Low temperature sleeve grouting material for steel bar connection and preparation method thereof
Through reasonable proportioning and preparation of modified silicon fume, combined with gypsum and antifreeze and other components, the problem of hydration of low-temperature sleeve grouting is solved, and high-performance construction is achieved in an environment of -5-10℃. Simplify production processes and reduce costs.
Patent Information
- Application Number
- CN202211688629.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-12-27
AI Technical Summary
The existing low-temperature sleeve grouting material is limited in hydration under an environment of -5℃, which affects the construction progress and is complex in production processes or high in cost.
Use reasonable proportions of ordinary silicate cement, sulfur aluminate cement, high alumina cement and modified silica fume, gypsum, antifreeze, phase change materials, early strength agent, retarder, water reducing agent and expansion agent, The grafting reaction of modified fume and isoprenol polyoxyethylene ether is improved by modifying the silane coupling agent, and the fluidity and strength of the grouting material are improved, and early and late expansion agents are combined to meet the construction performance requirements.
The characteristics of high flow state, micro-expansion, fast early strength development and high later strength are achieved in an environment of -5-10℃, which solves the problem of limited hydration, simplifies the production process and reduces costs.
Smart Images

Figure BDA0004020244180000061 
Figure BDA0004020244180000071 
Figure BDA0004020244180000021
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sleeve grouting materials, and in particular relates to a low-temperature sleeve grouting material for steel bar connection and a preparation method thereof. Background Art
[0002] At present, the steel sleeve connection technology is widely used in component connection technology of prefabricated buildings. This connection technology has the advantages of excellent performance, low cost, reduced deadweight, convenient construction, reduced garbage, and reduced pollution. Sleeve grouting material is the key to steel sleeve connection technology, and its performance plays a vital role in structural safety and durability. However, the performance of ordinary sleeve grouting materials is greatly restricted by the construction environment temperature. It needs to be constructed at a temperature above 5°C. Under low temperature conditions, cement hydration is limited, and early strength development is slow, which seriously affects the construction progress. For northern my country, the low temperature season is long, and low-temperature construction is inevitable due to the construction progress. Therefore, the development of sleeve grouting materials that can be used in negative temperature environments is of great significance to promoting the development of prefabricated buildings.
[0003] CN201910357884.9 discloses a sleeve grouting material that can be constructed in a negative temperature environment of -10℃. On the basis of conventional grouting material components such as cement, fine powder, coarse aggregate, composite expansion agent, water reducer, defoamer, retarder, and early strength agent, a freezing point lowering component, a heating component, and a phase change heat storage component are added to prepare the sleeve grouting material. The produced grouting material can meet various construction performances in an environment of -10℃. It solves the technical problem of heating during winter construction in the vast northern regions, but the production process uses quicklime and stearic acid, and the complex components increase the instability of the system. It requires the materials to be ground together, and the production process is complicated.
[0004] CN201711273212.7 discloses a low-temperature sleeve grouting material and its production process. On the basis of conventional high-strength non-shrinkage sleeve grouting, antifreeze components, early strength admixtures, setting components, and low-temperature plastic expansion catalysts are added, which can achieve high fluidity, slight expansion, and high early strength at a minimum of -5°C. The problem that the sleeve grouting material performance is affected by temperature in a low-temperature environment (minimum -5°C), the early strength is low or no strength, the expansion rate cannot meet the requirements, or even shrinks, etc. is solved. However, polyols and lithium hydroxide are used as raw materials. Polyols are generally liquids, and they need to be measured separately during construction, and the measurement accuracy requirements are extremely high. In addition, lithium hydroxide is easy to deliquesce and is corrosive, which brings many inconveniences to construction and storage.
[0005] CN202010259183.4 discloses a sleeve grouting material for low-temperature steel bar connection and its use method, which mainly uses fast-setting and fast-hardening high-belite sulphoaluminate cement, silicate cement, ultra-high-strength sulphoaluminate cement, gypsum, admixtures, aggregates, nanocrystalline cores, antifreeze agents, powdered polycarboxylic acid high-performance water reducers, polyether defoamers, expansion agents, cellulose ethers, and viscosity reducers as raw materials. The shortcomings of the prior art are overcome, and a sleeve grouting material is provided that meets the requirements of workability, mechanical properties and expansion rate under negative temperature conditions, especially below -10°C, but the fast-setting and fast-hardening high-belite sulphoaluminate cement and ultra-high-strength sulphoaluminate cement used in the raw materials are expensive, and the preparation of the nanocrystalline core is complicated, which greatly increases the production cost. Summary of the invention
[0006] The technical problem to be solved by the present invention is to provide a low-temperature sleeve grouting material for steel bar connection and a preparation method thereof in view of the deficiencies of the above-mentioned prior art. The low-temperature sleeve grouting material for steel bar connection can achieve the characteristics of high fluidity, micro-expansion, fast early strength development and high later strength under -5°C conditions, thereby solving the problem that conventional sleeve grouting materials are difficult to meet construction requirements due to limited hydration in low temperature environments.
