A kind of moisture absorption and perspiration polyester fiber and preparation method thereof

Through the design of discontinuous spinneret holes and the FDY process, moisture-absorbing and sweating polyester fibers with special-shaped cross-sections and uneven strip-dry structures were prepared, which solved the problem of insufficient moisture-absorbing and sweating performance caused by the continuity of spinneret holes in the prior art. , achieving efficient moisture and sweat discharge, improving the breathability and comfort of the fabric.

CN115852505BActive Publication Date: 2024-11-01JIANGSU XUANDA POLYMER MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211648389.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-11-01
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

The spinneret holes of existing moisture-absorbent and sweat-absorbent polyester fibers are continuous and cannot use the unevenness of the strip and dryness to improve moisture-absorbent and sweat-absorbent performance.

Method used

The design of discontinuous spinneret holes is specifically designed as spinneret holes with a "cross" font structure. The moisture-absorbing and sweating polyester fiber is prepared through the FDY process, and the melt orifice puffing effect is used to form a special-shaped cross-section and uneven strip-dry structure. , increase the gaps and surface area between the fibers, and improve the moisture-absorbing and sweating ability of the fabric.

Benefits of technology

A significant improvement in moisture-absorbing and sweating performance has been achieved. The fiber surface has non-periodic arrangement of nodes and "L"-shaped grooves, forming capillaries that quickly absorb and discharge moisture and sweat, enhancing the breathability and comfort of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115852505B_ABST
    Figure CN115852505B_ABST
Patent Text Reader

Abstract

The present invention relates to a moisture absorbing and perspiration releasing polyester fiber and a preparation method thereof. The spinneret holes in the spinneret used are discontinuous "cross"-like structures, and the orifice expansion effect of the melt is utilized to prepare the moisture absorbing and perspiration releasing polyester fiber from the polyester melt. The obtained polyester fiber is not only a fiber with a special-shaped cross section, but also forms a structure with uneven strips, which can increase the gaps between the fibers, increase the contact area between the fabric and the outside air, and is conducive to the discharge of moisture and sweat. The surface of the polyester fiber has nodes arranged non-periodically, which causes uneven stress of the fiber, thereby forming curling, which is conducive to the moisture absorbing and perspiration releasing of the fabric. In addition, the obtained polyester fiber has a high specific surface area, and the surface of the single fiber has an "L"-shaped groove, which can form a capillary with the grooves of other fibers. The capillary principle is utilized to enable the fiber to quickly absorb water, transport water, diffuse and volatilize, and can quickly absorb moisture and sweat from the skin surface and discharge them to the outer layer for evaporation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a moisture absorbing and perspiration releasing polyester fiber and a preparation method thereof. Background Art

[0002] As one of the three main fibers in synthetic fibers, polyester fiber is widely used in clothing fabrics and other non-clothing fields due to its excellent physical and chemical properties. Since its launch, polyester fiber products have been used by downstream users as the main textile raw materials for weaving various textiles due to their good drape and high strength. However, people later discovered that due to the regularity of polyester macromolecular chains and the absence of hydrophilic groups, this will lead to poor moisture absorption and air permeability, making the fabrics or clothing made from them uncomfortable to wear, poor air permeability, and stuffy. Therefore, polyester that can absorb moisture and perspiration has attracted people's attention.

[0003] At present, moisture-wicking polyester fabrics have a wide range of uses, mainly in sportswear, casual wear, underwear, travel wear, outerwear and socks, etc., and can even be used in geotextiles, with broad application prospects. At present, moisture-wicking polyester is mainly achieved through two methods: chemical modification and physical modification. Chemical modification methods include hydrophilic group grafting copolymerization and hydrophilic compound coating treatment. Physical modification methods include fiber cross-section profiling, raw material blending spinning, and two-component composite co-spinning.

[0004] Among them, moisture wicking fibers are mainly achieved through the profiling of fiber cross-sections. The moisture wicking mechanism is based on the capillary phenomenon produced by the fine grooves on the fiber surface, which enables sweat to quickly migrate to the surface of the fabric and dissipate through wicking, diffusion, and transmission, thereby achieving the purpose of moisture conduction and quick drying.

