pack (6) is cleaned, and then the cell pack (6) is inspected for defects; S5, remove the left mold plate (2) on the upper panel (4) and the right mold plate (3) on the lower panel (5), then the upper panel (4) and the lower panel (5) clamp the battery cell group (6) and place it in the rear laminator for lamination, thereby bonding the upper panel (4), the battery cell group (6) and the lower panel (5) together to form a photovoltaic module (1). S6, remove the burrs on the edge of the photovoltaic module (1), and then perform performance testing on the photovoltaic module (1); The cavities of the left pre-laminator, right pre-laminator, and rear laminator are also equipped with electrode plates and electromagnets. The electrode plates and electromagnets can generate uniform electric fields and uniform magnetic fields in six directions along the X, Y, and Z axes. At the same time, the directions of the uniform electric field and the uniform magnetic field are perpendicular to each other, and at the same time, the uniform electric field and the uniform magnetic field each have only one direction. Furthermore, the directions of the uniform electric field and the uniform magnetic field change with time. During the pretreatment in S2 and the lamination process in S5, the uniform electric field attracts and rearranges the ethylene and vinyl acetate copolymer molecules in the molten EVA film, thereby increasing the macromolecular structure aligned along the electric field direction. At the same time, the polar molecules in the molten EVA film are also affected by the uniform magnetic field during their movement and change direction, thereby reducing or even eliminating the network irregular cross-linked structure of the ethylene and vinyl acetate copolymer molecules in the EVA film.

2. The method for densifying EVA lamination in photovoltaic modules according to claim 1, characterized in that, All processes S1 to S6 are completed in a fully automated workshop with constant temperature, humidity and dust-free environment.

3. The method for densifying EVA lamination in photovoltaic modules according to claim 1, characterized in that, In S1 and S4, the glass and battery cell assembly (6) are cleaned by dry ice cleaning, and a negative pressure suction device is used simultaneously to remove impurities and debris during the dry ice cleaning process.

4. The method for densifying EVA lamination in photovoltaic modules according to claim 1, characterized in that, In S1, S3 and S4, the defect detection is performed using machine vision technology.

5. The method for densifying EVA lamination in photovoltaic modules according to claim 1, characterized in that, In S2, the inner surfaces of the left mold plate (2) and the right mold plate (3) are coated with a non-stick layer, and the embossed shapes of the left mold plate (2) and the right mold plate (3) are the same as the shapes of the top and bottom of the battery cell assembly (6) in S4.

6. The method for densifying EVA lamination in photovoltaic modules according to claim 1, characterized in that, In S2 and S5, during the stacking of glass and left mold plate (2), glass and right mold plate (3), and upper panel (4) and lower panel (5), a detachable fixing component is used to fix the shape. The fixing component includes four fixing frames and two elastic bands (13). The fixing frame is composed of a main telescopic rod (11), a secondary telescopic rod (14), a right-angle arm (15), and a vacuum suction cup (10). The two right-angle arms (15) are arranged in parallel and connected in the middle by the main telescopic rod (11). Two secondary telescopic rods (14) are symmetrically distributed on both sides of the main telescopic rod (11), and the two ends of the two secondary telescopic rods (14) are respectively connected to the corresponding right-angle arms (15). The ends of the right-angle arms (15) are provided with inward-facing vacuum suction cups (10). The outer wall of the fixing rod (7) of the main telescopic rod (11) is provided with a guide groove block (12) that cooperates with the elastic band (13). In S2, when the glass and the left mold plate (2) are stacked, a first robotic arm extends from each of the four top corners of the glass. Each first robotic arm holds a shaping frame. The first robotic arm holds the shaping frame close to the glass, so that the two vacuum suction cups (10) at the lower end of the shaping frame are respectively attached to the two adjacent side walls of the glass, and the two vacuum suction cups (10) at the upper end of the shaping frame are respectively attached to the two adjacent side walls of the left mold plate (2). Then the first robotic arm retracts, and then a second robotic arm extends from the top of the glass. The second robotic arm opens the elastic band (13) and puts it on the guide groove block (12). Then the second robotic arm retracts. In S2, when the glass and the right mold plate (3) are stacked, a first robotic arm extends from each of the four top corners of the glass. Each first robotic arm holds a shaping frame. The first robotic arm holds the shaping frame close to the glass, so that the two vacuum suction cups (10) at the lower end of the shaping frame are respectively attached to the two adjacent side walls of the glass, and the two vacuum suction cups (10) at the upper end of the shaping frame are respectively attached to the two adjacent side walls of the right mold plate (3). Then the first robotic arm retracts, and then a second robotic arm extends from the top of the glass. The second robotic arm opens the elastic band (13) and puts it on the guide groove block (12). Then the second robotic arm retracts. In S5, when the upper panel (4) and the lower panel (5) are stacked, a first robotic arm extends from each of the four corners of the lower panel (5). Each first robotic arm holds a shaping frame. The first robotic arm holds the shaping frame close to the lower panel (5), so that the two vacuum suction cups (10) at the lower end of the shaping frame are respectively attached to the two adjacent side walls of the lower panel (5), and the two vacuum suction cups (10) at the upper end of the shaping frame are respectively attached to the two adjacent side walls of the upper panel (4). Then the first robotic arm retracts, and then a second robotic arm extends from the top of the lower panel (5). The second robotic arm opens the elastic band (13) and puts it on the guide groove block (12). Then the second robotic arm retracts.

