A method for directly reducing iron concentrate by microwave-assisted gasification of discarded disposable medical masks
Through microwave-assisted gasification technology, disposable medical masks are mixed with iron-based catalysts, and microwave heating is used to generate high-content reducing gases, which solves the high energy consumption and high emission problems of traditional recycling methods and achieves low energy consumption and low emissions of iron concentrates. High-value recycling significantly reduces carbon emission pressure and has industrialization potential.
Patent Information
- Application Number
- CN202211667108.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-22
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-12-22
AI Technical Summary
It is difficult to effectively recycle disposable medical masks with existing technology. The traditional incineration method consumes high energy and high emissions, and it is difficult to achieve low energy consumption, low emissions and high value recovery of iron concentrate.
The microwave-assisted gasification method is used to mix disposable masks with iron-based catalysts, prepare bimetallic catalysts through microwave combustion methods, and use microwave heating to convert the masks into high-content reducing gases, which can be used to directly reduce iron concentrates and reduce CO2 emissions. And increase the calorific value of pyrolysis gas.
It has achieved high-value recycling of disposable medical masks with low energy consumption and low emissions. It generates high-quality reducing gas through microwave gasification and quickly reduces iron concentrate pellets into sponge iron, reducing the carbon emission pressure of steel companies. It has significant prospects for industrialization.
Smart Images

Figure CN115874004B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of microwave catalytic pyrolysis and iron and steel metallurgy, and in particular to a method for directly reducing iron concentrate by using microwave-assisted gasification of discarded disposable medical masks. Background Art
[0002] According to estimates by the World Health Organization, at least 129 billion disposable medical masks were produced worldwide in 2020 alone. The heterogeneity of disposable medical masks makes it difficult to establish a reliable recycling platform. In fact, disposable medical masks are made of polypropylene, polyurethane, polyethylene terephthalate, etc. Although recycling disposable medical masks is the best disposal option, this method has not been promoted due to the difficulty in proper separation and high biological hazards. In these cases, thermal treatment provides a reliable disposal method for discarded disposable medical masks. In the thermal treatment process, incineration is one of the most common methods for recycling plastic waste such as masks, but with the intensification of global carbon emission pressure, there is an urgent need to find a low-emission, low-energy, and high-value recycling method.
[0003] Gasification provides an effective recycling method for discarded disposable medical masks through carbon and hydrogen rearrangement. However, the traditional gasification recovery process requires a high temperature of more than 500°C, and the gasification product is mainly pyrolysis oil, which has many types and low added value. Therefore, it is urgent to find a low-emission, low-energy consumption and high-value recycling method for discarded disposable medical masks. Summary of the invention
[0004] The purpose of the present invention is to provide a method for directly reducing iron concentrate by microwave-assisted gasification of discarded disposable medical masks, so as to solve the problems existing in the above-mentioned prior art, and realize gas-based direct reduction of iron concentrate while recycling discarded disposable medical masks with low emissions and low energy consumption.
[0005] To achieve the above object, the present invention provides the following solutions:
[0006] One of the technical solutions of the present invention is a method for gasifying a disposable mask into a reducing gas, comprising the following steps:
[0007] The disposable mask is mixed with an iron-based catalyst and subjected to microwave gasification reaction to obtain a reducing gas; the H2 content in the reducing gas is close to 70 vol.%, the CO content exceeds 20 vol.%, and the C 2+ The content is less than 5 vol.%;
[0008] The chemical formula of the iron-based catalyst is Fe a Y b Al c O d; Wherein, a=0.1-1, b=0.5-1, c=a+b, d=1.5(a+b+c), Y represents Co or Ni;
[0009] Co or Ni has better dehydrogenation ability than other metals, therefore, the present invention limits the second phase metal Y to Co or Ni.
[0010] Furthermore, the preparation method of the iron-based catalyst comprises the following steps:
[0011] It is prepared by microwave combustion method with urea as fuel, aluminum nitrate as carrier, iron nitrate and Y salt as metal sources;
[0012] The Y salt is cobalt nitrate or nickel nitrate.
[0013] The molar ratio of urea, aluminum nitrate, iron nitrate and Y salt is A:B:C:D, wherein A=(15B+15C+10D) / 6; B=C+D; C=0.1-1; D=0.5-1.