[0007] In order to achieve the above object, the present invention adopts the following technical scheme:
[0008] Provided is a low-temperature sleeve grouting material for steel bar connection, comprising the following components by weight: 800-1000 parts of cement, 10-50 parts of modified silica fume, 10-100 parts of gypsum, 900-1100 parts of fine aggregate, 0.1-0.5 parts of early strength agent, 1-3 parts of retarder, 2-5 parts of water reducer, 0.2-0.6 parts of defoamer, 0.1-0.5 parts of expansion agent, 1-5 parts of antifreeze agent, 1-5 parts of phase change material, and a water-to-material ratio of 0.11-0.15; wherein:
[0009] The cement comprises 300-600 parts of ordinary Portland cement, 100-400 parts of sulphoaluminate cement and 50-200 parts of high-alumina cement; wherein the strength grade of ordinary Portland cement and sulphoaluminate cement is 42.5;
[0010] The modified silica fume is obtained by surface-modifying silica fume with a silane coupling agent and then grafting an organic component onto the surface; the silane coupling agent is vinyl tri(β-methoxyethoxy) silane, and the organic component is isopentanol polyoxyethylene ether;
[0011] The expansion agent includes an early expansion agent and a late expansion agent.
[0012] According to the above scheme, the preparation of the modified silica ash includes the following steps: immersing the silica ash in dilute hydrochloric acid for activation, taking it out and drying it after 2-4 hours, then adding it to a vinyl tri(β-methoxyethoxy)silane ethanol solution in a 50-60°C water bath, then heating it to 70-90°C for reaction for 4-6 hours, and then adding isopentanol polyoxyethylene ether, hydrogen peroxide, and deionized water in a nitrogen environment for grafting reaction for 1-3 hours, and finally filtering and separating to obtain the modified silica ash.
[0013] Preferably, the concentration of dilute hydrochloric acid is 10%-15%.
[0014] Preferably, the weight ratio of vinyl tri(β-methoxyethoxy)silane to silica fume is (2-6):100.
[0015] Preferably, the weight ratio of isopentanol polyoxyethylene ether to silica fume is (5-20):100.
[0016] According to the above scheme, the gypsum is anhydrite.
[0017] According to the above scheme, the fine aggregate is at least one of washed and dried river sand, quartz sand, machine-made sand and corundum. Preferably, by weight percentage, the particle size of 1-3 mm accounts for 45%-55%, and the particle size of 0-1 mm accounts for 45%-55%.
[0018] According to the above scheme, the early strength agent is at least one of lithium carbonate, lithium sulfate, lithium fluoride, lithium hydroxide, and lithium fluoride; the retarder is at least one of sodium gluconate, tartaric acid, citric acid, and boric acid.
[0019] According to the above scheme, the water reducing agent is a dry powder polycarboxylic acid-based water reducing agent; the defoaming agent is a dry powder organosilicon defoaming agent.
[0020] According to the above scheme, in the expansion agent, the mass ratio of the early expansion agent to the late expansion agent is (1-3):1.
[0021] According to the above scheme, the early expansion agent is at least one of azo compounds, sulfonylhydrazide compounds, and nitroso compounds; the late expansion agent is at least one of calcium oxide, calcium sulfoaluminate, and magnesium oxide.
[0022] According to the above scheme, the antifreeze agent is at least one of sodium nitrate, sodium nitrite, calcium nitrite, potassium carbonate and calcium chloride.
[0023] According to the above scheme, the phase change material is a high thermal conductivity nano-scale microcapsule phase change material with a particle size of 20-60 μm and a phase change temperature of 5-30°C.