[0005] At present, the spinnerets used for fiber cross-section profiling are mostly continuous, and it is impossible to use the unevenness of the yarn to further improve the moisture absorption and perspiration wicking capacity. Therefore, a new type of spinneret is needed to prepare a polyester fiber with better performance. Summary of the invention

[0006] The object of the present invention is to provide a moisture absorbing and perspiration-releasing polyester fiber and a preparation method thereof, and to use discontinuous spinneret holes to prepare a moisture absorbing and perspiration-releasing polyester fiber with an uneven strip structure, which has excellent moisture absorbing and perspiration-releasing performance.

[0007] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: a method for preparing a moisture-absorbing and perspiration-releasing polyester fiber, which adopts the FDY process to prepare the moisture-absorbing and perspiration-releasing polyester fiber by metering, extruding, cooling, oiling, stretching, heat-setting and winding a polyester melt, wherein the spinneret in the spinneret used is a "cross"-shaped structure, and the spinneret includes two unconnected first L-shaped holes and a second L-shaped hole, and the first L-shaped hole and the second L-shaped hole are both formed by connecting two straight holes, and the angles a and b formed by the two straight holes are 80°-90° respectively, and a straight hole of the first L-shaped hole and a straight hole of the second L-shaped hole are located on the same straight line; the areas of the first L-shaped hole and the second L-shaped hole are S1 and S2 respectively, and S1:S2=1.3-1.5:1.

[0008] Further, the hole width of the first L-shaped hole is the same as the hole width of the second L-shaped hole; and the shortest distance between the first L-shaped hole and the second L-shaped hole is the hole width of the first L-shaped hole.

[0009] Furthermore, the ratio of the outer side length to the hole width of the first L-shaped hole is 7-9:1.

[0010] Furthermore, the parameters of the FDY process are:

[0011] Spinning temperature: 285℃-290℃;

[0012] Cooling temperature: 20℃-25℃;

[0013] Network pressure: 0.20MPa-0.25MPa;

[0014] One roller speed: 2000m / min-2100m / min;

[0015] First roller temperature: 82℃-90℃;

[0016] Second roller speed: 3800m / min-4000m / min;

[0017] Second roller temperature: 125℃-135℃;

[0018] Winding speed: 3750m / min-3940m / min.

[0019] The present invention also provides a moisture wicking polyester fiber, which is prepared by the method for preparing the moisture wicking polyester fiber as described above. The cross-section of the moisture wicking polyester fiber is an asymmetric "cross" structure, the CV value of the strip unevenness is 3.5-5.0%, the U value of the strip unevenness is 2.5-5.5%, the vertical wicking height is ≥120mm, and the evaporation rate is 0.21g / h.

[0020] Furthermore, the fineness of the moisture absorbing and perspiration-releasing polyester fiber monofilament is 2.5-3.0 dtex.

[0021] Furthermore, the moisture wicking polyester fiber has a fineness of 80-120 dtex, a breaking strength of ≥3.2 cN / dtex, a breaking elongation of 50.0±5.0%, a boiling water shrinkage of 8.0-12.0%, an oil content of 0.90±0.20%, and a profile of 45-55%.

[0022] The beneficial effects of the present invention are as follows: the spinneret holes in the spinneret used are of a discontinuous "cross"-like structure, and the orifice expansion effect of the melt is utilized to make the polyester melt into moisture-absorbing and perspiration-releasing polyester fibers; because the spinneret holes are of a discontinuous special-shaped structure, the obtained polyester fibers are not only special-shaped cross-section fibers, but also form a structure with uneven strips, which can increase the gaps between the fibers, increase the contact area between the fabric and the outside air, and facilitate the discharge of moisture and sweat; the surface of the polyester fiber has non-periodically arranged nodes, which causes uneven stress of the fiber, thereby forming curling, which is beneficial to the moisture absorption and perspiration release of the fabric.

[0023] In addition, the obtained polyester fiber has a higher specific surface area, and the surface of a single fiber has an "L"-shaped groove, which can form capillaries with the grooves of other fibers. Utilizing the capillary principle, the fiber can quickly absorb, transport, diffuse and volatilize water, and can quickly absorb moisture and sweat from the skin surface and discharge it to the outer layer for evaporation.

