Anode catalytic electrode for hydrogen production by seawater electrolysis at industrial current density and preparation method and application thereof

By using a metal foam carrier to grow a cobalt-doped nickel sulfide array and covering it with a highly active sulfur protective layer in seawater electrolysis, the activity and stability problems caused by the interference of chlorine anions in seawater electrolysis are solved, and high current density output at low potential is achieved. and stability, suitable for industrial applications.

CN115852427BActive Publication Date: 2024-10-25SHANDONG NORMAL UNIV +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211590787.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-12
Publication Date
2024-10-25
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

The existing anode catalyst for hydrogen production by seawater electrolysis has unsatisfactory activity and stability due to the interference of chlorine anions under alkaline conditions. It is difficult to achieve industrial-grade high current density output at a potential lower than 480mV, and is prone to chlorine evolution side reactions. and corrosion.

Method used

Metal foam is used as a three-dimensional carrier, and a cobalt-doped nickel sulfide array is grown in situ and covered with a highly active sulfur protective layer on its surface to form a multi-level porous nanochannel structure to improve catalytic activity and stability and inhibit the adsorption of chloride ions. .

Benefits of technology

It achieves continuous and stable hydrogen production at ampere-level current density, avoids chlorine evolution side reactions, significantly improves the stability of the anode catalyst and industrial-level current density output, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115852427B_ABST
    Figure CN115852427B_ABST
Patent Text Reader

Abstract

The present invention discloses an anode catalytic electrode for hydrogen production by electrolysis of seawater under industrial-grade current density, and a preparation method and application thereof, which belongs to the field of nanomaterial preparation and clean energy. The anode catalytic electrode uses metal foam as a three-dimensional carrier, and a cobalt-doped nickel sulfide array is in-situ grown on the surface of the three-dimensional carrier, and a layer of highly active sulfur protective layer containing vacancies is covered on the surface of the array. The preparation method of the present invention is simple and easy to operate, low in cost, and can be expanded in batches. The anode catalytic electrode has the characteristics of high intrinsic catalytic activity, high exposed active sites, fast proton and gas mass transfer rates, and inhibition of chloride ion adsorption on the surface. When used as an anode electrode for hydrogen production by electrolysis of seawater, it has industrial-grade current density and stability at a relatively low overpotential (less than 400mV) in alkaline simulated seawater, while avoiding the occurrence of chlorine evolution side reactions, reducing energy consumption, and can be used as an anode electrode for industrial seawater electrolysis hydrogen production equipment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of nano material preparation and clean energy, and specifically relates to an anode catalytic electrode used for producing hydrogen by electrolyzing seawater at an industrial-grade current density, and a preparation method and application thereof. Background Art

[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] Hydrogen (H 2 ) as a sustainable and safe energy source with 142.351MJ kg -1 The high energy density and no pollution emissions are crucial to solving the current urgent environmental crisis and insufficient supply of fossil energy. Hydrogen production by water electrolysis is superior to traditional petrochemical technologies in terms of processing efficiency, renewable energy compatibility, and carbon neutrality in producing high-purity hydrogen. Therefore, hydrogen production by water electrolysis has become an attractive renewable energy storage solution for the future. In addition to the cathode hydrogen evolution half-reaction (HER), hydrogen production by water electrolysis must also include an anode half-reaction, generally the oxygen evolution reaction (OER). However, due to its slow, multi-step proton-coupled electron transfer process, the overall efficiency of hydrogen production by water electrolysis is greatly hindered. Therefore, the development of highly active and stable OER catalytic electrodes is the key to hydrogen production by water electrolysis.