[0014] The ratio of the Y salt to Fe in the synthesized catalyst must be greater than 0.5, otherwise the synthesized catalyst has a low microwave absorption capacity and cannot initiate microwave pyrolysis of DMMs at room temperature.
[0015] The microwave combustion process for preparing the iron-based catalyst is to dissolve urea, aluminum nitrate, iron nitrate and Y salt in an aqueous solution and then heat them in a microwave field until a combustion reaction occurs to obtain the iron-based catalyst.
[0016] Furthermore, the mass ratio of the disposable mask to the iron-based catalyst is 1:0.3-1; the microwave gasification reaction is specifically: passing 50-200 mLmin -1 The nitrogen containing CO2 is used as the purge gas, and the reaction is carried out for 15-30 minutes at a power of 500-2000 W. The purpose of introducing nitrogen rich in CO2 is to convert CO2 waste gas into CO, olefins or alkanes through an iron-based catalyst in a microwave field during the synthesis process, thereby reducing CO2 emissions and increasing the calorific value of the pyrolysis gas.
[0017] Furthermore, the volume ratio of CO2 to nitrogen in the nitrogen containing CO2 is 0-1:1.
[0018] Furthermore, the disposable mask is disinfected and broken into pieces of 1-5 mm before being mixed with the iron-based catalyst.
[0019] The second technical solution of the present invention is a method for directly reducing iron concentrate by microwave-assisted gasification of discarded disposable medical masks, comprising the following steps: using the above method of gasifying disposable masks into reducing gas to prepare reducing gas at a rate of 100-800 mL min-1 The reducing gas is continuously introduced into a container containing iron concentrate at a rate of 1000 to perform gas-based direct reduction to obtain metallic iron. If the flow rate of the reducing gas is lower than the parameter range recorded above, it will affect the metallization rate of the direct-reduced iron and increase the cost of subsequent electric furnace refining.
[0020] Furthermore, the temperature of the gas-based direct reduction is 800-1100°C and the time is 0.5-2h. The temperature and time of the gas-based direct reduction below the above-mentioned range will affect the metallization rate of the direct-reduced iron.
[0021] Furthermore, before the reducing gas is introduced into the container containing the iron ore concentrate, CO2 in the reducing gas is removed.
[0022] The CO2 in the reducing gas is removed by absorption through the CO2 wash bottle.
[0023] Technical concept of the present invention:
[0024] Microwave heating is a clean and efficient heating method. By constructing a suitable microwave gasification catalyst, discarded disposable medical masks can be selectively converted into high-content reducing gas, which can be used as a substitute for coke in steel production in the metallurgical field. While alleviating the CO2 emission pressure of steel companies to prepare sponge iron, it can also achieve high-value recycling of discarded disposable medical masks.
[0025] Since the oxygen vacancies and lattice defects that appear during the formation of the bimetallic catalyst enhance the microwave absorption capacity of the iron-based catalyst, the waste disposable masks can be microwave-assisted gasified into oil-less and gas-rich gasification products in a short time, wherein the content of reducing gas in the non-condensable gas exceeds 90 vol.%, and the iron ore pellets can be directly reduced to sponge iron. The method of the present invention not only realizes the high-value utilization of waste disposable medical masks, but also can alleviate the pressure of carbon emissions of steel enterprises, and has significant industrial prospects.
[0026] The present invention discloses the following technical effects:
[0027] The present invention aims at the problems of high cost, wide distribution of products, low added value and high carbon emission pressure in steel production in the existing waste plastic pyrolysis recovery process, and proposes a method for directly reducing iron concentrate by microwave-assisted gasification of discarded disposable medical masks. The present invention mainly constructs a suitable bimetallic iron-based catalyst, utilizes the unique hot spot heating mechanism of microwaves to enhance interfacial mass transfer, and quickly gasifies the discarded disposable medical masks with poor microwave absorption capacity into high-quality reducing gas by microwaves, and basically does not produce condensable liquid. At the same time, the method can also use greenhouse gas CO2 as a purge gas to catalytically convert it into carbon-containing gases such as CO. The reducing gas generated by the gasification of discarded disposable medical masks can quickly reduce iron concentrate pellets to sponge iron, which has significant industrialization potential.
