Weakly confined semiconductor nanocrystals, preparation method and application thereof

Through the reaction of cationic precursors and fatty acids and the subsequent growth of anionic precursors, weakly confined semiconductor nanocrystals with a size larger than the exciton diameter are prepared, which solves the problem of difficulty in synthesizing large-sized monodisperse nanocrystals in the existing technology and realizes nano The unique optical properties and high quantum yield of the crystal expand its application potential.

CN115893474BActive Publication Date: 2024-10-22ZHEJIANG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211363622.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-09-05
Filing Date
2022-11-02
Publication Date
2024-10-22
Estimated Expiration
2042-11-02

AI Technical Summary

Technical Problem

It is difficult to effectively synthesize and control weakly localized semiconductor nanocrystals, especially large-sized monodispersed nanocrystals of groups II-IV and III-V, with existing technology, resulting in insufficient understanding of their properties and limited applications.

Method used

Nanocrystal seeds are synthesized by reacting cationic precursors with fatty acids, and then grown by adding anionic precursors and fatty acyl chlorides to prepare weakly confined semiconductor nanocrystals with a size larger than the exciton diameter. Dynamic exciton characteristics are used to achieve unique optics and optoelectronics. nature.

Benefits of technology

Weakly confined semiconductor nanocrystals with a size larger than the exciton diameter have been successfully prepared, exhibiting bimodal fluorescence, quasi-continuous absorption spectrum and high biexciton fluorescence quantum yield, and are suitable for applications such as lighting, photovoltaics and quantum light sources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115893474B_ABST
    Figure CN115893474B_ABST
Patent Text Reader

Abstract

The present invention discloses a weakly confined semiconductor nanocrystal, a preparation method thereof and an application thereof, wherein the size of the nanocrystal is larger than the diameter of its exciton, the exciton of the nanocrystal is a dynamic exciton, the electron-hole Coulomb interaction of the dynamic exciton is not enough to bind each other to become a stable combined exciton at the operating temperature, and the electron and hole of the dynamic exciton are constrained by the boundary of the nanocrystal. Since the exciton of the weakly confined nanocrystal of the present application has the characteristics of a dynamic exciton, the nanocrystal of the present application has unique optical and photoelectric properties different from conventional semiconductor nanomaterials. For example, the band edge energy level density of the electron (or hole) of the dynamic exciton is high and the energy gap within the band is small, which leads to a rare room temperature double peak steady-state luminescence, which has unique value for applications (such as lighting) that require wide-band luminescence. For another example, the electron (or hole) wave functions of the dynamic exciton are not strongly constrained to each other and are rapidly weakened with increasing temperature, which is conducive to electron-hole transfer, which is of great significance for photovoltaic solar devices, photodetectors, and photocatalysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor nanocrystals, and in particular to a weakly confined semiconductor nanocrystal, a preparation method thereof and an application thereof. Background Art

[0002] Since the rise of semiconductor nanomaterials, the development of their synthetic chemistry has always been one of the core topics. After decades of development, the synthesis of strongly confined semiconductor nanomaterials has made significant progress in morphology control, crystal control, size control, etc., not only the size and morphology are monodisperse, but also the optical properties are monodisperse: the fluorescence quantum yield reaches 100%, the fluorescence lifetime decays exponentially, the fluorescence is flicker-free, and the fluorescence peak width of the aggregate is consistent with the peak width of a single particle. However, for traditional II-VI and III-V groups, most of the current research focuses on strongly confined small-sized semiconductor nanomaterials, and the synthesis system of monodisperse small-sized semiconductor nanocrystals has been continuously improved, while the controllable synthesis of monodisperse weakly confined large-sized semiconductor nanomaterials is difficult to achieve.

[0003] In bulk semiconductors, excitons are pairs of electrons and holes that are bound together by strong Coulomb interactions and are generated when the semiconductor absorbs a photon. In addition, electron-hole pairs can also be generated by electrical injection, and as long as the Coulomb interaction between electron-hole pairs significantly exceeds the thermal energy at a given temperature (about 25 meV at room temperature), the electron-hole pairs generated by electrical excitation in the semiconductor will also form excitons.

[0004] Semiconductor nanocrystals with geometric dimensions larger than the diameter of bulk semiconductor excitons are called weakly confined semiconductor nanocrystals. Monodisperse II-IV and III-V weakly confined semiconductor nanocrystals have not been reported so far. Due to the inability to obtain high-quality samples, little is known about the properties of weakly confined semiconductor nanocrystals.

[0005] In the open literature, the representative of weakly confined nanocrystals is cuprous chloride (CuCl) nanocrystals, rather than the common stable II-IV and III-V semiconductor nanocrystals. At present, the theoretical model of weakly confined semiconductor nanocrystals is also based on experimental facts related to CuCl. Specifically, since the exciton binding energy of CuCl is very large (~233meV) and the exciton diameter is less than 1nm, the excitons in the cuprous chloride nanocrystals can exist stably at room temperature without ionizing into free electrons and holes (called free carriers). Therefore, after the CuCl nanocrystals are excited, their electronic structure will show typical Wannier excitons (hydrogen-like exciton energy levels) and the quantum confinement kinetic energy of the exciton mass center, rather than being determined by the quantum confinement kinetic energy of the electrons and holes respectively.

[0006] In recent years, people have begun to study another type of metal halide nanocrystals: cesium lead halide perovskite (such as CsPbI3) nanocrystals. Due to the small exciton diameter and the poor controllability of ionic lattice growth, the resulting nanocrystals are generally larger than their exciton diameter and can be classified as weakly confined semiconductor nanocrystals. However, cesium lead halide perovskite nanocrystals are ionic lattices with poor chemical, optical and electrical stability. The unique properties of weakly confined semiconductor nanocrystals revealed so far are limited, and their practicality is very challenging. Summary of the invention

[0007] An object of the present invention is to provide a weakly confined semiconductor nanocrystal, a preparation method thereof and an application thereof.