[0004] Another major problem with water electrolysis for hydrogen production is the lack of fresh water resources in nature. Using fresh water as an electrolyte for water electrolysis to produce hydrogen will put heavy pressure on important water resources. The ocean occupies 96.5% of the earth's water reserves, providing unlimited hydrogen resources without causing serious impact on global fresh water resources. It is a promising electrolyte for water electrolysis to produce hydrogen in the future. However, the interference of various metal ions in seawater has led to unsatisfactory activity and stability of OER electrocatalysts for hydrogen production by seawater electrolysis, which has not been able to meet the needs of industrialization. In particular, the chloride anions (Cl - , about 0.5M), will lead to a chlorine evolution side reaction (ClER) at the anode, competing with OER. Although OER has a thermodynamic advantage, its complex four-electron transfer reaction is more kinetically sluggish than the ClER reaction with only two electrons. Under alkaline conditions (pH>7.5), Cl - With OH - Further reaction generates hypochlorite (Cl - +2OH - →ClO - +H 2 O+2e -), maintaining the maximum thermodynamic potential difference with OER (about 480mV), providing a convenient selective potential difference window for OER. In summary, alkaline conditions are conducive to the selective oxidation of seawater, and the OER catalyst can avoid the formation of hypochlorite if it achieves industrial-grade high current density output before 480mV overpotential. In addition, chloride corrosion and poisoning by insoluble precipitates or microorganisms can also impair the stability and service life of electrode materials, which puts higher requirements on the structural stability and corrosion resistance of electrode materials. However, to date, to reduce the polarization overpotential, it is necessary to conduct the reaction at current densities far below the industrial standard (500-1000mA cm -2 ) was electrolyzed (<200 mA cm -2 Therefore, in order to meet the needs of industrial applications, it is necessary to develop a device that can drive high current density (500-1000mA cm) at ultra-low potential (less than 480mV). -2 ) and maintain good stability of OER electrocatalysts is very necessary and challenging. Summary of the invention

[0005] In order to solve the deficiencies of the prior art, the purpose of the present invention is to provide an anode catalytic electrode for hydrogen production by electrolysis of seawater at an industrial-grade current density, and a preparation method and application thereof. The anode catalytic electrode provided by the present invention continuously and stably produces hydrogen at an ampere-level current density without being affected by Cl - The influence of side reactions such as oxidation.

[0006] In order to achieve the above object, the technical solution of the present invention is:

[0007] In the first aspect, an anode catalytic electrode for use in seawater electrolysis to produce hydrogen at an industrial-grade current density is provided, characterized in that the anode catalytic electrode uses metal foam as a three-dimensional carrier, a cobalt-doped nickel sulfide array is in situ grown on the surface of the three-dimensional carrier, and a highly active sulfur protective layer containing vacancies is covered on the surface of the array.

[0008] In a second aspect, a method for preparing the above-mentioned anode catalytic electrode for hydrogen production by seawater electrolysis at an industrial-grade current density is provided, comprising the following steps:

[0009] Step 1: Weigh cobalt salt, nickel salt and urea and dissolve them in deionized water to form a solution;

[0010] Step 2: placing the metal foam in the solution of step 1, and reacting in a closed manner to obtain a cobalt-doped nickel hydroxide precursor;

[0011] Step 3: adding the precursor obtained in step 2 to an aqueous solution containing a sulfur salt, and conducting a closed reaction to obtain a cobalt-doped nickel sulfide precursor;

[0012] Step 4: Add the precursor obtained in step 3 into a hydrogen peroxide solution and react to obtain the product.

[0013] The anode catalytic electrode of the present invention, which is applied to the electrolysis of seawater to produce hydrogen at an industrial-grade current density, can continuously and stably produce hydrogen at an ampere-grade current density without being affected by Cl - The influence of side reactions such as oxidation, therefore, in the third aspect, provides the application of the above-mentioned anode catalytic electrode for hydrogen production by electrolysis of seawater under industrial-grade current density in hydrogen production by electrolysis of seawater.

[0014] The beneficial effects of the present invention are:

[0015] (1) The synthesis of the anode catalytic electrode of the present invention is carried out at a relatively low temperature, which is easy to operate and prepare in batches; and the method is applicable to different three-dimensional substrates, and is a universal method for synthesizing sulfide material arrays, which is suitable for large-scale industrial production.

[0016] (2) The anode catalytic electrode prepared by the present invention has multi-level pore nanochannels, which can quickly promote the transfer and transportation of substances; at the same time, the in-situ grown nanoarray helps to improve the stability of the material catalytic process and the rapid transmission of electrons; the anionic sulfur vacancies easily formed on the surface of the anode catalytic electrode material can adjust the electronic structure of the active site, thereby improving the intrinsic electrocatalytic oxygen evolution activity of the highly uncoordinated cobalt atoms on the surface; the surface sulfur protective layer can inhibit the precipitation of chloride ions on the surface of the material, so that the anode catalytic electrode exhibits excellent stability in simulated seawater. In summary, the anode catalytic electrode of the present invention has high intrinsic catalytic activity, highly exposed active sites, fast proton and gas mass transfer rates, and inhibits the adsorption of chloride ions on the surface.