[0028] The method of the invention has simple equipment requirements and low energy consumption, and is easy to realize a continuous and large-scale operation mode. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1 The microwave heating conditions in the microwave gasification reactor after the catalyst is mixed with the discarded disposable medical mask in Examples 1 and 2 and Comparative Example 1;
[0031] Figure 2 The XRD patterns of the iron concentrates before and after reduction in Examples 1 and 2 are shown. DETAILED DESCRIPTION
[0032] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0033] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0034] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0035] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0036] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0037] Unless otherwise specified, the "parts" described in the present invention are all based on mass parts.
[0038] The FeCoAl2O6 catalyst used in the embodiment of the present invention uses urea as fuel, aluminum nitrate as carrier, ferric nitrate and cobalt nitrate as metal sources, and is prepared by microwave combustion method. The specific steps are as follows: 0.1M ferric nitrate, 0.1M cobalt nitrate, 0.2M aluminum nitrate and 0.92M urea are mixed and dissolved in water, and then reacted in a 2000W microwave field for 10 minutes to obtain a FeCoAl2O6 catalyst.
[0039] The FeNiAlO6 catalyst used in the embodiment of the present invention uses urea as fuel, aluminum nitrate as carrier, ferric nitrate and nickel nitrate as metal sources, and is prepared by microwave combustion method. The specific steps are as follows: 0.1M ferric nitrate, 0.1M nickel nitrate, 0.2M aluminum nitrate and 0.92M urea are mixed and dissolved in water, and then reacted in a 2000W microwave field for 10 minutes to obtain a FeNiAl2O6 catalyst.
[0040] The FeAlO3 catalyst used in the embodiment of the present invention uses urea as fuel, aluminum nitrate as carrier, and ferric nitrate as metal source, and is prepared by microwave combustion method. The specific steps are as follows: 0.1M ferric nitrate, 0.1M aluminum nitrate and 0.67M urea are mixed and dissolved in water, and then reacted in a 2000W microwave field for 10 minutes to obtain a FeAlO3 catalyst.
[0041] Example 1
[0042] Step 1: Disinfect the used disposable medical masks and break them into 1-5mm pieces.
[0043] Step 2: Mix the broken disposable medical masks and FeCoAl2O6 catalyst in a mass ratio of 1:1, place them in a 1000 W microwave gasification reactor, and introduce 100 mL min -1 Nitrogen containing 50 vol.% CO2 was used as the purge gas. The microwave reaction was started for 15 min to obtain high-quality reducing gas.
[0044] Step 3: The CO2 in the reducing gas prepared in step 2 is absorbed by the CO2 washing bottle and then washed at a rate of 500 mL min -1 The iron ore concentrate is reduced to sponge iron (Fe-FeCoAl2O6) by continuously passing it into a furnace at 1000°C at a rate of 1.5 and keeping it warm for 1 hour.
[0045] In this embodiment, the microwave heating conditions of FeCoAl2O6 catalyst mixed with waste disposable medical masks (FeCoAl2O6+M) in the microwave gasification reactor are as follows: Figure 1 shown.
[0046] The XRD patterns of the iron concentrate before and after the reduction of the iron concentrate by the reducing gas generated by gasification are as follows: Figure 2 shown.
[0047] In this embodiment, after the disposable medical mask is subjected to microwave gasification, the yield of non-condensable gas is 77.65 wt.%, of which the content of CO and H2 exceeds 95 vol.%, and the distribution of the microwave gasification products is specifically shown in Table 1.
[0048] Comparative Example 1
[0049] The only difference from Example 1 is that the FeCoAl2O6 catalyst is replaced by a FeAlO3 catalyst.
[0050] In this comparative example, the microwave heating conditions of FeAlO3 catalyst mixed with waste disposable medical masks (FeAlO3+M) in the microwave gasification reactor are as follows: Figure 1 As shown. Figure 1 It can be seen that the mixture of FeAlO3 catalyst and disposable medical mask can be heated to 175°C in 10 minutes, while the mixture of Co-doped bimetallic catalyst FeCoAl2O6 and disposable medical mask can be quickly heated to about 900°C in 13 minutes, with an average heating rate of 59°C min -1 .
[0051] Example 2
[0052] Step 1: Disinfect the used disposable medical masks and break them into 1-5mm pieces.