[0024] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic structural diagram of the spinneret hole shown in the present invention. DETAILED DESCRIPTION

[0026] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0028] The invention provides a method for preparing moisture absorbing and perspiration releasing polyester fiber. The FDY process is adopted to prepare the moisture absorbing and perspiration releasing polyester fiber by metering, extruding, cooling, oiling, stretching, heat setting and winding polyester melt.

[0029] See also Figure 1 The spinneret used has several spinneret holes of a "cross"-shaped structure. The structure of the spinneret is the prior art, and the difference lies in the structure of the spinneret holes, which will not be described in detail here.

[0030] In this embodiment, the spinneret includes two unconnected first L-shaped holes 1 and second L-shaped holes 2. The first L-shaped hole 1 and the second L-shaped hole 2 are both of "L"-shaped structure, and the first L-shaped hole 1 and the second L-shaped hole 2 are both formed by connecting two straight holes, and the angles a and b formed by the two straight holes are 80°-90° respectively. One straight hole of the first L-shaped hole 1 and one straight hole of the second L-shaped hole 2 are located on the same straight line.

[0031] Specifically, the first L-shaped hole 1 includes a first straight hole 11 and a second straight hole 12 connected to the first straight hole 11, and the angle a formed by the first straight hole 11 and the second straight hole 12 is 80°-90°. The second L-shaped hole 2 includes a third straight hole 21 and a fourth straight hole 22 connected to the third straight hole 21, and the angle b formed by the third straight hole 21 and the fourth straight hole 22 is 80°-90°.

[0032] It is worth noting that the above numerical values ​​include all values ​​of lower and upper values ​​increased by one unit from the lower limit to the upper limit, and there is a gap of at least two units between any lower value and any higher value.

[0033] For example, the angle a formed by the first straight hole 11 and the second straight hole 12 is 80°-90°, preferably 82°-88°, and more preferably 84°-86°, in order to illustrate the values ​​not explicitly listed above, such as 81°, 83°, 85°, etc.

[0034] As mentioned above, the example range with 2° as the interval unit does not exclude the increase of the numerical unit with appropriate units such as 0.5°, 1°, 3°, etc. These are just examples intended to be clearly expressed, and it can be considered that all possible combinations of numerical values ​​listed between the lowest value and the highest value are clearly stated in this specification in a similar manner.

[0035] Unless otherwise specified, all ranges include endpoints and all numbers between the endpoints. For other limiting descriptions of numerical ranges appearing in this article, please refer to the above description and will not be repeated here.

[0036] The hole width of the first L-shaped hole 1 is the same as the hole width of the second L-shaped hole 2, that is, the hole widths of the first linear hole 11, the second linear hole 12, the third linear hole 21 and the fourth linear hole 22 are all the same.

[0037] In this embodiment, the first linear hole 11 and the third linear hole 21 are located on the same straight line. Since the hole widths of the two are the same, the inner edges and outer edges of the two are respectively located on the same straight line. Among them, the size of the inner edge is shorter than the size of the outer edge.

[0038] The inner edge of the first straight hole 21 and the inner edge of the second straight hole 12 form an angle a, and the inner edge of the third straight hole 21 and the inner edge of the fourth straight hole 22 form an angle b.

[0039] The areas of the first L-shaped hole 1 and the second L-shaped hole 2 are S1 and S2 respectively, and S1:S2=1.3-1.5:1. That is, the area of ​​the first L-shaped hole 1 is greater than the area of ​​the second L-shaped hole 2.

[0040] The shortest distance between the first L-shaped hole 1 and the second L-shaped hole 2 is the hole width of the first L-shaped hole 1. The shortest distance between the first L-shaped hole 1 and the second L-shaped hole 2 is the size of the gap between the first straight hole 11 and the third straight hole 21, which is as follows: Figure 1 As shown in c.

[0041] The ratio of the outer side length to the hole width of the first L-shaped hole 1 is 7-9:1.