[0008] To achieve the above purpose, the present invention provides a weakly confined semiconductor nanocrystal, wherein the size of the nanocrystal is larger than the diameter of its exciton, the size of the nanocrystal is the average value of its diameter or the average value of its centroid length, the exciton of the nanocrystal is a dynamic exciton, at the operating temperature, the electron-hole Coulomb interaction of the dynamic exciton is not sufficient to bind each other to form a stable combined exciton, the electrons and holes of the dynamic exciton are constrained by the boundary of the nanocrystal, and the operating temperature includes room temperature.

[0009] According to another aspect of the present application, the present invention provides a weakly confined semiconductor nanocrystal, wherein the size of the nanocrystal is larger than its exciton diameter, the size of the nanocrystal is the average value of its diameter or the average value of its center of mass length, and under room temperature test conditions, the ultraviolet-visible absorption spectrum of the nanocrystal exhibits quasi-continuous band absorption.

[0010] According to another aspect of the present application, the present invention provides a weakly confined semiconductor nanocrystal, the size of the nanocrystal is larger than its exciton diameter, the size of the nanocrystal is the average value of its diameter or the average value of its center of mass length, and under room temperature testing conditions, the fluorescence spectrum of the nanocrystal has an asymmetric characteristic of tailing to high energy.

[0011] According to another aspect of the present application, the present invention provides a weakly confined semiconductor nanocrystal, the size of the nanocrystal is larger than its exciton diameter, the size of the nanocrystal is the average value of its diameter or the average value of its center of mass length, and under room temperature test conditions, the double Gaussian fitting results of the fluorescence emission spectrum of the nanocrystal show that: the fluorescence emission spectrum of the nanocrystal contains two fluorescence emission peaks with different energies, that is, the nanocrystal has a dual-level emission fluorescence property.

[0012] According to another aspect of the present application, the present invention provides a weakly confined semiconductor nanocrystal, wherein the size of the nanocrystal is larger than its exciton diameter, the size of the nanocrystal is the average value of its diameter or the average value of its center of mass length, and the biexciton fluorescence quantum yield of the nanocrystal is not less than 50%.

[0013] Furthermore, the biexciton fluorescence quantum yield of the nanocrystal is not less than 70%, preferably not less than 80%, more preferably not less than 90%, and more preferably not less than 95%.

[0014] Furthermore, the size of the nanocrystal is 1 to 20 times the diameter of its exciton. Preferably, the size of the nanocrystal is 1 to 6 times the diameter of its exciton.

[0015] Furthermore, the size of the nanocrystal is greater than 10 nm, preferably greater than 15 nm, preferably greater than 20 nm, more preferably greater than 25 nm, and more preferably greater than or equal to 30 nm.

[0016] Furthermore, the relative standard deviation of the size distribution of the nanocrystals does not exceed 10%, preferably does not exceed 6%, preferably does not exceed 5%, preferably does not exceed 4%, and more preferably does not exceed 3%.

[0017] Furthermore, the nanocrystal is a core-structured nanocrystal or a core-shell-structured nanocrystal.

[0018] Furthermore, the nanocrystal is a cubic nanocrystal, and a transmission electron microscope photograph shows that the nanocrystal has a square two-dimensional projection, and a high-resolution transmission electron microscope photograph shows that the nanocrystal has single-period non-dislocated lattice fringes and atomically smooth boundaries.

[0019] Furthermore, the nanocrystal is CdS or CdSe or CdSe / CdS core / shell cubic nanocrystal, the size of the CdSe core in the CdSe / CdS core / shell cubic nanocrystal is 6nm-25nm, and the number of CdS shell layers is 1-20 monolayers.

[0020] Furthermore, the nanocrystal is a II-IV semiconductor or a III-V semiconductor.

[0021] Furthermore, the nanocrystal is a sphalerite single crystal structure.

[0022] Furthermore, the excitation spectra of the nanocrystals at different fluorescence emission positions substantially overlap.

[0023] Furthermore, the fluorescence emission peak position of the nanocrystal is substantially consistent with the band gap width of its bulk material.

[0024] Furthermore, the fluorescence half-peak width of the nanocrystal is greater than 70 meV.

[0025] Furthermore, the single particle fluorescence corresponding to the nanocrystal has no fluorescence flickering for at least 1000 seconds.

[0026] The present application also provides a method for preparing semiconductor nanocrystals, comprising the following steps:

[0027] Synthesis of nanocrystal seeds: a cationic precursor reacts with a first fatty acid at a first temperature, and then a first anionic precursor is added to react to obtain nanocrystal seeds, wherein the size of the nanocrystal seeds is smaller than the exciton diameter thereof, and the size of the nanocrystal seeds is the average value of the diameter thereof or the average value of the length passing through the center of mass thereof;

[0028] Growth of nanocrystals: a cationic precursor, a first fatty acid, a second fatty acid and a fatty acid chloride react at a second temperature, and then the nanocrystal seeds and a second anionic precursor are added in sequence for growth to obtain nanocrystals, wherein the size of the nanocrystals is not less than the exciton diameter thereof, and the size of the nanocrystals is the average value of their diameters or the average value of their center of mass lengths.

[0029] Furthermore, the cation precursor is cadmium carboxylate, and the first anion precursor is a Se precursor or a S precursor.

[0030] Furthermore, the first fatty acid is a fatty acid having no less than 10 carbon atoms, preferably, a fatty acid having no more than 18 carbon atoms.