[0017] (3) The anode catalytic electrode prepared by the present invention exhibits excellent industrial-grade current density before the chlorine evolution potential (480 mV), avoiding the chlorine evolution side reaction and solving the problem of chlorine gas byproduct generation at high current density, thus realizing industrial seawater electrolysis to produce hydrogen. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0019] Figure 1 It is a schematic diagram of the synthesis route for preparing the cobalt-doped nickel sulfide array of the present invention;

[0020] Figure 2 is a field emission scanning electron microscope image of the cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention;

[0021] Figure 3is a field emission scanning electron microscope image of the cobalt-doped nickel sulfide (CoNiS-30) array prepared in Example 2 of the present invention;

[0022] Figure 4 is a field emission scanning electron microscope image of the cobalt-doped nickel sulfide (CoNiS-90) array prepared in Example 3 of the present invention;

[0023] Figure 5 is a field emission scanning electron microscope image of the cobalt-doped nickel sulfide (CoNiS) array prepared in Comparative Example 1 of the present invention;

[0024] Figure 6 is an X-ray diffraction pattern of the cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention;

[0025] Figure 7 The cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention, the cobalt-doped nickel sulfide (CoNiS) array prepared in Comparative Example 1, and the commercial RuO 2 , Linear sweep voltammetry curve of oxygen evolution reaction of NF in 1M KOH electrolyte;

[0026] Figure 8 Linear sweep voltammetry curves of the oxygen evolution reaction of the cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention, the cobalt-doped nickel sulfide (CoNiS) array prepared in Comparative Example 1, the cobalt-doped nickel sulfide (CoNiS-30) array prepared in Example 2, and the cobalt-doped nickel sulfide (CoNiS-90) array prepared in Example 3 in 1M KOH electrolyte;

[0027] Fig. 9 It is commercial NF, RuO 2 , Tafel curves of oxygen evolution reaction of CoNiS and CoNiS-60 in 1M KOH electrolyte;

[0028] Fig.10 The Tafel curves of the oxygen evolution reaction of the cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention, the cobalt-doped nickel sulfide (CoNiS) array prepared in Comparative Example 1, the cobalt-doped nickel sulfide (CoNiS-30) array prepared in Example 2, and the cobalt-doped nickel sulfide (CoNiS-90) array prepared in Example 3 in 1M KOH electrolyte;

[0029] Fig.11 The cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention, the cobalt-doped nickel sulfide (CoNiS) array prepared in Comparative Example 1, and the commercial RuO 2, Linear sweep voltammetry curve of oxygen evolution reaction of NF in 1M KOH+0.5M NaCl (simulated seawater) electrolyte;

[0030] Fig.12 Linear sweep voltammetry curves of oxygen evolution reaction of the cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention, the cobalt-doped nickel sulfide (CoNiS) array prepared in Comparative Example 1, the cobalt-doped nickel sulfide (CoNiS-30) array prepared in Example 2, and the cobalt-doped nickel sulfide (CoNiS-90) array prepared in Example 3 in 1M KOH + 0.5M NaCl (simulated seawater) electrolyte;

[0031] Fig.13 The cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention, the cobalt-doped nickel sulfide (CoNiS) array prepared in Comparative Example 1, and the commercial RuO 2 , Tafel curve of oxygen evolution reaction of NF in 1M KOH+0.5M NaCl (simulated seawater) electrolyte;

[0032] Fig.14 The Tafel curves of the oxygen evolution reaction of the cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention, the cobalt-doped nickel sulfide (CoNiS) array prepared in Comparative Example 1, the cobalt-doped nickel sulfide (CoNiS-30) array prepared in Example 2, and the cobalt-doped nickel sulfide (CoNiS-90) array prepared in Example 3 in 1M KOH + 0.5M NaCl (simulated seawater) electrolyte;

[0033] Fig.15 The cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention, the cobalt-doped nickel sulfide (CoNiS) array prepared in Comparative Example 1, and the commercial RuO 2 , Linear sweep voltammetry curve of oxygen evolution reaction of NF in 1M KOH + seawater (alkaline seawater) electrolyte;

[0034] Fig.16 Linear sweep voltammetric curves of oxygen evolution reaction of the cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention, the cobalt-doped nickel sulfide (CoNiS) array prepared in Comparative Example 1, the cobalt-doped nickel sulfide (CoNiS-30) array prepared in Example 2, and the cobalt-doped nickel sulfide (CoNiS-90) array prepared in Example 3 in 1M KOH + seawater (alkaline seawater) electrolyte;