[0024] The present invention also provides a method for preparing a low-temperature sleeve grouting material for steel bar connection, comprising the following steps: weighing cement, modified silica fume, gypsum, fine aggregate, early strength agent, retarder, water reducer, defoamer, expansion agent, antifreeze agent and phase change material according to a formula, mixing and stirring evenly, adding water at a water-to-material ratio of 0.11-0.15 and stirring to obtain the low-temperature sleeve grouting material for steel bar connection.
[0025] The present invention provides a low-temperature sleeve grouting material for steel bar connection. First, ordinary silicate cement, sulphoaluminate cement and high-alumina cement are used in a reasonable proportion. The gypsum and tricalcium silicate in the ordinary silicate cement produce Ca(OH)2, which makes the high-alumina cement produce CAH 10 , C2AH8 and AH3 gel are immediately transformed into C3AH6. At the same time, gypsum can also make C4A3S in sulphoaluminate cement react quickly to generate a large amount of calcium sulfonate. A large amount of calcium sulfonate does not have time to wrap cement particles, thus showing an obvious induction period. In addition, the consumption of calcium hydroxide and gypsum will accelerate the hydration of C3S, thereby promoting the synergistic hydration of the composite system. At the same time, in the modified silica fume, the silica fume is modified by silane coupling agent to achieve surface grafting of isopentanol polyoxyethylene ether; the steric repulsion generated by the organic component isopentanol polyoxyethylene ether overcomes the van der Waals attraction between silica fume particles, and realizes the good dispersion of silica fume in cement-based materials. On the one hand, it can replace the free water between cement particles, and on the other hand, the electrostatic repulsion increases the dispersion of cement, which is beneficial to improve the overall density and fluidity. In addition, the modified silica fume can not only provide nucleation sites to promote cement hydration, but also has a volcanic ash effect, directly participates in the hydration of cement, and improves strength. The use of gypsum can further promote the formation of calcium sulfonate and improve the strength of grouting materials at all ages. The reasonable combination of early strength agent, retarder and water reducer makes the grouting material have better initial fluidity and less fluidity loss after 30 minutes, and can promote the rapid development of strength after 30 minutes to ensure early strength. The combination of early expansion agent and late expansion agent allows the composite expansion component to react and expand in the early and late stages of hydration, better compensating for the shrinkage of concrete in different periods. The use of antifreeze can reduce the freezing point of the slurry pore solution, so that the cementitious material can still undergo hydration reaction at negative temperature. The use of phase change material can absorb and store part of the heat in the initial stage of hydration temperature rise, reduce the slurry temperature peak, and reduce the heat dissipation rate; in the cooling stage, it can release heat, so that the slurry temperature can be maintained in the temperature range suitable for the hydration reaction of the sleeve grouting material for a longer time, promoting the complete hydration of cement.
[0026] The beneficial effects of the present invention are as follows:
[0027] 1. The present invention provides a low-temperature sleeve grouting material for steel bar connection, which is composited with ordinary silicate cement, sulphoaluminate cement and high-alumina cement in a reasonable ratio and supplemented with modified silica fume and gypsum, and is further matched with antifreeze agent, phase change material, early strength agent, retarder, water reducer, early expansion agent and late expansion agent, so as to improve the strength development speed of the grouting material under low temperature environment conditions, ensure that the grouting material reaches the critical freezing strength as soon as possible, and at the same time ensure that the grouting material has good working performance and sufficient operation time, and has the characteristics of no shrinkage in the early stage and slight expansion in the late stage under low negative temperature conditions; in addition, the negative temperature hydration and hardening characteristics are improved, and it is suitable for sleeve grouting construction in an environment of -5-10℃ without taking heating and insulation measures, so as to solve the problem that the existing conventional grouting materials cannot be used due to insufficient strength caused by limited hydration under low temperature conditions.
[0028] 2. The present invention provides a method for preparing a low-temperature sleeve grouting material for steel bar connection. The raw materials are widely available, the preparation method is simple, and the construction is convenient. Grouting can be performed after directly adding water and stirring evenly on site. Ordinary Portland cement and sulphoaluminate cement are both grade 42.5, and the cost is relatively low. DETAILED DESCRIPTION
[0029] In order to better understand the content of the present invention, it is further described below in conjunction with examples, but the content of the present invention is not limited to the following embodiments.