[0031] Furthermore, the second fatty acid is a fatty acid having no less than 22 carbon atoms.

[0032] The weakly confined semiconductor nanocrystals are used for lighting or display, or for photovoltaic solar devices, or for photoelectric detectors, or for lasers, or for quantum light sources, or for photochemical catalysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The upper part is the synthesis scheme of large-sized CdE (CdSe, CdS, CdSe / CdS core-shell) cubic nanocrystals; the lower part is the corresponding TEM photo of 30nm CdSe cubic nanocrystals.

[0034] Figure 2 Characterization results of 21nm CdSe cubic nanocrystals: large-scale TEM photos (a), HRTEM photos (b, c) and their corresponding FFT photos (d), XRD spectra (e), normalized fluorescence excitation spectra at different emission positions (f), and normalized UV-visible absorption and fluorescence emission spectra (g). The inset in the TEM photo in (a) is the statistical result of the size distribution of the nanocrystals.

[0035] Figure 3Characterization results of 21nm CdS cubic nanocrystals: large-range TEM photos (a), HRTEM photos (b, c) and their corresponding FFT photos (d), XRD spectra (e), normalized fluorescence excitation spectra at different emission positions (f), and normalized UV-visible absorption and fluorescence emission spectra (g). The inset in the TEM photo in (a) is the statistical result of the size distribution of the nanocrystals.

[0036] Figure 4 The characterization results corresponding to 20nm CdSe8 / CdS core-shell cubic nanocrystals: (a) TEM photo, the inset is the statistical result of the size distribution of the nanocrystals; (b) element distribution diagram under STEM; (c, d) HRTEM photos at different magnifications; (e) corresponding FFT photo; (f) XRD spectrum; (g) normalized fluorescence excitation spectrum at different emission positions; (h) normalized UV-visible absorption and fluorescence emission spectra.

[0037] Figure 5 The characterization results corresponding to 22nm CdSe12 / CdS core-shell cubic nanocrystals: (a) TEM photo, the inset is the statistical result of the size distribution of the nanocrystals; (b) element distribution diagram under STEM; (c, d) HRTEM photos at different magnifications; (e) corresponding FFT photo; (f) XRD spectrum; (g) normalized fluorescence excitation spectrum at different emission positions; (h) normalized UV-visible absorption and fluorescence emission spectra.

[0038] Figure 6 Comparison of optical properties of CdSe cubic nanocrystals of different sizes: (a) normalized UV-visible absorption spectrum / fluorescence emission spectrum, (b) fluorescence emission peak position, (c) fluorescence half-peak width FWHM, (d) fluorescence peak skewness. The inset in (b) is the fluorescence spectrum corresponding to 12nm CdSe cubic nanocrystal, and the triangle data in (c) is the fluorescence half-peak width of single zinc blende CdSe nanocrystal particles reported in the literature.

[0039] Figure 7 Comparison of the optical properties of CdS cubic nanocrystals of different sizes: (a) normalized UV-visible absorption spectrum / fluorescence emission spectrum, (b) fluorescence emission peak position, (c) fluorescence half-maximum width FWHM, and (d) fluorescence peak skewness.

[0040] Figure 8 The normalized UV-visible absorption spectrum (a), fluorescence emission spectrum (b), transient fluorescence spectrum (c), fluorescence emission peak position and fluorescence quantum yield (d), fluorescence peak skewness and fluorescence half-maximum width FWHM (e), and fluorescence lifetime and goodness of fit (f) of CdSe8 / CdS cubic nanocrystals vary with the thickness of the CdS shell.

[0041] Fig. 9 The normalized UV-visible absorption spectrum (a), fluorescence emission spectrum (b), transient fluorescence spectrum (c), fluorescence emission peak position (d), fluorescence peak skewness and fluorescence half-maximum width FWHM (e), and fluorescence lifetime and goodness of fit (f) of CdSe12 / CdS cubic nanocrystals are plotted as a function of CdS shell thickness (ML). The inset in d is the fluorescence spectrum of the aggregate (dark line) and single particle (light line) of CdSe12 / 20CdS cubic nanocrystals.

[0042] Fig.10 The power-dependent fluorescence emission spectrum corresponding to 15 nm CdSe cubic nanocrystals (a) and the variation of fluorescence intensity with excitation power (b), where the inset in (a) is its power-dependent normalized fluorescence emission spectrum.

[0043] Fig.11 Figure 2 shows the power-dependent fluorescence emission spectrum of CdSe8 / 20CdS cubic nanocrystals (a) and the variation of fluorescence intensity with excitation power (b). The inset in (a) is the power-dependent normalized fluorescence emission spectrum, (c) the fluorescence emission spectrum of CdSe8 / 20CdS cubic nanocrystal aggregates and single particles after the fluorescence center peak position and fluorescence intensity are normalized, (d) upper figure: fluorescence emission spectrum of CdSe8 / 20CdS cubic nanocrystals and the result of double Gaussian fitting, lower figure: transient fluorescence spectrum of CdSe8 / 20CdS cubic nanocrystals at different emission positions.

[0044] Fig.12 The corresponding fluorescence lifetime (a) and the corresponding relative change rate of fluorescence lifetime (b) of CdSex / yCdS cubic nanocrystals change with temperature.

[0045] Fig.13 The single-particle fluorescence intensity of CdSe8 / 20CdS and CdSe12 / 20CdS cubic nanocrystals changes with time (a, c) and the corresponding single-particle photon second-order correlation curve and g0 (2) Values ​​(b, d). DETAILED DESCRIPTION

[0046] The present invention is further described below in conjunction with specific implementation methods. It should be noted that, under the premise of no conflict, the various embodiments or technical features described below can be arbitrarily combined to form a new embodiment.

