A slow-release anti-mud polycarboxylate water-reducing agent and preparation method thereof
By introducing sustained release polymerizable monomers and functional monomers into polycarboxylic acid water reducing agents, the problems of low water reduction rate and short flow in machined sand and inferior sand gravel are solved, and wettability and mud resistance are achieved The improvement is suitable for special construction applications.
Patent Information
- Application Number
- CN202211461013.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-17
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-11-17
AI Technical Summary
When using machined sand and inferior sand, existing polycarboxylic acid water reducing agents have problems such as low water reduction rate, short mobility maintenance time, and poor adaptability. The synthesis process of small molecule organic phosphine is complex and has a large environmental pollution.
Using aqueous solution free radical polymerization method, polyether macromonomer, acrylic acid, functional monomer allyloxy-3-(4-nonylphenol)-2-propanol polyoxyethylene phosphate monoester and sustained release monomer Propyrimie acid ester and other raw materials are synthesized to form a sustained-release anti-sludge polycarboxylic acid water reducing agent. By introducing sustained-release polymerizable monomers and functional monomers, the wetting and mud resistance of the water reducing agent are improved.
It has achieved significant wetting, gas induction and water reduction rate for machined sand and inferior sand and gravel, extended the concrete flow time, improved the working performance of concrete, and was suitable for the long term of machined sand, inferior sand and gravel and concrete. Distance transport and special construction applications.
Smart Images

Figure BDA0003955376970000061
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of water reducing agents for construction engineering materials, and in particular to a slow-release anti-mud polycarboxylic acid water reducing agent and a preparation method thereof. Background Art
[0002] With the continuous reduction of high-quality sand and gravel resources, the mud content of inferior sand and gravel has become an uncertain factor affecting the performance of concrete. Anti-mud agents have emerged in concrete construction. Anti-mud agents or anti-mud components can improve the working performance of concrete and are of great significance. However, with the continuous consumption of high-quality sand and gravel resources in my country, the use of machine-made sand is an inevitable trend. Machine-made sand is made by mechanical crushing of rocks. Due to the sharp edges and corners on the surface, large amount of fine powder, poor surface wettability and other problems, water reducers, especially polycarboxylate water reducers, have always had problems such as large losses and poor adaptability, resulting in low water reduction rate and insufficient slump retention performance.
[0003] Document CN111518243A discloses a mud-resistant polycarboxylic acid water-reducing agent prepared from organic phosphorus, organic phosphorus polyoxyethylene ether glycerol phosphate, diethylene triamine pentamethylene phosphonic acid, etc. Such small molecule organic phosphorus is easily lost and harmful to the environment, and the fluidity retention time is short. CN109553729A discloses an amphoteric mud-resistant water-reducing agent, which is made of polyetheramine monomer and phosphonate polyether monomer. The synthesis process is complicated, especially the synthesis and polymerization monomer yield of small molecule organic phosphorus is low, resulting in the presence of small molecule organic phosphorus being retained in concrete in the later stage, causing environmental pollution with rainwater erosion, and the fluidity retention time is short. At present, the problems of short fluidity retention time, large loss and poor adaptability of concrete such as machine-made sand and inferior sand (such as beach sand containing organic impurities, etc.) have not been well solved. Summary of the invention
[0004] In order to overcome the deficiencies of the above-mentioned prior art, the object of the present invention is to provide a slow-release anti-mud polycarboxylic acid water-reducing agent and a preparation method thereof, wherein a new reactive multifunctional monomer and a slow-release polymerizable monomer are introduced into the synthesis of the water-reducing agent to synthesize a slow-release anti-mud water-reducing agent, which has the characteristics of good wettability, high water reduction rate, early strength, good mud resistance, etc., and can improve the wettability of the water-reducing agent to sand and cement, air entrainment, and change the working performance of concrete, etc.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A slow-release anti-mud polycarboxylic acid water reducer, using aqueous solution free radical polymerization, the raw material ratio is:
[0007] Polyether macromonomer, 200 parts by weight;
[0008] Acrylic acid (AA), 15.0 to 30.0 parts by weight;
[0009] Functional monomer: allyloxy-3-(4-nonylphenol)-2-propanol polyoxyethylene (10) phosphate monoester (ANPEO10-P1), 5.0 to 10.0 parts by weight;
[0010] Sustained-release monomer: allyl Michaelisate, 10.0 to 20.0 parts by weight;
[0011] Distilled water: total mass parts is 300 parts;
[0012] Initiator: 10 to 15 parts by weight of persulfate and 10 to 15 parts by weight of sodium hypophosphite.