[0042] The FDY process is a prior art and will not be described in detail herein. The parameters of the FDY process are:

[0043] Spinning temperature: 285℃-290℃;

[0044] Cooling temperature: 20℃-25℃;

[0045] Network pressure: 0.20MPa-0.25MPa;

[0046] One roller speed: 2000m / min-2100m / min;

[0047] First roller temperature: 82℃-90℃;

[0048] Second roller speed: 3800m / min-4000m / min;

[0049] Second roller temperature: 125℃-135℃;

[0050] Winding speed: 3750m / min-3940m / min.

[0051] Polymer materials have viscoelasticity in the molten state, and their volume will shrink under pressure. When the pressure is released, the volume of the polymer melt will recover and expand, which is called the orifice expansion effect. At the same time, the orifice expansion effect of the melt has a certain relationship with the spinneret hole area. The smaller the spinneret hole area, the more serious the orifice expansion phenomenon of the melt.

[0052] In this embodiment, moisture wicking polyester fibers are prepared by changing the shape and distribution of the spinneret holes of the spinneret. The spinneret holes are made into a "cross"-like structure, and the orifice expansion effect when the melt is extruded from the spinneret holes is utilized to make the melt streams adhere to each other to form special-shaped fibers.

[0053] The spinneret hole is composed of two discontinuous L-shaped long holes, including the first L-shaped hole 1 and the second L-shaped hole 2. The first L-shaped hole 1 and the second L-shaped hole 2 are a group, which are respectively viscous flow No. 1 and viscous flow No. 2. The areas of the two L-shaped holes are S1 and S2, respectively, and S1>S2. If the hole areas of the two L-shaped holes are different, the shear rates passing through the two L-shaped holes are different.

[0054] Under the same material, spinning process conditions and spinneret length, the shear rate decreases with the increase of the L-shaped hole area. The spinneret length is the length of the first L-shaped hole 1 and the second L-shaped hole 2 perpendicular to the Figure 1 The length in the direction of the plane shown.

[0055] γ=(n+3)BQ / (2A 2 )

[0056] Where γ is the shear rate, B is the perimeter of the shaped hole, Q is the volume flow rate, A is the area of ​​the shaped hole, and n is the rheological index.

[0057] The shear rates of the melt passing through the first L-shaped hole 1 and the second L-shaped hole 2 are γ1 and γ2 respectively, and γ1<γ2. At the same time, due to the orifice expansion effect, the two melt flows will adhere to each other. At the same time, the orifice expansion ratio (the ratio of the equilibrium cross-sectional area of ​​the extrudate to the cross-sectional area of ​​the die) will increase with the increase of the shear rate, resulting in the orifice expansion ratios of flow No. 1 and flow No. 2 increasing successively.

[0058] There are two types of viscosity: ① molecular viscosity, which reflects the momentum transport effect of molecules in motion; ② turbulent viscosity, which reflects the effect of turbulent motion on momentum transport. Since both No. 1 and No. 2 are polyester melts, their melt viscosity will decrease with the increase of shear rate. The shear rate of No. 1 in the monomer volume is lower than that of No. 2, which will increase the shear rate of the part of No. 1 that adheres to No. 2, thereby reducing the viscosity of this part of No. 1 and improving fluidity, making it easier to break away from the main No. 1 and attach to the No. 2.

[0059] Since the shear rate of the No. 1 flow is lower than that of the No. 2 flow, when the No. 1 and No. 2 flows are bonded into a filament, the No. 1 flow tends to follow the No. 2 flow and flow at a rate exceeding its own shear rate, which causes the No. 1 flow to be periodically interrupted, resulting in the formation of non-periodic nodes on the fiber surface. The result of the above phenomenon is that the obtained fiber is not only a fiber with a special cross-section, but also forms an uneven structure.

[0060] The present invention also provides a moisture absorbing and perspiration releasing polyester fiber, which is prepared by the above method for preparing the moisture absorbing and perspiration releasing polyester fiber.

[0061] The spinneret holes in the spinneret used are discontinuous "cross"-like structures, and the orifice expansion effect of the melt is utilized to make the polyester melt into moisture-absorbing and perspiration-releasing polyester fibers, the cross section of which is an asymmetric "cross"-shaped structure.