[0047] For clarity, the term "substantially" or "approximately" is used herein to imply the possibility of variation in a numerical value within an acceptable range known to those skilled in the art. According to one example, the terms "substantially" or "approximately" as used herein should be interpreted as implying a possible variation of up to 10% above or below any specified value. According to another example, the terms "substantially" or "approximately" as used herein should be interpreted as implying a possible variation of up to 5% above or below any specified value. According to another example, the terms "substantially" or "approximately" as used herein should be interpreted as implying a possible variation of up to 2.5% above or below any specified value.

[0048] The present application provides a weakly confined semiconductor nanocrystal, wherein the size of the nanocrystal is larger than its exciton diameter, the exciton of the nanocrystal is a dynamic exciton, the electron-hole Coulomb interaction of the dynamic exciton is insufficient to bind each other to form a stable combined exciton at the operating temperature, and the electrons and holes of the dynamic exciton are constrained by the boundary of the nanocrystal. The aforementioned operating temperature includes room temperature. In some embodiments, the aforementioned operating temperature is not lower than room temperature.

[0049] In the present application, the size of the nanocrystal is larger than its exciton diameter, that is, it is a weakly confined semiconductor nanocrystal. The "size of the nanocrystal" mentioned in the present application refers to the diameter of the nanocrystal or the average value of the length through the center of mass.

[0050] When a semiconductor material is excited by energy greater than its band gap, the valence band electrons are excited to the conduction band, and a hole is generated in the valence band. The Coulomb interaction between the electron and the hole causes the two to form an electron-hole pair similar to the structure of a hydrogen atom in a certain space, also known as an "exciton". The size of the exciton can be described by the exciton Bohr radius. The "exciton diameter" mentioned in this application is twice the exciton Bohr radius. The exciton radius of bulk semiconductor materials is a fixed value. For example, the exciton Bohr radius of CdS is 2.8nm (that is, the exciton diameter is 5.6nm), and the exciton Bohr radius of CdSe is 5.6nm (that is, the exciton diameter is 11.2nm).

[0051] The present application mainly uses spectral methods to study the electronic structure of the nanocrystals, and then determines the energy level structure of the nanocrystals. Experiments show that the exciton energy level structure based on CuCl is not suitable for the nanocrystals of the present application under normal temperature conditions. Taking the nanocrystals of II-IV and III-V as an example, the binding energy of their excitons is very small, and the excitons in the weakly confined nanocrystals at common temperatures cannot exist stably, but are in an ionized state. However, the ionized electrons and holes are constrained by the boundaries of the nanocrystals, and do not obviously overflow into the ambient medium outside the nanocrystals, which causes the kinetic energy of the ionized electrons and holes to be determined by the size of the boundaries and significantly greater than the exciton binding energy of the bulk semiconductor. The overall result is that such an energy level structure does not meet the weakly confined nanocrystal model based on CuCl suggested in the literature, but is mainly determined by the confined kinetic energy of free electrons and holes, and the electron-hole Coulomb interaction caused by spatial confinement is suitable for calculation as a perturbation term.

[0052] Generally, excitons in solids can be divided into two categories: the first category is bound excitons or Frenkel excitons. In materials with small dielectric constants, such as ionic crystals, excited electrons and holes are tightly bound together in the same or nearest unit cell. The typical binding energy of this type of exciton is 0.1 to 1 eV. The second category is Wannier excitons. In materials with larger dielectric constants, the electric field shielding within the crystal reduces the Coulomb interaction between electrons and holes, resulting in an exciton radius that is much larger than the unit cell size of the lattice. Therefore, it is necessary to consider the effect of the lattice potential on the effective mass of electrons and holes. Due to the lower mass and shielding Coulomb force, its binding energy is usually significantly less than 0.01 eV.

[0053] However, the excitons of the nanocrystals described in the present application are different from the two traditional types of excitons, and are named dynamic excitons in the present application. The electron-hole Coulomb interaction of the dynamic excitons of the present application is not sufficient to bind each other to form stable bound excitons at the working temperature, but is in an ionized state. At the same time, the ionized electrons and holes are constrained by the boundaries of the nanocrystals and cannot obviously overflow into the ambient medium outside the nanocrystals.

[0054] Since the excitons of the nanocrystals of the present application have the characteristics of dynamic excitons, the nanocrystals have unique optical and optoelectronic properties different from conventional semiconductor nanomaterials. For example, the band edge energy level density of the electrons (or holes) of the dynamic excitons is high and the intraband energy gap is small, which leads to a rare room temperature double peak steady-state luminescence, which has unique value for applications (such as lighting) that require wide-band luminescence. For another example, the electron (or hole) wave functions of the dynamic excitons are not strongly constrained to each other and are rapidly weakened as the temperature rises, which is conducive to electron-hole transfer, which is of great significance for photovoltaic solar devices, photodetectors, and photocatalysis.

[0055] In addition, the dynamic exciton wave function in the nanocrystal is far away from the irregular surface and confined inside the lattice. Under low temperature conditions, the dynamic excitons of the nanocrystal have good determinism, which is manifested as low temperature (<10K) emission with ultra-narrow half-peak width and narrow peak emission with a certain lifetime. This luminescence half-peak width is much narrower than that of strongly confined nanocrystals of the same material, and is suitable for the development of quantum light sources.

[0056] The experiment also proves that when the dynamic exciton of the nanocrystal contains more than two free carriers, the multiple wave functions of the same-sign carriers (electrons or holes) have enough free delocalization space and rarely overlap with each other, which makes the Auger effect of the nanocrystal of the present application very small. In this regard, the charged state of the weakly confined nanocrystals of the II-IV and III-V groups can still guarantee a near-perfect single exciton and multi-exciton luminescence quantum yield. Under strong excitation conditions, whether it is luminescence, photovoltaic, laser or photochemical applications, the biexciton or multi-exciton state of the weakly confined nanocrystals of the II-IV and III-V groups can guarantee a high quantum yield.