[0013] The reaction temperature is controlled at: 45~65℃.
[0014] The polyether macromonomer is one of isopentanol polyoxyethylene ether (TPEG-2400), vinyl butanediol polyoxyethylene ether (EPEG-3000) or methyl allyl polyoxyethylene ether (HPEG-2400).
[0015] A method for preparing a slow-release anti-mud polycarboxylate water-reducing agent comprises the following steps:
[0016] (1) Add 200 parts by weight of a polyether macromonomer and 200 parts by weight of distilled water into a stirred reaction vessel, stir thoroughly for 10 minutes, then continue to add persulfate, stir and control the reaction temperature;
[0017] (2) In 50 parts of distilled water, add the formulated amount of acrylic acid (AA), ANPEO10-P1 and allyl Michaelisate in sequence, mix and stir to emulsify, and together form the dropwise component I; in another 50 parts of distilled water, add the formulated amount of initiator sodium hypophosphite, and dissolve to form the dropwise component II;
[0018] (3) simultaneously adding the component I and the component II in the step (2) to the reaction container in the step (1) to react, and keeping the mixture warm after the reaction is completed, and cooling the mixture to room temperature to obtain an anti-mud multifunctional polycarboxylate water-reducing agent;
[0019] (4) The pH value is adjusted to between 6 and 7 using triethanolamine to obtain a slow-release anti-mud water-reducing agent.
[0020] In the steps (1) and (3), the temperature is raised to 45-65° C., the dropwise addition time is 2-3 hours, and the temperature is kept for 2-3 hours after the reaction is completed.
[0021] The polyether macromonomer is one of isopentanol polyoxyethylene ether (TPEG-2400), vinyl butanediol polyoxyethylene ether (EPEG-3000) or methyl allyl polyoxyethylene ether (HPEG-2400).
[0022] The slow-release anti-mud water-reducing agent is used for long-distance transportation of machine-made sand, inferior sand and gravel, and concrete, and for the construction of super-high-rise buildings and long tunnels.
[0023] Beneficial effects of the present invention:
[0024] The slow-release anti-mud water-reducing agent of the present invention has the advantages of good wettability, good air entrainment, high water reduction rate, good mud resistance, etc. on mud-containing sand, especially machine-made sand, while maintaining good water-reducing performance. It can overcome the defects of the current common polycarboxylic acid water-reducing agent, such as poor adaptability to machine-made sand and soil sensitivity.
[0025] The slow-release anti-mud water-reducing agent has a simple preparation process. The functional monomer plays its role in wetting, anti-mud, and regulating air content. At the same time, it promotes the uniform dispersion of the slow-release monomer and polyether, which can maintain the fluidity of concrete for 2-3 hours, overcome the adverse effects of inferior sand and gravel on concrete, and greatly improve the working performance of concrete. It is suitable for special applications such as long-distance transportation of machine-made sand, inferior sand and gravel, and concrete, super high-rise buildings, and long tunnel construction.
[0026] The slow-release anti-mud water-reducing agent molecules simultaneously introduce a cyclic ether group with a slowly released carboxyl group, an anti-mud phosphonate group, and a wetting group of nonylphenol ether. The allyl Michaelisate monomer contains a cyclic ester formed by two carboxyl groups, which will slowly hydrolyze and gradually release the two carboxyl groups when encountering the alkaline environment of cement, thereby enhancing the adsorption and anchoring with the cement surface and prolonging the cement flow time; the functional monomer allyloxy-3-(4-nonylphenol)-2-propanol polyoxyethylene (10) phosphate monoester (ANPEO10-P1) surface active monomer has an anti-mud phosphate group and a nonylphenol group with a strong wettability of a polyether long chain, which has a strong wettability to the surface of sand and gravel, and promotes the water-reducing agent molecules to be evenly dispersed on the surface of sand and gravel and cement particles. At the same time, the monomer also has a certain air entraining function, which promotes the uniformity of concrete microbubbles and the smoothness of the concrete macroscopic surface. DETAILED DESCRIPTION
[0027] The present invention is further described in detail below in conjunction with embodiments.