7. The method for densifying EVA lamination in photovoltaic modules according to claim 6, characterized in that, The main telescopic rod (11) and the auxiliary telescopic rod (14) are both composed of a movable rod (8) with a fixed rod (7) sliding at both ends. The ends of the movable rod (8) and the bottom of the groove of the fixed rod (7) are provided with permanent magnets (9). The permanent magnets (9) are all unipolar magnets made of Heilbeck array. Two adjacent permanent magnets (9) on the same movable rod (8) repel each other. The elastic band (13) is embedded with a full-length temperature memory alloy wire. When the temperature rises, the full-length temperature memory alloy wire will deform and drive the circumference of the elastic band (13) to shorten.

8. The method for densifying EVA lamination in photovoltaic modules according to claim 1, characterized in that, The process of manufacturing the upper panel (4) by the left pre-lamination machine is as follows: Step 1, the left pre-lamination machine closes the cavity and evacuates the vacuum, then the internal temperature is raised to 135-145 ℃, then the upper chamber is filled with gas and pressurized to perform a first lamination and encapsulation of the glass and EVA film, then the lower chamber is evacuated, and then the upper chamber is evacuated until the silicone plate is reset; Step 2, the left pre-lamination machine is directly evacuated, then the upper chamber is filled with gas and pressurized to perform a second lamination and encapsulation of the glass and EVA film, then the lower chamber is evacuated, and then the upper chamber is evacuated to reset the silicone plate. After filling with gas, the cover is opened, and finally the upper panel (4) is removed from the left pre-lamination machine and cooled to room temperature; The process of manufacturing the upper panel (4) by the right pre-lamination machine is as follows: Step 3, firstly, the right pre-lamination machine closes the cavity and evacuates the vacuum, then the internal temperature is raised to 135-145 ℃, then the upper chamber is filled with gas and pressurized to perform a first lamination and encapsulation of the glass and EVA film, then the lower chamber is evacuated, and then the upper chamber is evacuated until the silicone plate is reset; Step 4, firstly, the right pre-lamination machine directly evacuates the vacuum, then the upper chamber is filled with gas and pressurized to perform a second lamination and encapsulation of the glass and EVA film, then the lower chamber is evacuated, and then the upper chamber is evacuated to reset the silicone plate. After filling with gas, the cover is opened, and finally the lower panel (5) is removed from the right pre-lamination machine and cooled to room temperature; The process of manufacturing photovoltaic module (1) by the post-lamination press is as follows: Step 5, firstly, the post-lamination press closes the cavity and evacuates the vacuum, then the internal temperature is raised to 135-145 ℃, then the upper chamber is filled with gas and pressurized to perform a first lamination and encapsulation of the upper panel (4) and the lower panel (5), then the lower chamber is evacuated, and then the upper chamber is evacuated until the silicone plate is reset; Step 6, firstly, the post-lamination press directly evacuates the vacuum, then the upper chamber is filled with gas and pressurized to perform a second lamination and encapsulation of the upper panel (4) and the lower panel (5), then the lower chamber is evacuated, and then the upper chamber is evacuated to reset the silicone plate. After filling with gas, the cover is opened, and finally the photovoltaic module (1) is removed from the left pre-lamination press and cooled to room temperature.

9. A method for densifying EVA lamination in photovoltaic modules according to claim 8, characterized in that, The uniform electric field and uniform magnetic field change direction every 0.02 to 5 seconds.

Citation Information

Patent Citations

  • Photovoltaic component laminating technology

    CN108269882A

  • Segmented laminating method for solar module and laminating machine

    CN114864718A

  • Photovoltaic module laminating method

    CN114883436A