[0057] In some embodiments, the size of the nanocrystal is 1 to 20 times the diameter of its exciton. Preferably, the size of the nanocrystal is 1 to 6 times the diameter of its exciton. For example, the exciton diameter of CdSe is 11.2 nm, and the present application prepares CdSe cubic crystals with a size of 10-30 nm; the exciton diameter of CdS is 5.6 nm, and the present application prepares CdS cubic crystals with a size of 7-21 nm. Alternatively, the size of the nanocrystal is 2 to 6 times the diameter of its exciton.

[0058] In some embodiments, the size of the nanocrystals is greater than 10 nm, preferably greater than 15 nm, preferably greater than 20 nm, more preferably greater than 25 nm, and more preferably greater than or equal to 30 nm.

[0059] In some embodiments, the nanocrystals are monodisperse nanocrystals. The present application provides a method for preparing nanocrystals, which can achieve controllable growth of nanocrystal size and morphology, and synthesize monodisperse, large-sized nanocrystals. The "monodisperse" mentioned in the present application refers to nanocrystals with uniform size and morphology, and good dispersibility in a specific medium.

[0060] In some embodiments, the relative standard deviation of the size distribution of the nanocrystals is no more than 10%, preferably no more than 6%, preferably no more than 5%, preferably no more than 4%, and more preferably no more than 3%. A lower relative standard deviation indicates that the nanocrystals have good size and morphology monodispersity.

[0061] In some embodiments, transmission electron microscope illumination shows that the nanocrystal has a uniform and regular square two-dimensional projection, that is, the nanocrystal has good morphological monodispersity.

[0062] In some embodiments, high-resolution transmission electron microscopy images show that the nanocrystal has single-period non-dislocated lattice fringes and atomically smooth boundaries. Clear single-period non-dislocated lattice fringes indicate that the nanocrystal has good single crystallinity. Atomic-level smooth boundaries indicate that the flatness of the nanocrystal surface is good, that is, the integrity of its morphology is good.

[0063] In some embodiments, the excitation spectra of the nanocrystals at different fluorescence emission positions are substantially overlapped. Generally, only when the nanocrystal size is monodisperse, the exciton state of the nanocrystals is monodisperse, and the fluorescence contributions of different emission peaks of the fluorescence spectrum come from the same nanoparticle, the excitation spectra of the nanocrystals at different emission positions will be completely consistent. This shows that the nanocrystals have good size monodispersity and their size distribution will not affect the exciton energy level structure corresponding to the nanocrystals.

[0064] In some embodiments, the nanocrystals are of a sphalerite single crystal structure. According to XRD characterization results, the nanocrystals prepared in the present application are of a pure sphalerite structure without obvious defects.

[0065] In some embodiments, under room temperature test conditions, the UV-visible absorption spectrum of the nanocrystal has no obvious exciton absorption peak, showing a quasi-continuous band absorption similar to the bulk phase. The quantum confinement effect of the nanocrystal of the present application is weak, and its absorption has properties similar to the bulk phase.

[0066] In some embodiments, under room temperature test conditions, the fluorescence spectrum of the nanocrystal has an asymmetric characteristic, specifically, the fluorescence spectrum of the nanocrystal has an asymmetric characteristic of tailing to high energy. Due to the asymmetric characteristic of the fluorescence spectrum of the nanocrystal, the fluorescence spectrum of the nanocrystal has a wide half-peak width.

[0067] In some embodiments, the intrinsic fluorescence half-peak width of the monodisperse nanocrystals is greater than 70 meV.

[0068] In some embodiments, under room temperature test conditions, double Gaussian fitting results of the fluorescence emission spectrum of the nanocrystal show that the fluorescence emission spectrum of the nanocrystal includes two fluorescence emission peaks with different energies, that is, the nanocrystal has a dual-level emission fluorescence property.

[0069] In some embodiments, the fluorescence emission peak of the nanocrystal is substantially consistent with the band gap width of its bulk material. The quantum confinement effect of the nanocrystal of the present application is weak, so its spectral properties are extremely similar to those of the bulk material. For example, the fluorescence emission peak corresponding to the CdS nanocrystal with a size of 21 nm prepared in the present application reaches 2.38 eV, which is consistent with the band gap width of bulk zinc blende CdS reported in the literature as 2.38 eV (300K).

[0070] In some embodiments, the single particle fluorescence corresponding to the nanocrystal has no fluorescence flickering for at least 1000 s.

[0071] In some embodiments, the biexciton fluorescence yield of the nanocrystal is not less than 50%, preferably not less than 70%, preferably not less than 80%, more preferably not less than 90%, and more preferably not less than 95%.

[0072] In some embodiments, the nanocrystal is a core-structured nanocrystal or a core-shell structured nanocrystal.

[0073] In some embodiments, the nanocrystal is a Group II-IV semiconductor or a Group III-V semiconductor, such as a telluride semiconductor, a selenide semiconductor, a sulfide semiconductor, a phosphide semiconductor, or an arsenide semiconductor.

[0074] In some embodiments, the nanocrystals are CdS or CdSe or CdSe / CdS core / shell cubic nanocrystals.

[0075] In some embodiments, the size of the CdSe core in the CdSe / CdS core / shell cubic nanocrystals is 6 nm to 25 nm, and the number of CdS shell layers is 1 to 20 monolayers.