[0062] Different from the continuous spinneret holes used in the preparation of general moisture wicking fibers, the spinneret holes in this application are discontinuous and shaped structures, so the obtained polyester fibers are not only shaped cross-section fibers, but also form an uneven structure with a CV value of 3.5-5.0% and a U value of 2.5-5.5%. This can increase the gaps between fibers, increase the contact area between the fabric and the outside air, and facilitate the discharge of moisture and sweat.

[0063] The surface of polyester fiber has non-periodic nodes, which causes uneven stress on the fiber, thus forming curls, which is beneficial to the moisture absorption and perspiration removal of the fabric.

[0064] The cross-section of the moisture-absorbing and perspiration-wicking fiber is a "cross" shape, which makes the fiber have a higher specific surface area, and the surface of a single fiber has "L"-shaped grooves, which can form capillaries with the grooves of other fibers. By utilizing the capillary principle (that is, when the liquid is on the inside of a tubular object, it overcomes gravity and rises due to the difference between the liquid's own cohesion and the adhesion between the liquid and the tube wall), the fiber can quickly absorb water, transport water, diffuse and volatilize, and can quickly absorb moisture and sweat from the skin surface and discharge them to the outer layer for evaporation.

[0065] The vertical wicking height of the obtained moisture wicking fiber is ≥120mm, and the evaporation rate is 0.21g / h. The fineness of the moisture wicking polyester fiber monofilament is 2.5-3.0dtex. The fineness of the moisture wicking polyester fiber is 80-120dtex, the breaking strength is ≥3.2cN / dtex, the breaking elongation is 50.0±5.0%, the boiling water shrinkage is 8.0-12.0%, the oil content is 0.90±0.20%, and the degree of irregularity is 45-55%.

[0066] The above preparation method is described in detail below with reference to specific examples.

[0067] Embodiment 1

[0068] The area of ​​the first L-shaped hole of the spinneret is 0.0461 mm 2 , the outer side length is 0.42mm, the hole width is 0.06mm, the angle a between the first straight hole and the second straight hole is 80°; the area of ​​the second L-shaped hole is 0.0354mm 2 The outer side length is 0.33 mm, the hole width is 0.06 mm, and the angle a formed by the third straight hole and the fourth straight hole is 80°.

[0069] The spinneret is used to prepare moisture-absorbing and perspiration-releasing polyester fibers by adopting the FDY process, through metering, extrusion, cooling, oiling, stretching, heat setting and winding of polyester melt.

[0070] The parameters of the FDY process are:

[0071] Spinning temperature: 285℃;

[0072] Cooling temperature: 25℃;

[0073] Network pressure: 0.20MPa;

[0074] One roller speed: 2000m / min;

[0075] First roller temperature: 82℃;

[0076] Second roller speed: 3800m / min;

[0077] Second roller temperature: 125℃;

[0078] Winding speed: 3750m / min.

[0079] The moisture wicking polyester fiber obtained by the above steps has a CV value of 3.5%, a U value of 2.5%, a vertical wicking height of 122 mm, an evaporation rate of 0.21 g / h, a monofilament fineness of 2.5 dtex, a fiber fineness of 80 dtex, a breaking strength of 3.3 cN / dtex, a breaking elongation of 55%, a boiling water shrinkage of 12.0%, an oil content of 0.90%, and a profile of 45%.

[0080] Embodiment 2

[0081] The area of ​​the first L-shaped hole of the spinneret is 0.0612 mm 2 , the outer side length is 0.54mm, the hole width is 0.06mm, the angle a between the first straight hole and the second straight hole is 90°; the area of ​​the second L-shaped hole is 0.0408mm 2The outer side length is 0.37 mm, the hole width is 0.06 mm, and the angle a formed by the third straight hole and the fourth straight hole is 90°.

[0082] The spinneret is used to prepare moisture-absorbing and perspiration-releasing polyester fibers by adopting the FDY process, through metering, extrusion, cooling, oiling, stretching, heat setting and winding of polyester melt.