[0028] Example 1
[0029] Add 200g EPEG-3000 to a reaction container equipped with a stirrer, add 200mL distilled water, stir to dissolve, then dissolve 10g sodium persulfate, control the temperature to 65°C, and start to drop component I (5g ANPEO10-P1, 10g allyl Michaelisate and 15g acrylic acid are added to 50mL distilled water and stirred to emulsify and disperse evenly) and component II (10g sodium hypophosphite is dissolved in 50mL distilled water and stirred evenly) at the same time; the dropping time is 2h, and the heat preservation reaction is continued for 2h. After the reactant is cooled to room temperature, the pH value is adjusted to between 6 and 7 with triethanolamine to obtain a slow-release anti-mud water-reducing agent.
[0030] Example 2
[0031] Add 200g EPEG-3000 to a reaction container equipped with a stirrer, add 200mL distilled water, stir to dissolve, then dissolve 15g ammonium persulfate, wait until the temperature rises to 55°C, start to simultaneously add component I (10g ANPEO10-P1, 20g allyl Michaelisate and 30g acrylic acid are added to 50mL distilled water and stirred evenly) and component II (25g sodium hypophosphite is dissolved in 50mL distilled water and stirred evenly); the addition time is 3h, and the heat preservation reaction is continued for 3h. After the reactant is cooled to room temperature, the pH value is adjusted to between 6 and 7 with triethanolamine to obtain a slow-release anti-mud water-reducing agent.
[0032] Example 3
[0033] 200 mL of distilled water and 200 g of TPEG-2400 were added to a reaction container equipped with a stirrer in sequence and stirred to dissolve, and then 12 g of potassium persulfate was added, and the stirring was continued and the temperature was raised to 45° C. Component I (13 g of ANPEO10-P1, 15 g of allyl Michaelisate and 25 g of acrylic acid were added to 50 mL of distilled water and stirred evenly) and component II (12 g of sodium hypophosphite was dissolved in 50 mL of distilled water and stirred evenly) were added dropwise at the same time; the addition time was 2.5 h, and the reaction was continued at 45° C. for 1.5 h. After the reactant was cooled to room temperature, the pH value was adjusted to between 6 and 7 with triethanolamine to obtain a slow-release anti-mud water-reducing agent.
[0034] Example 4
[0035] In a reaction container equipped with a stirrer, 200 mL of distilled water and 200 g of HPEG-2400 were added in sequence and stirred to dissolve, and then 10 g of potassium persulfate was added, stirring was continued and the temperature was raised to 50° C., and component I (10 g of ANPEO10-P1, 15 g of allyl Michaelisate and 25 g of acrylic acid were added to 50 mL of distilled water and stirred for emulsification) and component II (12 g of sodium hypophosphite was dissolved in 50 mL of distilled water and stirred evenly) were added dropwise at the same time; the addition time was 2.5 h, and the reaction was kept at 50° C. for 2.5 h. After the reactant was cooled to room temperature, the pH value was adjusted to between 6 and 7 with triethanolamine to obtain a slow-release anti-mud water-reducing agent.
[0036] Example 5
[0037] In a reaction container equipped with a stirrer, 200 mL of distilled water and 200 g of TPEG-2400 were added in sequence and stirred to dissolve, and then 15 g of potassium persulfate was added, and stirring was continued and the temperature was raised to 45° C. Component I (13 g of ANPEO10-P1, 15 g of allyl Michaelisate and 23 g of acrylic acid were added to 20 mL of distilled water and stirred for emulsification) and component II (15 g of sodium hypophosphite was dissolved in 50 mL of distilled water and stirred evenly) were added dropwise at the same time; the addition time was 2.5 h, and the reaction was kept warm at 45° C. for 1.5 h. After the reactant was cooled to room temperature, the pH value was adjusted to between 6 and 7 with triethanolamine to obtain a slow-release anti-mud water-reducing agent.