[0076] The weakly confined CdE (CdS or CdSe or CdSe / CdS core / shell) cubic nanocrystals of the present application have excellent light emission properties. For example, the biexciton emission efficiency of the weakly confined CdSe / CdS core / shell nanocrystals is close to 100%, the single particle fluorescence has no flickering, and the fluorescence spectrum of the aggregate completely overlaps with the fluorescence spectrum of the single particle. In addition, the CdE cubic nanocrystals also exhibit unique size-related intrinsic optical properties. For example, as the size of the nanocrystal increases, the fluorescence half-peak width of CdE does not gradually decrease, but first decreases, then rapidly increases, and then decreases; in addition, when the size of the CdE cubic nanocrystal reaches a certain critical size, its corresponding absorption spectrum gradually becomes a quasi-continuous band absorption similar to the bulk phase, and its corresponding fluorescence spectrum tails to high energy and appears asymmetric; and when the size of the CdSe / CdS core / shell cubic nanocrystal is larger than its corresponding critical size, its corresponding fluorescence peak position will also appear to move to high energy and the fluorescence lifetime will increase rapidly. It is worth noting that the critical size corresponding to different nanocrystals is close to the corresponding exciton Bohr diameter.

[0077] The corresponding relationship between the band edge energy level structure of weakly confined CdE cubic nanocrystals and their optical properties is revealed through theoretical calculation of the energy level structure of CdE cubic nanocrystals and fitting of the corresponding fluorescence spectrum and absorption spectrum. As the size of the nanocrystal increases, the band edge energy level state density gradually increases, so the exciton absorption peak characteristics of the absorption spectrum degenerate into quasi-continuous band absorption. In addition, the higher energy level state density leads to the phenomenon of dual-level simultaneous emission in the fluorescence emission process at room temperature, so the fluorescence emission spectrum becomes asymmetric and the fluorescence half-peak width increases rapidly.

[0078] The exciton decay properties of CdSe / CdS core / shell cubic nanocrystals were analyzed through size-dependent and temperature-dependent experiments. The experimental results show that the decay rate of excitons is not only related to the strength of the electron confinement effect, but also to the strength of the hole confinement effect, and that the temperature-dependent lifetime change rates of CdSe / CdS core / shell cubic nanocrystals with different confinement effects are different.

[0079] The biexciton efficiency of the CdSe12 / 20CdS (12nm CdSe as the core, 20 monolayers of CdS grown) cubic nanocrystals prepared in this application is as high as 99%, which indicates that there is almost no Auger effect in the multi-exciton process. This is an ideal material for high-power devices such as light-emitting diodes and lasers.

[0080] Preliminary experimental results show that cubic nanocrystals are easier to self-assemble into close-packed superlattices, which will also effectively improve the conductivity between particles. By adjusting the composition of II-VI semiconductor nanocrystals, their fluorescence emission position can reach the standard position of green and red light. Therefore, weakly confined core / shell cubic nanocrystals have more advantages in the practical application of high-power devices.

[0081] Preliminary experimental results show that the low-temperature fluorescence half-peak width of weakly confined CdSe8 / 20CdS cubic nanocrystals with room temperature fluorescence half-peak width exceeding 70meV is reduced to 30μeV (the minimum resolution of the detector). Linear fluorescence emission means that the emission photon purity of weakly confined CdSe8 / 20CdS cubic nanocrystals at low temperatures basically meets the requirements of single-photon devices.

[0082] The present application provides a method for preparing semiconductor nanocrystals, comprising the following steps:

[0083] Synthesis of nanocrystal seeds: a cationic precursor reacts with a first fatty acid at a first temperature, and then a first anionic precursor is added to react to obtain a nanocrystal seed, wherein the size of the nanocrystal seed is smaller than the exciton diameter thereof;

[0084] Growth of nanocrystals: the cationic precursor, the first fatty acid, the second fatty acid and the fatty acid chloride react at a second temperature, and then the nanocrystal seeds and the second anionic precursor are added in sequence for growth to obtain nanocrystals having a size larger than the exciton diameter.

[0085] The synthesis of weakly confined nanocrystals adopts a two-step growth synthesis strategy of separating nucleation and growth. The preparation method of the present application introduces fatty acyl chloride in the growth step of nanocrystals because chloride ions are also beneficial to the synthesis of cubic nanocrystals. Considering the strong binding energy between chloride ions and cadmium ions, it is not favorable to introduce chloride ions in the nucleation stage, so acyl chloride is not added in the synthesis step of nanocrystal seeds.

[0086] In some embodiments, the second reaction temperature is greater than the first reaction temperature.

[0087] In some embodiments, the cation precursor is a cadmium carboxylate, and the first anion precursor is a Se precursor or a S precursor.

[0088] Furthermore, the first fatty acid is a fatty acid having no less than 10 carbon atoms, preferably, a fatty acid having no more than 18 carbon atoms.

[0089] Furthermore, the second fatty acid is a fatty acid having no less than 22 carbon atoms.

[0090] The present application also provides uses of the nanocrystals for lighting, or for photovoltaic solar devices, or for photodetectors, or for lasers, or for quantum light sources.

[0091] [Example]

[0092] (1) Preparation of reaction precursors

[0093] 0.1M (mol / L) selenium powder-ODE suspension (Se-SUS): Weigh 1mmol selenium powder (0.079g) and place it in a 20mL glass bottle and add 10mL of octadecene (ODE) solution. After ultrasonication for 5 minutes, oscillate to obtain 0.1M Se-SUS suspension. Se-SUS suspensions of other concentrations can be prepared by the same steps. Commonly used concentrations are 0.025M, 0.1M and 0.2M.