[0053] Step 2: Mix the broken disposable medical masks and FeNiAl2O6 catalyst in a mass ratio of 1:1, place them in a 1000 W microwave gasification reactor, and introduce 100 mL min -1 Nitrogen containing 50 vol.% CO2 was used as the purge gas. After the microwave reaction was started for 20 min, high-quality reducing gas was obtained.
[0054] Step 3: The CO2 in the reducing gas is absorbed by the CO2 washing bottle and then washed at 500 mL min -1 The iron ore concentrate is reduced to sponge iron (Fe-FeNiAl2O6) by continuously passing it into a furnace at 1000°C at a rate of 1.5 and keeping it warm for 1 hour.
[0055] In this embodiment, the microwave heating conditions of FeNiAl2O6 catalyst mixed with waste disposable medical masks (FeNiAl2O6+M) in the microwave gasification reactor are as follows: Figure 1 As shown. Figure 1 It can be seen that the microwave heating conditions of FeNiAl2O6 catalyst and FeCoAl2O6 catalyst are similar. The XRD patterns before and after the iron concentrate is reduced by the reducing gas generated by gasification in this embodiment are as follows: Figure 2 As shown. Figure 2 It can be seen that after reduction, the iron in the iron concentrate mainly exists in the form of metallic iron, and its metallization rate is as high as over 90%.
[0056] In this embodiment, after the disposable medical mask is subjected to microwave gasification, the yield of non-condensable gas is 77.21 wt.%, of which the content of CO and H2 exceeds 95 vol.%, and the distribution of the microwave gasification products is specifically shown in Table 1.
[0057] Table 1 Product distribution of microwave-assisted gasification of DMMs over iron-based catalysts
[0058]
[0059] Example 3
[0060] Step 1: Disinfect the used disposable medical masks and break them into 1-5mm pieces.
[0061] Step 2: Mix the broken disposable medical masks and FeCoAl2O6 catalyst in a mass ratio of 1:1, place them in a 1000 W microwave gasification reactor, and introduce 200 mL min -1 Nitrogen containing 10 vol.% CO2 was used as the purge gas. The microwave reaction was started for 14 min to obtain high-quality reducing gas.
[0062] Step 3: The CO2 in the reducing gas is absorbed by the CO2 washing bottle and then washed at 100 mL min -1 The iron ore concentrate pellets were reduced to sponge iron at a rate of 92.8%.
[0063] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. A method for gasifying a disposable mask into a reducing gas, characterized in that: The following steps are involved: The disposable mask is mixed with an iron-based catalyst and subjected to microwave gasification reaction to obtain a reducing gas; The chemical formula of the iron-based catalyst is Fe a Y b Al c O d ; Wherein, a=0.1-1, b=0.5-1, c=a+b, d=1.5(a+b+c), and Y represents Co or Ni; The preparation method of the iron-based catalyst comprises the following steps: The method is prepared by microwave combustion method using urea as fuel, aluminum nitrate as carrier, iron nitrate and Y salt as metal sources; the Y salt is cobalt nitrate or nickel nitrate; The mass ratio of the disposable mask to the iron-based catalyst is 1:0.3-1; the microwave gasification reaction is specifically: passing 50-200mLmin -1 Nitrogen containing CO2 is used as the purge gas and the reaction is carried out for 15-30 minutes at a power of 500-2000W.
2. The method for gasifying a disposable mask into a reducing gas according to claim 1, characterized in that: The disposable mask is disinfected and broken into pieces of 1-5 mm before being mixed with the iron-based catalyst.
3. A method for directly reducing iron concentrate by microwave-assisted gasification of discarded disposable medical masks, characterized in that: The method comprises the following steps: using the reducing gas prepared by the method for gasifying a disposable mask into reducing gas according to claim 1 at a rate of 100-800 mL / min -1 The gas is continuously introduced into a container containing iron concentrate at a rate of 1.5 to 2.5 % for gas-based direct reduction to obtain metallic iron.
4. The method for directly reducing iron concentrate by microwave-assisted gasification of discarded disposable medical masks according to claim 3, characterized in that: The temperature of the gas-based direct reduction is 800-1100° C., and the time is 0.5-2 h.
5. The method for directly reducing iron concentrate by microwave-assisted gasification of discarded disposable medical masks according to claim 3, characterized in that: Before the reducing gas is introduced into the container containing the iron ore concentrate, CO2 in the reducing gas is removed.