[0035] Fig.17The cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention, the cobalt-doped nickel sulfide (CoNiS) array prepared in Comparative Example 1, and the commercial RuO 2 , Tafel curve of oxygen evolution reaction of NF in 1M KOH + seawater (alkaline seawater) electrolyte;

[0036] Fig.18 The Tafel curves of the oxygen evolution reaction of the cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention, the cobalt-doped nickel sulfide (CoNiS) array prepared in Comparative Example 1, the cobalt-doped nickel sulfide (CoNiS-30) array prepared in Example 2, and the cobalt-doped nickel sulfide (CoNiS-90) array prepared in Example 3 in 1M KOH + seawater (alkaline seawater) electrolyte;

[0037] Fig.19 The linear sweep voltammetric curves of the oxygen evolution reaction of the cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention in 1M KOH, 1M KOH+0.5M NaCl (simulated seawater) and 1M KOH+seawater (alkaline seawater) electrolytes;

[0038] Fig. 20 It is a Tafel curve of the oxygen evolution reaction of the cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention in 1M KOH, 1M KOH+0.5M NaCl (simulated seawater) and 1M KOH+seawater (alkaline seawater) electrolytes;

[0039] Fig.21 It is a stability curve of the current density of the oxygen evolution reaction of the cobalt-doped nickel sulfide (CoNiS-60) array prepared in Example 1 of the present invention in 1M KOH+seawater (alkaline seawater) electrolyte over time. DETAILED DESCRIPTION

[0040] In view of the current industrial application, it is necessary to develop a device that can drive a large current density (500-1000mA cm) at an ultra-low potential (less than 480mV). -2 ) and maintain good stability of OER electrocatalysts is very necessary. The present invention proposes an anode catalytic electrode for seawater electrolysis to produce hydrogen at an industrial current density and a preparation method and application thereof.

[0041] A typical embodiment of the present invention provides an anode catalytic electrode for use in seawater electrolysis to produce hydrogen at an industrial-grade current density. The anode catalytic electrode uses metal foam as a three-dimensional carrier, a cobalt-doped nickel sulfide array is in situ grown on the surface of the three-dimensional carrier, and a highly active sulfur protective layer containing vacancies is covered on the surface of the array.

[0042] In some examples of this implementation manner, the metal foam includes nickel foam, copper foam, nickel-iron foam, or cobalt foam.

[0043] In some examples of this embodiment, the cobalt content in the cobalt-doped nickel sulfide array and the vacancy-containing high-activity sulfur protective layer is 0%-10%, the nickel content is 40%-50%, the sulfur content is 30%-50%, and the vacancy content accounts for 0%-10% of the sulfur content, in a molar ratio.

[0044] Another typical embodiment of the present invention provides a method for preparing the above-mentioned anode catalytic electrode for hydrogen production by seawater electrolysis at an industrial-grade current density, comprising the following steps:

[0045] Step 1: Weigh cobalt salt, nickel salt and urea and dissolve them in deionized water to form a solution;

[0046] Step 2: placing the metal foam in the solution of step 1, and reacting in a closed manner to obtain a cobalt-doped nickel hydroxide precursor;

[0047] Step 3: adding the precursor obtained in step 2 to an aqueous solution containing a sulfur salt, and conducting a closed reaction to obtain a cobalt-doped nickel sulfide precursor;

[0048] Step 4: Add the precursor obtained in step 3 into a hydrogen peroxide solution and react to obtain the product.

[0049] In some examples of this embodiment, the cobalt salt and the nickel salt are selected from any soluble metal salt.

[0050] Wherein, the molar ratio of cobalt salt: nickel salt is 1:1-50;

[0051] In some examples of this embodiment, in the solution of step 1, the total molar concentration of the metal salt is 50-200 mM.

[0052] Wherein, the molar ratio of urea to metal salt is 1:1-10.

[0053] In some examples of this embodiment, in step 2, the reaction temperature is 100-200° C., and the reaction time is 2-72 h.

[0054] In some examples of this embodiment, in step 3, the reaction temperature is 100-200° C., and the reaction time is 2-72 hours.

[0055] In some examples of this embodiment, the sulfur salt includes sodium sulfide, thioacetamide, thiourea, and sulfur powder.

[0056] In some examples of this embodiment, the molar concentration of the sulfur salt in the aqueous solution containing the sulfur salt is 0.2-1M.

[0057] In some examples of this embodiment, the concentration of the hydrogen peroxide solution is 3%-30% by volume.