[0094] 0.1M (mol / L) selenium powder-ODE solution (Se-ODE): Weigh 3mmol selenium powder (0.237g) and place it in a 20mL glass bottle and add 5mL ODE solution, ultrasonicate for 5 minutes, take another 25mL octadecene solution and add it to a 50mL three-necked flask and heat it to 250℃, shake the selenium powder suspension and inject it into the three-necked flask at a rate of 1mL / time for 5 times, after all the selenium powder is injected into the three-necked flask, reduce the reaction temperature to 200℃ and keep it for 4 hours to stop the reaction.

[0095] 0.1M (mol / L) sulfur powder-ODE solution (S-ODE): Weigh 1.5mmol sulfur powder (0.048g) and place it in a 20mL glass bottle and add 15mL ODE solution. Ultrasonicate until the sulfur powder is completely dissolved to obtain 0.1M S-ODE solution. S-ODE solutions of other concentrations can be prepared using the same steps. Commonly used concentrations are 0.1M and 0.2M, and the S-ODE stock solution also needs to be stored away from light.

[0096] 0.1M (mol / L) octadecanoyl chloride stock solution: Weigh 1mmol octadecanoyl chloride (0.309g) and place it in a 20mL glass bottle and add 10mL of L ODE solution. Shake well to prepare 0.1M octadecanoyl chloride solution.

[0097] 0.1M (mol / L) cadmium carboxylate solution: Weigh 0.4mmol cadmium acetate dihydrate (0.106g), 0.6mmol oleic acid (erucic acid), 0.6mmol decacarboxylic acid and 4mL ODE solution into a 25mL three-necked flask, blow with argon and raise the temperature to 150℃ and maintain for 30min.

[0098] 0.1M (mol / L) cadmium chloride carboxylate solution: weigh 0.2mmol cadmium acetate dihydrate (0.054g), 0.6mmol oleic acid (erucic acid), 0.4mmol decacarboxylic acid and 2mL ODE solution into a 10mL three-necked flask, blow with argon and heat to 150℃ for 10 minutes, then heat to 270℃, inject 0.4mL octadecanoyl chloride stock solution (0.04mmol acyl chloride) and maintain the reaction temperature at 270℃ for 10 minutes, finally cool to 100℃ for standby use; Note: For the preparation of large-sized nanocrystals, oleic acid can be replaced with an equal amount of erucic acid, and the prepared cadmium chloride carboxylate salt needs to be used on the same day.

[0099] (2) Synthesis of CdSe and CdS Nanocrystals

[0100] Synthesis of CdSe nanocrystal seeds: 0.2mmol cadmium acetate dihydrate, 4mmol stearic acid, 12mmol oleic acid and 28mLODE solution were added to a 50mL three-necked flask, heated to 150℃ with argon gas and maintained for 10 minutes, then heated to 250℃ and quickly injected with 1mL 0.1M Se-SUS suspension. After 5min of reaction, 0.1mL 0.1M Se-SUS suspension was injected every 5 minutes. During the reaction, a small amount of reaction solution was added to a cuvette containing toluene, and then UV-visible absorption spectrum or fluorescence emission spectrum test was performed to detect the progress of the reaction. After about 5 subsequent injections of Se-SUS (about 30 minutes in total), the first exciton absorption peak of the absorption spectrum corresponding to the CdSe nanocrystal seeds reached 550nm (the fluorescence emission peak reached about 560nm, and the nanocrystal size was about 3nm). At this time, the heating device was removed and the temperature was lowered to below 100℃ to stop the reaction.

[0101] Synthesis of CdS nanocrystal seeds: 0.2mmol cadmium oxide, 3mmol oleic acid and 6mL ODE solution were placed in a 25mL three-necked flask, and the temperature was raised to 260℃ with argon gas until the solution was completely clear. Then the temperature was lowered to 230℃ and 0.5mL 0.1MS-ODE solution was injected. During the reaction, a small amount of the reaction solution was added to a cuvette containing toluene, and then UV-visible absorption spectroscopy or fluorescence emission spectroscopy was performed to detect the progress of the reaction. After 15 minutes of reaction, the first exciton absorption peak corresponding to the CdS nanocrystal seeds reached 430nm (the fluorescence emission peak reached 442nm, and the size was about 3nm). At this time, the heating device was removed and the temperature was lowered to below 100℃ to stop the reaction.

[0102] (3) Synthesis of CdSe cubic nanocrystals

[0103] Synthesis of CdSe cubic nanocrystals with a typical size of less than 10nm: 0.2mmol cadmium acetate dihydrate, 1.2mmol oleic acid and 10mL ODE solution are placed in a 25mL three-necked flask, purged with argon and heated to 150℃ for 10 minutes. Then the temperature is raised to 270℃ and 0.4mL 0.1M octadecanoyl chloride stock solution is added. After reacting for 5 minutes, 70nmol of purified CdSe nanocrystal seeds are added. 0.03M Se-ODE precursor solution is added dropwise at a rate of 1.2mL / h until the CdSe cubic nanocrystals reach the target size, and the heating and Se precursor addition are stopped to stop the reaction. About 4 hours after the Se-ODE is added, the first exciton absorption peak of the UV-visible absorption spectrum corresponding to the CdSe cubic nanocrystals reaches 690nm (the peak position of the fluorescence emission spectrum reaches 695nm, and the size is about 8nm). During the reaction, a certain amount of reaction solution (~250 μL) was added to a cuvette containing a certain amount of toluene (2 mL) for UV-visible absorption spectrum and fluorescence emission spectrum measurement to detect the progress of the reaction. Generally, quantitative sampling is performed for quantitative measurement of UV-visible absorption spectrum and fluorescence emission spectrum. Note: When the size of CdSe cubic nanocrystals exceeds 8 nm, a certain amount of deca acid needs to be added to form an entropic ligand system to maintain the solution stability of CdSe cubic nanocrystals. Among them, the molar ratio of oleic acid to deca acid is optimal between 4:1 and 2:1. In addition, after the reaction is completed, 1 mmol of oleic acid is added when the solution temperature drops to 150°C and maintained at 150°C for 10 minutes. This is to reduce the solubility of CdSe cubic nanocrystal seeds to facilitate the purification and separation of CdSe cubic nanocrystal seeds in the mixed solution.