[0083] The parameters of the FDY process are:

[0084] Spinning temperature: 290℃;

[0085] Cooling temperature: 20℃;

[0086] Network pressure: 0.25MPa;

[0087] One roller speed: 2100m / min;

[0088] First roller temperature: 90℃;

[0089] Second roller speed: 4000m / min;

[0090] Second roller temperature: 135℃;

[0091] Winding speed: 3940m / min.

[0092] The moisture wicking polyester fiber obtained by the above steps has a CV value of 5.0%, a U value of 5.5%, a vertical wicking height of 123 mm, an evaporation rate of 0.21 g / h, a monofilament fineness of 3.0 dtex, a fiber fineness of 120 dtex, a breaking strength of 3.4 cN / dtex, a breaking elongation of 45%, a boiling water shrinkage of 8.0%, an oil content of 1.10%, and a profile of 55%.

[0093] Embodiment 3

[0094] The area of ​​the first L-shaped hole of the spinneret is 0.0612 mm 2 , the outer side length is 0.48mm, the hole width is 0.06mm, the angle a between the first straight hole and the second straight hole is 90°; the area of ​​the second L-shaped hole is 0.04380mm 2 The outer side length is 0.33 mm, the hole width is 0.06 mm, and the angle a formed by the third straight hole and the fourth straight hole is 80°.

[0095] The spinneret is used to prepare moisture-absorbing and perspiration-releasing polyester fibers by adopting the FDY process, through metering, extrusion, cooling, oiling, stretching, heat setting and winding of polyester melt.

[0096] The parameters of the FDY process are:

[0097] Spinning temperature: 288°C;

[0098] Cooling temperature: 22℃;

[0099] Network pressure: 0.25MPa;

[0100] One roller speed: 2050m / min;

[0101] First roller temperature: 85℃;

[0102] Second roller speed: 3900m / min;

[0103] Second roller temperature: 130℃;

[0104] Winding speed: 3820m / min.

[0105] The moisture wicking polyester fiber obtained by the above steps has a CV value of 4.0%, a U value of 3.5%, a vertical wicking height of 125 mm, an evaporation rate of 0.21 g / h, a monofilament fineness of 2.8 dtex, a fiber fineness of 100 dtex, a breaking strength of 3.3 cN / dtex, a breaking elongation of 50%, a boiling water shrinkage of 12.0%, an oil content of 1.00%, and a profile of 53%.

[0106] Embodiment 4

[0107] The area of ​​the first L-shaped hole of the spinneret is 0.0608 mm 2 , the outer side length is 0.54mm, the hole width is 0.06mm, the angle a between the first straight hole and the second straight hole is 85°; the area of ​​the second L-shaped hole is 0.0450mm 2 The outer side length is 0.34 mm, the hole width is 0.06 mm, and the angle a formed by the third straight hole and the fourth straight hole is 85°.

[0108] The spinneret is used to prepare moisture-absorbing and perspiration-releasing polyester fibers by adopting the FDY process, through metering, extrusion, cooling, oiling, stretching, heat setting and winding of polyester melt.

[0109] The parameters of the FDY process are:

[0110] Spinning temperature: 288°C;

[0111] Cooling temperature: 22℃;

[0112] Network pressure: 0.25MPa;

[0113] One roller speed: 2050m / min;

[0114] First roller temperature: 85℃;

[0115] Second roller speed: 3900m / min;

[0116] Second roller temperature: 130℃;

[0117] Winding speed: 3820m / min.

[0118] The moisture wicking polyester fiber obtained by the above steps has a CV value of 4.5%, a U value of 4.7%, a vertical wicking height of 122 mm, an evaporation rate of 0.21 g / h, a monofilament fineness of 3.0 dtex, a fiber fineness of 120 dtex, a breaking strength of 3.3 cN / dtex, a breaking elongation of 48%, a boiling water shrinkage of 11.0%, an oil content of 1.00%, and a profile of 54%.

[0119] In summary, the spinneret holes used in the spinneret are discontinuous "cross"-like structures, and the orifice expansion effect of the melt is used to make moisture-absorbing and perspiration-releasing polyester fibers from the polyester melt. Since the spinneret holes are discontinuous special-shaped structures, the obtained polyester fibers are not only special-shaped cross-section fibers, but also form an uneven structure, which can increase the gaps between the fibers, increase the contact area between the fabric and the outside air, and facilitate the discharge of moisture and sweat; the surface of the polyester fiber has non-periodically arranged nodes, which causes uneven stress in the fiber, thereby forming curls, which is beneficial to the moisture absorption and perspiration release of the fabric.