[0058] In some examples of this embodiment, the reaction temperature in step 4 is 0-60° C., preferably 25° C.; and the reaction time is 10 s-20 min.

[0059] In some examples of this embodiment, in step 4, after the reaction is completed, the electrode is rinsed with deionized water to obtain a cobalt-doped nickel sulfide electrode having surface vacancies.

[0060] A third typical embodiment of the present invention provides the use of the above-mentioned anode catalytic electrode for hydrogen production by seawater electrolysis at industrial-grade current density in hydrogen production by seawater electrolysis.

[0061] In some examples of this embodiment, the application is that the anode catalytic electrode is used as the anode of an electrocatalytic seawater electrolysis hydrogen production device.

[0062] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.

[0063] Example 1: Preparation method of anode catalytic electrode for hydrogen production by seawater electrolysis at industrial current density

[0064] Step 1: Add nickel nitrate, cobalt nitrate and urea weighed according to the stoichiometric ratio into 40 mL of deionized water and stir to form a mixed solution; the concentration of nickel nitrate in the mixed solution is 150 mM, the concentration of cobalt nitrate is 10 mM, and the concentration of urea is 900 mM;

[0065] Step 2: 3*3cm 2 The foamed metal is placed in the solution prepared in step 1 and reacted in a sealed container at 120° C. for 6 hours;

[0066] Step 3: Add the metal foam obtained in step 2 into 40 mL of 625 mM sodium sulfide aqueous solution and react in a sealed container at 120° C. for 8 h;

[0067] Step 4: Add the metal foam obtained in step 3 to 20 mL of 30% hydrogen peroxide solution at 25° C., let it react for 60 seconds, then rinse with deionized water to obtain a CoNiS-60 anode catalytic electrode.

[0068] The field emission scanning electron microscopy image of the obtained CoNiS-60 anode catalytic electrode is shown in Figure 2As shown, the morphology of the catalytic electrode is a multi-level array structure formed by the ordered arrangement of nanorods wrapped by nanosheet arrays. The multi-level array structure is conducive to the transfer of charges and the diffusion of gases, while the two-dimensional nanosheets can expose more active areas. The strong adhesion between the nanosheets and nanorods helps to improve the activity and stability of the catalyst.

[0069] X-ray diffraction pattern Figure 6 As shown, it has good crystallinity, and the comparison with the PDF card proves that its single Ni 3 S 2 Mutually.

[0070] The linear sweep voltammetric curve of oxygen evolution in 1M KOH electrolyte is as follows Figure 7 As shown, at 500 and 1000 mA cm -2 The overpotentials of RuO 2 The Tafel curve of oxygen evolution in 1M KOH electrolyte is as follows Fig. 9 As shown, the Tafel slope of CoNiS-60 is only 113 mV dec. -1 , much lower than commercial RuO 2 (208mVdec -1 ).

[0071] The linear sweep voltammetric curve of oxygen evolution in 1M KOH+0.5M NaCl (simulated seawater) electrolyte is as follows Fig.11 As shown, at 500 and 1000 mA cm -2 The overpotentials of RuO 2 The Tafel curve of oxygen evolution in 1M KOH + 0.5M NaCl (simulated seawater) electrolyte is as follows: Fig.13 As shown, the Tafel slope of CoNiS-60 is only 108 mV dec. -1 , much lower than commercial RuO 2 (225mV dec -1 ).

[0072] The linear sweep voltammetric curve of oxygen evolution in 1M KOH + seawater (alkaline seawater) electrolyte is as follows Fig.15 As shown, at 500 and 1000 mA cm -2 The overpotentials of commercial RuO 2 At an overpotential of 700 mV, the current still did not reach 500 mA cm -2 The Tafel curve of oxygen evolution in 1M KOH + seawater (alkaline seawater) electrolyte is as follows Fig.17As shown, the Tafel slope of CoNiS-60 is only 120mV dec -1 , much lower than commercial RuO 2 (310mV dec -1 ), indicating that CoNiS-60 has excellent oxygen evolution kinetics.