[0030] In the following embodiments, the ordinary Portland cement is Yangfang PO 42.5, the sulfate cement is Yicheng Anda 42.5 grade R.SAC, the high alumina cement is Zhengzhou Jinghua CA50-Ⅱ, the gypsum is natural anhydrite, the fine aggregate is quartz sand (55% of the particle size is 1-3 mm, and 45% of the particle size is 0-1 mm), the early strength agent is commercially available lithium carbonate, the retarder is commercially available boric acid, the defoamer is German AGITAN brand powder defoamer P803, the water reducing agent is Xingbang Building Materials PC-1030, the expansion agent is a 1:1 composite of azodicarbonamide and calcium sulfoaluminate, the antifreeze agent is commercially available sodium nitrite, and the phase change material is produced by German Rubitherm Company PX.
[0031] In the following examples, the preparation of modified silica fume includes the following steps:
[0032] Soak 10g of silica ash in 100ml of 15% dilute hydrochloric acid for activation, take it out and dry it after 3 hours, then add it to 200ml of vinyl tri(β-methoxyethoxy)silane ethanol solution (containing 0.5g of vinyl tri(β-methoxyethoxy)silane) in a 50°C water bath, then heat it to 80°C for reaction for 5h, then add 1g of isopentanol polyoxyethylene ether, 30ml of hydrogen peroxide, and 100g of deionized water under a nitrogen environment for grafting reaction for 2h, and finally filter and separate to obtain the modified silica ash.
[0033] Example 1
[0034] A low-temperature sleeve grouting material for steel bar connection comprises the following components in parts by weight: 570 parts of ordinary silicate, 100 parts of sulphoaluminate cement, 200 parts of high-alumina cement, 40 parts of modified silica fume, 90 parts of gypsum, 1000 parts of fine aggregate, 0.5 parts of early strength agent, 2.5 parts of retarder, 0.4 parts of defoamer, 4.5 parts of water reducer, 0.2 parts of expansion agent, 2 parts of antifreeze agent and 2 parts of phase change material.
[0035] A method for preparing a low-temperature sleeve grouting material for steel bar connection comprises the following steps: weighing cement, admixture, fine aggregate, early strength agent, retarder, water reducer, defoamer, expansion agent, antifreeze agent and phase change material according to a formula, mixing and stirring evenly, adding water at a water-to-material ratio of 0.115 and stirring to obtain the low-temperature sleeve grouting material for steel bar connection.
[0036] Example 2
[0037] A low-temperature sleeve grouting material for steel bar connection comprises the following components in parts by weight: 520 parts of ordinary silicate, 200 parts of sulphoaluminate cement, 150 parts of high-alumina cement, 40 parts of modified silica fume, 90 parts of gypsum, 1000 parts of fine aggregate, 0.2 parts of early strength agent, 2.1 parts of retarder, 0.4 parts of defoamer, 4.5 parts of water reducer, 0.2 parts of expansion agent, 2 parts of antifreeze agent and 2 parts of phase change material.
[0038] A method for preparing a low-temperature sleeve grouting material for steel bar connection comprises the following steps: weighing cement, admixture, fine aggregate, early strength agent, retarder, water reducer, defoamer, expansion agent, antifreeze agent and phase change material according to a formula, mixing and stirring evenly, adding water at a water-to-material ratio of 0.115 and stirring to obtain the low-temperature sleeve grouting material for steel bar connection.
[0039] Example 3
[0040] A low-temperature sleeve grouting material for steel bar connection comprises the following components in parts by weight: 470 parts of ordinary silicate, 300 parts of sulphoaluminate cement, 100 parts of high-alumina cement, 40 parts of modified silica fume, 90 parts of gypsum, 1000 parts of fine aggregate, 0.4 parts of early strength agent, 1.9 parts of retarder, 0.4 parts of defoamer, 4.5 parts of water reducer, 0.2 parts of expansion agent, 2 parts of antifreeze agent and 2 parts of phase change material.
[0041] A method for preparing a low-temperature sleeve grouting material for steel bar connection comprises the following steps: weighing cement, admixture, fine aggregate, early strength agent, retarder, water reducer, defoamer, expansion agent, antifreeze agent and phase change material according to a formula, mixing and stirring evenly, adding water at a water-to-material ratio of 0.115 and stirring to obtain the low-temperature sleeve grouting material for steel bar connection.