[0038] Comparative Example:
[0039] Add 200g of isopentanol polyoxyethylene ether TPEG-2400 to a reaction container equipped with a stirrer, add 200mL of distilled water, stir to dissolve, then add 25g of hydrogen peroxide, control the temperature to 25°C, and start to drop component 1 (22g of acrylic acid and 5g of sodium allyl sulfonate dissolved in 50mL of distilled water in sequence and stirred evenly) and component 2 (12g of initiator Vc dissolved in 50mL of distilled water and stirred evenly) at the same time; the dropping time is 2h, and the heat preservation reaction is continued for 3h. After the reactant is cooled to room temperature, the pH value is adjusted to between 6 and 7 with sodium hydroxide to obtain a market-general polycarboxylate water reducer.
[0040] Comparison of performance test results of the embodiments:
[0041] According to GB / T8077-2000 and JGJ 70-2009 standards, relevant tests were carried out, using Yaobai 42.5 cement, 1.8% water reducer, and standard machine-made sand. The test results of the mortar are as follows:
[0042]
[0043] The test results show that the mortar specimens with the water-reducing agent after adding the anti-mud and slow-release functional monomers have uniform bubbles, good fluidity in 1 hour, the maximum fluidity in 120 hours, and even good fluidity in 3 hours. It has strong adaptability to inferior sand and soil, and has good slow-release and anti-mud effects. It is particularly suitable for special applications such as long-distance transportation of machine-made sand, inferior sand and gravel, and concrete, super high-rise buildings, and long tunnel construction, and has broad prospects.
Claims
1. A slow-release anti-mud polycarboxylate water reducer, It is characterized in that Using aqueous solution free radical polymerization, the raw material ratio is: Polyether macromonomer, 200 parts by weight; Acrylic acid (AA), 15.0-30.0 parts by weight; Functional monomer: allyloxy-3-(4-nonylphenol)-2-propanol polyoxyethylene (10 ) phosphate monoester (ANPEO10-P1), 5.0-10.0 parts by weight; Sustained-release monomer: allyl Michaelisate, 10.0-20.0 parts by weight; Distilled water: total mass parts is 300 parts; Initiator: 10-15 parts by weight of persulfate and 10-15 parts by weight of sodium hypophosphite; The reaction temperature is controlled at: 45~65℃.
2. A method for preparing a slow-release anti-mud polycarboxylate water-reducing agent according to claim 1, It is characterized in that The steps include: (1) Add 200 parts by weight of polyether macromonomer and 200 parts by weight of distilled water into a stirred reaction vessel, stir thoroughly for 10 minutes, then continue to add persulfate, stir and control the reaction temperature; (2) In 50 parts of distilled water, add the formulated amount of acrylic acid (AA), ANPEO10-P1 and allyl Michaelisate in sequence, mix and stir to emulsify, and together form the dropwise component I; in another 50 parts of distilled water, add the formulated amount of initiator sodium hypophosphite, and dissolve it to form the dropwise component II; (3) simultaneously adding the component I and the component II in the above step (2) to the reaction container in step (1) to react, and keeping the temperature after the reaction is completed and cooling to room temperature to obtain an anti-mud multifunctional polycarboxylate water-reducing agent; (4) The pH value was adjusted to between 6 and 7 using triethanolamine to obtain a slow-release anti-mud water-reducing agent.
3. The method for preparing a slow-release anti-mud polycarboxylate water-reducing agent according to claim 2, It is characterized in that In the steps (1) and (3), the reaction temperature is 45-65° C., the dropwise addition time is 2-3 hours, and the reaction is kept warm for 2-3 hours after the reaction is completed.
4. The method for preparing a slow-release anti-mud polycarboxylate water-reducing agent according to claim 3, It is characterized in that The polyether macromonomer is one of isopentanol polyoxyethylene ether, vinyl butanediol polyoxyethylene ether or methyl allyl polyoxyethylene ether.
5. The slow-release anti-mud polycarboxylate water reducer according to claim 1 or the slow-release anti-mud polycarboxylate water reducer prepared by the method according to any one of claims 2 to 4, It is characterized in that The slow-release anti-mud water-reducing agent is used for long-distance transportation of machine-made sand, inferior sand and gravel, and concrete, and for the construction of super-high-rise buildings and long tunnels.