[0073] Furthermore, the oxygen evolution performance of CoNiS-60 in 1M KOH, 1M KOH+0.5M NaCl (simulated seawater) and 1M KOH+seawater (alkaline seawater) was comprehensively compared. Fig.19 As shown in the figure, the performance of CoNiS-60 in 1M KOH+0.5M NaCl (simulated seawater) is better than that in 1M KOH, and further better than that in 1MKOH+seawater (alkaline seawater). However, overall, there is little difference between the three, indicating that CoNiS-60 can resist Cl - Such as Fig. 20 As shown, the Tafel slopes in 1M KOH, 1M KOH + 0.5M NaCl (simulated seawater) and 1M KOH + seawater (alkaline seawater) are 113 mV dec, respectively. -1 , 108mV dec -1 and 120mV dec -1 , with a small kinetic difference. There was no obvious decrease in current density after running in 1M KOH + seawater (alkaline seawater) for 100h, indicating that CoNiS-60 has excellent stability in oxygen separation in seawater.

[0074] Example 2: Preparation method of anode catalytic electrode for hydrogen production by seawater electrolysis at industrial current density

[0075] Step 1: Add nickel nitrate, cobalt nitrate and urea weighed according to the stoichiometric ratio into 40 mL of deionized water and stir to form a mixed solution; the concentration of nickel nitrate in the mixed solution is 150 mM, the concentration of cobalt nitrate is 10 mM, and the concentration of urea is 900 mM;

[0076] Step 2: 3*3cm 2 The foamed metal is placed in the solution prepared in step 1 and reacted in a sealed container at 120° C. for 6 hours;

[0077] Step 3: Add the metal foam obtained in step 2 into 40 mL of 625 mM sodium sulfide aqueous solution and react in a sealed container at 120° C. for 8 h;

[0078] Step 4: Add the metal foam obtained in step 3 to 20 mL of 30% hydrogen peroxide solution at 25° C., let it react for 30 seconds, and then rinse it with deionized water to obtain a CoNiS-30 anode catalytic electrode.

[0079] The field emission scanning electron microscopy image of the obtained CoNiS-30 anode catalytic electrode is shown in Figure 3 As shown, the morphology of the catalytic electrode is a multi-level array structure formed by ordered nanorods wrapped in nanosheet arrays.

[0080] The linear sweep voltammetric curve of oxygen evolution in 1M KOH electrolyte is as follows Figure 8 As shown, at 500 and 1000mAcm -2 The overpotentials are 372mV and 454mV respectively. The Tafel curve of oxygen evolution in 1M KOH electrolyte is as follows Fig.10 As shown, the Tafel slope of CoNiS-30 is 132 mV dec -1 , lower than commercial RuO 2 (208mV dec -1 ).

[0081] The linear sweep voltammetric curve of oxygen evolution in 1M KOH+0.5M NaCl (simulated seawater) electrolyte is as follows Fig.12 As shown, at 500 and 1000mAcm -2 The overpotentials are 325mV and 359mV respectively. The Tafel curve of oxygen evolution in 1M KOH + 0.5M NaCl (simulated seawater) electrolyte is as follows Fig.14 As shown, the Tafel slope of CoNiS-30 is only 114 mV dec. -1 , much lower than commercial RuO 2 (225mV dec -1 ).

[0082] The linear sweep voltammetric curve of oxygen evolution in 1M KOH + seawater (alkaline seawater) electrolyte is as follows Fig.16 As shown, at 500 and 1000 mA cm -2 The overpotentials are 408mV and 503mV respectively. The Tafel curve of oxygen evolution in 1M KOH + seawater (alkaline seawater) electrolyte is as follows Fig.18 As shown, the Tafel slope of CoNiS-30 is only 151mV dec -1 .

[0083] Example 3: Preparation method of anode catalytic electrode for hydrogen production by seawater electrolysis at industrial current density

[0084] Step 1: Add nickel nitrate, cobalt nitrate and urea weighed according to the stoichiometric ratio into 40 mL of deionized water and stir to form a mixed solution; the concentration of nickel nitrate in the mixed solution is 150 mM, the concentration of cobalt nitrate is 10 mM, and the concentration of urea is 900 mM;

[0085] Step 2: 3*3cm 2 The foamed metal is placed in the solution prepared in step 1 and reacted in a sealed container at 120° C. for 6 hours;

[0086] Step 3: Add the metal foam obtained in step 2 into 40 mL of 625 mM sodium sulfide aqueous solution and react in a sealed container at 120° C. for 8 h;

[0087] Step 4: Add the metal foam obtained in step 3 to 20 mL of 30% hydrogen peroxide solution at 25° C., let it react for 90 seconds, then rinse with deionized water to obtain a CoNiS-90 anode catalytic electrode.