[0042] Example 4
[0043] A low-temperature sleeve grouting material for steel bar connection comprises the following components in parts by weight: 420 parts of ordinary silicate, 400 parts of sulphoaluminate cement, 50 parts of high-alumina cement, 40 parts of modified silica fume, 90 parts of gypsum, 1000 parts of fine aggregate, 0.3 parts of early strength agent, 2.3 parts of retarder, 0.4 parts of defoamer, 4.5 parts of water reducer, 0.2 parts of expansion agent, 2 parts of antifreeze agent and 2 parts of phase change material.
[0044] A method for preparing a low-temperature sleeve grouting material for steel bar connection comprises the following steps: weighing cement, admixture, fine aggregate, early strength agent, retarder, water reducer, defoamer, expansion agent, antifreeze agent and phase change material according to a formula, mixing and stirring evenly, adding water at a water-to-material ratio of 0.115 and stirring to obtain the low-temperature sleeve grouting material for steel bar connection.
[0045] Example 5
[0046] A low-temperature sleeve grouting material for steel bar connection comprises the following components in parts by weight: 320 parts of ordinary silicate, 400 parts of sulphoaluminate cement, 150 parts of high-alumina cement, 40 parts of modified silica fume, 90 parts of gypsum, 1000 parts of fine aggregate, 0.4 parts of early strength agent, 2.5 parts of retarder, 0.4 parts of defoamer, 4.5 parts of water reducer, 0.2 parts of expansion agent, 2 parts of antifreeze agent and 2 parts of phase change material.
[0047] A method for preparing a low-temperature sleeve grouting material for steel bar connection comprises the following steps: weighing cement, admixture, fine aggregate, early strength agent, retarder, water reducer, defoamer, expansion agent, antifreeze agent and phase change material according to a formula, mixing and stirring evenly, adding water at a water-to-material ratio of 0.115 and stirring to obtain the low-temperature sleeve grouting material for steel bar connection.
[0048] Comparative Example 1
[0049] A low-temperature sleeve grouting material for steel bar connection comprises the following components in parts by weight: 160 parts of ordinary silicate, 640 parts of sulphoaluminate cement, 70 parts of high-alumina cement, 40 parts of modified silica fume, 90 parts of gypsum, 1000 parts of fine aggregate, 0.5 parts of early strength agent, 2.5 parts of retarder, 0.4 parts of defoamer, 4.5 parts of water reducer, 0.2 parts of expansion agent, 2 parts of antifreeze agent and 2 parts of phase change material.
[0050] A method for preparing a low-temperature sleeve grouting material for steel bar connection comprises the following steps: weighing cement, admixture, fine aggregate, early strength agent, retarder, water reducer, defoamer, expansion agent, antifreeze agent and phase change material according to a formula, mixing and stirring evenly, adding water at a water-to-material ratio of 0.115 and stirring to obtain the low-temperature sleeve grouting material for steel bar connection.
[0051] Comparative Example 2
[0052] A low-temperature sleeve grouting material for steel bar connection comprises the following components in parts by weight: 570 parts of ordinary silicate, 100 parts of sulphoaluminate cement, 200 parts of high-alumina cement, 40 parts of ordinary silica fume, 90 parts of gypsum, 1000 parts of fine aggregate, 0.5 parts of early strength agent, 2.5 parts of retarder, 0.4 parts of defoamer, 4.5 parts of water reducer, 0.2 parts of expansion agent, 2 parts of antifreeze agent and 2 parts of phase change material.
[0053] A method for preparing a low-temperature sleeve grouting material for steel bar connection comprises the following steps: weighing cement, admixture, fine aggregate, early strength agent, retarder, water reducer, defoamer, expansion agent, antifreeze agent and phase change material according to a formula, mixing and stirring evenly, adding water at a water-to-material ratio of 0.115 and stirring to obtain the low-temperature sleeve grouting material for steel bar connection.
[0054] The performance test results of the low-temperature sleeve grouting material for steel bar connection prepared in each embodiment are shown in the following table:
[0055] Table 1 Performance test results of various embodiments
[0056]
[0057]
[0058] Note: In the above table, -1d means curing at -5℃ for 1d, -3d means curing at -5℃ for 3d, and -7+21d means curing at -5℃ for 7d and then transferring to standard curing conditions for 21d.