[0120] In addition, the obtained polyester fiber has a higher specific surface area, and the surface of a single fiber has an "L"-shaped groove, which can form capillaries with the grooves of other fibers. Utilizing the capillary principle, the fiber can quickly absorb, transport, diffuse and volatilize water, and can quickly absorb moisture and sweat from the skin surface and discharge it to the outer layer for evaporation.

[0121] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0122] The above embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a moisture wicking polyester fiber, characterized in that: The FDY process is adopted to prepare the moisture-absorbing and perspiration-releasing polyester fiber by metering, extruding, cooling, oiling, stretching, heat-setting and winding the polyester melt. The spinneret in the spinneret is a "cross"-shaped structure, and the spinneret includes two unconnected first L-shaped holes and a second L-shaped hole. The first L-shaped hole and the second L-shaped hole are formed by connecting two straight holes, and the angles a and b of the two straight holes are 80°-90° respectively. A straight hole of the first L-shaped hole and a straight hole of the second L-shaped hole are located on the same straight line. The polyester melt extruded from the first L-shaped hole and the second L-shaped hole adhere to each other under the action of the orifice expansion effect, so that the cross section of the moisture-absorbing and perspiration-releasing polyester fiber is an asymmetric "cross" structure; The polyester melt extruded from the first L-shaped hole is a No. 1 viscous flow, and the polyester melt extruded from the second L-shaped hole is a No. 2 viscous flow. The areas of the first L-shaped hole and the second L-shaped hole are S1 and S2 respectively, and S1:S2=1.3-1.5:

1. The shear rate of the No. 1 viscous flow is less than the shear rate of the No. 2 viscous flow, so that when the No. 1 viscous flow and the No. 2 viscous flow are bonded into filaments, the No. 1 viscous flow is interrupted, resulting in the formation of non-periodically arranged nodes on the surface of the moisture absorbing and perspiration polyester fiber, forming an uneven structure. The CV value of the unevenness rate of the moisture absorbing and perspiration polyester fiber is 3.5-5.0%, the U value of the unevenness rate of the strip is 2.5-5.5%, the vertical wicking height is ≥120mm, and the evaporation rate is 0.21g / h.

2. The method for preparing the moisture wicking polyester fiber according to claim 1, characterized in that: The hole width of the first L-shaped hole is the same as the hole width of the second L-shaped hole; the shortest distance between the first L-shaped hole and the second L-shaped hole is the hole width of the first L-shaped hole.

3. The method for preparing the moisture wicking polyester fiber according to claim 1, characterized in that: The ratio of the outer side length to the hole width of the first L-shaped hole is 7-9:

1.

4. The method for preparing the moisture wicking polyester fiber according to claim 1, characterized in that: The parameters of the FDY process are: Spinning temperature: 285℃-290℃; Cooling temperature: 20℃-25℃; Network pressure: 0.20MPa-0.25MPa; One roller speed: 2000m / min-2100m / min; First roller temperature: 82℃-90℃; Second roller speed: 3800m / min-4000m / min; Second roller temperature: 125℃-135℃; Winding speed: 3750m / min-3940m / min.

5. A moisture wicking polyester fiber, characterized in that: The moisture wicking polyester fiber is prepared by the method for preparing the moisture wicking polyester fiber as described in any one of claims 1 to 4.

6. The moisture wicking polyester fiber according to claim 5, characterized in that The fineness of the moisture absorbing and perspiration wicking polyester fiber monofilament is 2.5-3.0 dtex.

7. The moisture wicking polyester fiber according to claim 5, characterized in that The moisture absorbing and perspiration-releasing polyester fiber has a fineness of 80-120 dtex, a breaking strength of ≥3.2 cN / dtex, a breaking elongation of 50.0±5.0%, a boiling water shrinkage of 8.0-12.0%, an oil content of 0.90±0.20%, and a profile of 45-55%.