[0088] The field emission scanning electron microscopy image of the obtained CoNiS-90 anode catalytic electrode is shown in Figure 4 As shown, the morphology of the catalytic electrode is agglomerated nanoparticles.

[0089] The linear sweep voltammetric curve of oxygen evolution in 1M KOH electrolyte is as follows Figure 8 As shown, at 500 and 1000 mA cm -2 The overpotentials are 365mV and 441mV respectively. The Tafel curve of oxygen evolution in 1M KOH electrolyte is as follows Fig.10 As shown, the Tafel slope of CoNiS-90 is 132 mV dec -1 , lower than commercial RuO 2 (208mV dec -1 ).

[0090] The linear sweep voltammetric curve of oxygen evolution in 1M KOH+0.5M NaCl (simulated seawater) electrolyte is as follows Fig.12 As shown, at 500 and 1000 mA cm -2 The overpotentials are 327mV and 361mV respectively. The Tafel curve of oxygen evolution in 1M KOH + 0.5M NaCl (simulated seawater) electrolyte is as follows Fig.14 As shown, the Tafel slope of CoNiS-90 is only 113 mV dec. -1 , much lower than commercial RuO2 (225mV dec -1 ).

[0091] The linear sweep voltammetric curve of oxygen evolution in 1M KOH + seawater (alkaline seawater) electrolyte is as follows Fig.16 As shown, at 500 and 1000mAcm -2 The overpotentials are 399mV and 508mV respectively. The Tafel curve of oxygen evolution in 1M KOH + seawater (alkaline seawater) electrolyte is as follows Fig.18As shown, the Tafel slope of CoNiS-90 is only 152 mV dec. -1 .

[0092] Comparative Example 1: A method for preparing an anode catalytic electrode

[0093] Step 1: Add nickel nitrate, cobalt nitrate and urea weighed according to the stoichiometric ratio into 40 mL of deionized water and stir to form a mixed solution; the concentration of nickel nitrate in the mixed solution is 150 mM, the concentration of cobalt nitrate is 10 mM, and the concentration of urea is 900 mM;

[0094] Step 2: 3*3cm 2 The foamed metal is placed in the solution prepared in step 1 and reacted in a sealed container at 120° C. for 6 hours;

[0095] Step 3: Add the metal foam obtained in step 2 into 40 mL of 625 mM sodium sulfide aqueous solution, and react in a sealed container at 120° C. for 8 h to obtain a CoNiS anode catalytic electrode.

[0096] The field emission scanning electron microscopy image of the obtained CoNiS anode catalyst electrode is shown in Figure 5 As shown, the morphology of the catalytic electrode is an array structure formed by orderly arrangement of nanorods.

[0097] The linear sweep voltammetric curve of oxygen evolution in 1M KOH electrolyte is as follows Figure 8 As shown, at 500 and 1000mAcm -2 The overpotentials are 394mV and 498mV respectively. The Tafel curve of oxygen evolution in 1M KOH electrolyte is as follows Fig.10 As shown, the Tafel slope of CoNiS is 183 mV dec -1 , lower than commercial RuO 2 (208mV dec -1 ).

[0098] The linear sweep voltammetric curve of oxygen evolution in 1M KOH+0.5M NaCl (simulated seawater) electrolyte is as follows Fig.12 As shown, at 500 and 1000mAcm -2 The overpotentials are 353mV and 420mV respectively. The Tafel curve of oxygen evolution in 1M KOH + 0.5M NaCl (simulated seawater) electrolyte is as follows Fig.14 As shown, the Tafel slope of CoNiS is only 141mV dec -1 , much lower than commercial RuO 2 (225mV dec -1 ).

[0099] The linear sweep voltammetric curve of oxygen evolution in 1M KOH + seawater (alkaline seawater) electrolyte is as follows Fig.16 As shown, at 500 and 1000mAcm -2 The overpotentials are 405mV and 505mV respectively. The Tafel curve of oxygen evolution in 1M KOH + seawater (alkaline seawater) electrolyte is as follows Fig.18 As shown, the Tafel slope of CoNiS is 185mV dec -1 .