[0059] It can be seen from Table 1 above that when the proportion of composite cement in Comparative Example 1 is not within the scope of the present invention, the strength of the sleeve grouting material is low and cannot meet the use requirements; when unmodified silica fume is used in Comparative Example 2, although the sleeve grouting material can meet the use requirements, its fluidity is low and the overall strength is not high; the low-temperature sleeve grouting material provided by the present invention has good performance, and all performance indicators meet or even far exceed the requirements of the JG / T408-2019 "Sleeve Grouting Material for Rebar Connection" standard, and is a high-performance sleeve grouting material with high fluidity, micro-expansion, fast early strength development and high later strength.
[0060] The embodiments described above are only preferred implementation modes of the present invention. It should be pointed out that all other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention belong to the protection scope of the present invention.
Claims
1. A low temperature sleeve grouting material for steel bar connection, characterized in that: By weight, it includes the following components: 800-1000 parts of cement, 10-50 parts of modified silica fume, 10-100 parts of gypsum, 900-1100 parts of fine aggregate, 0.1-0.5 parts of early strength agent, 1-3 parts of retarder, 2-5 parts of water reducer, 0.2-0.6 parts of defoamer, 0.1-0.5 parts of expansion agent, 1-5 parts of antifreeze agent, 1-5 parts of phase change material, water-to-cement ratio is 0.11-0.15; among which: The cement comprises 300-600 parts of ordinary Portland cement, 100-400 parts of sulphoaluminate cement and 50-200 parts of high-alumina cement; wherein the strength grade of ordinary Portland cement and sulphoaluminate cement is 42.5; The modified silica ash is obtained by surface-modifying silica ash with a silane coupling agent and then grafting an organic component on the surface; the silane coupling agent is vinyl tri(β-methoxyethoxy) silane, and the organic component is isopentanol polyoxyethylene ether; the specific steps are: immersing the silica ash in dilute hydrochloric acid for activation, taking it out and drying it after 2-4 hours, then adding it to a vinyl tri(β-methoxyethoxy) silane ethanol solution in a 50-60° C. water bath, then heating it to 70-90° C. for reaction for 4-6 hours, then adding isopentanol polyoxyethylene ether, hydrogen peroxide and deionized water in a nitrogen environment for grafting reaction for 1-3 hours, and finally filtering and separating to obtain the modified silica ash; wherein: the weight ratio of vinyl tri(β-methoxyethoxy) silane to silica ash is (2-6):100; the weight ratio of isopentanol polyoxyethylene ether to silica ash is (5-20):100; The expansion agent includes an early expansion agent and a late expansion agent.
2. The sleeve grouting material according to claim 1, characterized in that: The concentration of the dilute hydrochloric acid is 10%-15%.
3. The sleeve grouting material according to claim 1, characterized in that: The gypsum is anhydrite; the fine aggregate is at least one of washed and dried river sand, quartz sand, machine-made sand and corundum.
4. The sleeve grouting material according to claim 1, characterized in that: The early strength agent is at least one of lithium carbonate, lithium sulfate, lithium fluoride, lithium hydroxide and lithium fluoride; the retarder is at least one of sodium gluconate, tartaric acid, citric acid and boric acid; the water reducer is a dry powder polycarboxylic acid water reducer; and the defoamer is a dry powder organosilicon defoamer.
5. The sleeve grouting material according to claim 1, characterized in that: In the expansion agent, the mass ratio of the early expansion agent to the late expansion agent is (1-3):
1.
6. The sleeve grouting material according to claim 1, characterized in that: The early expansion agent is at least one of azo compounds, sulfonylhydrazide compounds and nitroso compounds; the late expansion agent is at least one of calcium oxide, calcium sulfoaluminate and magnesium oxide.
7. The sleeve grouting material according to claim 1, characterized in that: The antifreeze agent is at least one of sodium nitrate, sodium nitrite, calcium nitrite, potassium carbonate and calcium chloride; the phase change material is a high thermal conductivity nano-scale microcapsule phase change material with a particle size of 20-60 μm and a phase change temperature of 5-30°C.
8. A method for preparing the low-temperature sleeve grouting material for steel bar connection according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: cement, modified silica fume, gypsum, fine aggregate, early strength agent, retarder, water reducer, defoamer, expansion agent, antifreeze agent and phase change material are weighed according to the formula, mixed and stirred evenly, and then water is added at a water-to-material ratio of 0.11-0.15 to prepare low-temperature sleeve grouting material for steel bar connection.
Citation Information
Cited By
Low-temperature high-strength underwater non-dispersible grouting material
CN121990812A