[0100] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An anode catalytic electrode for hydrogen production by seawater electrolysis at industrial current density, It is characterized in that The anode catalytic electrode uses metal foam as a three-dimensional carrier, a cobalt-doped nickel sulfide array is in-situ grown on the surface of the three-dimensional carrier, and a highly active sulfur protective layer containing vacancies is covered on the surface of the array; The industrial current density range is 500-1000mAcm -2 ; The method for preparing the anode catalytic electrode comprises the following steps: Step 1: Weigh cobalt salt, nickel salt and urea and dissolve them in 40 mL of deionized water to form a solution, wherein the concentration of nickel salt in the mixed solution is 150 mM, the concentration of cobalt salt is 10 mM, and the concentration of urea is 900 mM; Step 2: placing the metal foam in the solution of step 1, and reacting in a closed manner to obtain a cobalt-doped nickel hydroxide precursor; Step 3: Add the precursor obtained in step 2 to 40 mL of an aqueous solution having a sulfur salt concentration of 625 mM, and conduct a closed reaction to obtain a cobalt-doped nickel sulfide precursor; Step 4: Add the precursor obtained in step 3 into a hydrogen peroxide solution and react to obtain the product.

2. The anode catalytic electrode according to claim 1, It is characterized in that The metal foam includes foamed nickel, foamed copper, foamed nickel-iron and foamed cobalt.

3. The anode catalytic electrode according to claim 1, It is characterized in that In the cobalt-doped nickel sulfide array and the high-activity sulfur protective layer containing vacancies, the cobalt content is 0%-10% and the cobalt content is not 0%, the nickel content is 40%-50%, the sulfur content is 30%-50%, and the vacancy content accounts for 0%-10% of the sulfur content, in a molar ratio.

4. The method for preparing an anode catalytic electrode for hydrogen production by seawater electrolysis at an industrial-grade current density according to any one of claims 1 to 3, It is characterized in that The following steps are involved: Step 1: Weigh cobalt salt, nickel salt and urea and dissolve them in deionized water to form a solution; Step 2: placing the metal foam in the solution of step 1, and reacting in a closed manner to obtain a cobalt-doped nickel hydroxide precursor; Step 3: adding the precursor obtained in step 2 to an aqueous solution containing a sulfur salt, and conducting a closed reaction to obtain a cobalt-doped nickel sulfide precursor; Step 4: Add the precursor obtained in step 3 into a hydrogen peroxide solution and react to obtain the product.

5. The preparation method according to claim 4, It is characterized in that The cobalt salt and the nickel salt are selected from any soluble metal salt.

6. The preparation method according to claim 4, It is characterized in that The molar ratio of cobalt salt:nickel salt is 1:1-50.

7. The preparation method according to claim 4, It is characterized in that In the solution of step 1, the total molar concentration of the metal salt is 50-200 mM.

8. The preparation method according to claim 4, It is characterized in that The molar ratio of urea to metal salt is 1:1 to 1:

10.

9. The preparation method according to claim 4, It is characterized in that In step 2, the reaction temperature is 100-200° C. and the reaction time is 2-72 h.

10. The preparation method according to claim 4, It is characterized in that In step 3, the reaction temperature is 100-200° C., and the reaction time is 2-72 h.

11. The preparation method according to claim 4, It is characterized in that The sulfur salts include sodium sulfide, thioacetamide, thiourea and sulfur powder.

12. The preparation method according to claim 4, It is characterized in that The molar concentration of the sulfide salt in the aqueous solution containing the sulfide salt is 0.2-1M.

13. The preparation step according to claim 4, It is characterized in that The concentration of the hydrogen peroxide solution is 3%-30% by volume.

14. The preparation step according to claim 4, It is characterized in that In step 4, the reaction temperature is 0-60°C; the reaction time is 10s-20min.

15. The preparation step according to claim 4, It is characterized in that The reaction temperature in step 4 is 25°C.

16. Use of the anode catalytic electrode for producing hydrogen by electrolysis of seawater at an industrial-grade current density as claimed in any one of claims 1 to 3 in producing hydrogen by electrolysis of seawater.

17. The use according to claim 16, It is characterized in that The application is that the anode catalytic electrode is used as the anode of the electrocatalytic seawater electrolysis hydrogen production device.

Citation Information

Patent Citations

  • Self-supporting NF@Co-Ni3S2 @ NiO nanorod material and preparation method and application thereof

    CN110880423A

  • Foamed nickel-based porous NiFe hydrotalcite nanosheet as well as preparation and application thereof

    CN111229232A

  • Preparation method of bimetal-doped Ni3S2 oxygen evolution electrocatalyst

    CN114438545A

  • Ferronickel hydrotalcite-like / ferronickel sulfide heterostructure seawater oxidation electrocatalyst and preparation method thereof

    CN114657591A

  • Composite, hierarchical electrocatalytic materials for water splitting

    US20210404073A1