[0104] Synthesis of CdSe cubic nanocrystals with a typical size of more than 10nm: 0.3mmol cadmium acetate dihydrate, 0.7mmol erucic acid, 0.7mmol decadecanoic acid and 10mL ODE solution were placed in a 25mL three-necked flask, purged with argon and heated to 150℃ for 10 minutes. Then the temperature was raised to 270℃ and 0.5mL 0.1M octadecanoyl chloride stock solution was added. After reacting for 5 minutes, the purified CdSe cubic nanocrystals prepared above were added. 0.03M Se-ODE precursor solution was added at a rate of 1.8mL / h until the CdSe cubic nanocrystals reached the target size (10nm), and the heating and Se precursor addition were stopped to stop the reaction. Take half of the purified and separated 10nm CdSe cubic nanocrystals for subsequent growth. After adding Se precursor for 4 hours, the size of the CdSe cubic nanocrystals will reach about 18nm (fluorescence emission peak ~726nm); if a quarter of the 10nm CdSe cubic nanocrystals are grown for 4 hours, their size will reach 22nm (fluorescence emission peak ~732nm). Quantitatively detect the reaction progress during the reaction, take 250μL of the reaction solution and add it to a cuvette containing 2mL of toluene for UV-visible absorption and fluorescence emission spectrum measurements. Note: When the size of the cubic nanocrystals (CdSe, CdS, and CdSe / CdS) exceeds 25nm, a certain amount of octadecanoic acid needs to be added to the reaction system to maintain the solution stability of the cubic nanocrystals.

[0105] (4) Synthesis of CdS cubic nanocrystals

[0106] The synthesis of CdS cubic nanocrystals is similar to that of CdSe cubic nanocrystals except that fatty acid needs to be added subsequently.

[0107] Synthesis of CdS cubic nanocrystals with a typical size of less than 10nm: 0.2mmol cadmium acetate dihydrate, 1.2mmol oleic acid and 10mL ODE solution were placed in a 25mL three-necked flask, purged with argon and heated to 150℃ for 10 minutes. Then the temperature was raised to 270℃ and 0.4mL 0.1M octadecanoyl chloride stock solution was added. After 5 minutes of reaction, 70nmol of purified CdS nanocrystal seeds were added. 0.03MS-ODE precursor solution was added dropwise at a rate of 0.6mL / h until the CdS cubic nanocrystals reached the target size. When the added 0.03M S-ODE solution was prepared by mixing 1mL 0.1M S-ODE with 1mL oleic acid and 1mL ODE solution, about 3 hours after the addition of S-ODE, the fluorescence emission spectrum corresponding to the CdS cubic nanocrystal reached a peak of 508nm, and its size was about 8nm. During the reaction, the reaction progress was quantitatively detected. 250 μL of the reaction solution was added to a cuvette containing 2 mL of toluene for UV-visible absorption and fluorescence emission spectrum measurements. Similar to the synthesis of CdSe cubic nanocrystals, when the size of CdS cubic nanocrystals exceeds 8 nm, a certain amount of deca-acid also needs to be introduced into the reaction system. The ratio of oleic acid to deca-acid is the same as above. At the end of the reaction, 1 mmol of oleic acid was also added to facilitate the purification of CdS cubic nanocrystals.

[0108] Synthesis of CdS cubic nanocrystals with a typical size of more than 10nm: 0.4mmol cadmium acetate dihydrate, 1mmol erucic acid, 1mmol decadecanoic acid and 10mLODE solution are placed in a 25mL three-necked flask, purged with argon and heated to 150℃ for 10 minutes. Then the temperature is raised to 270℃ and 0.6mL 0.1M octadecanoyl chloride stock solution is added. After 5 minutes of reaction, all the purified CdS cubic nanocrystals prepared above are added. 0.03M S-ODE precursor solution is added dropwise at a rate of 1.2mL / h until the CdS cubic nanocrystals reach the target size, and the heating and S precursor addition are stopped to stop the reaction. The 0.03M S-ODE solution contains a certain amount of fatty acids, and the molar ratio of fatty acids (erucic acid: decadecanoic acid = 1:1) to sulfur is optimally between 3:1 and 6:1. After 4 hours of growth, the size of the 10nm CdS cubic nanocrystal (fluorescence emission peak @ 512nm) will reach 20nm (fluorescence emission peak reaches 520nm). During the reaction, the reaction progress was quantitatively detected, and 250μL of the reaction solution was added to a cuvette containing 2mL of toluene for UV-visible absorption and fluorescence emission spectrum measurements.

[0109] (5) Synthesis of CdSe / CdS core-shell cubic nanocrystals

[0110] CdSex / yCdS core-shell structured cubic nanocrystals are prepared by epitaxially growing y layers of CdS shell using x nm (3≤x≤16) CdSe cubic nanocrystals as seeds. The synthesis conditions of CdSex / yCdS core-shell structured cubic nanocrystals are similar to those of CdS cubic nanocrystals, both of which require a higher fatty acid concentration to regulate the growth of CdS. It is worth noting that the ligand systems for the initial growth of CdSe cubic nanocrystals of different sizes are different. The synthesis of CdSe5 / CdS and CdSe8 / CdS cubic core-shell nanocrystals is used as an example to illustrate.

[0111] The typical preparation method of CdSe5 / CdS cubic core-shell nanocrystals is as follows: 0.3mmol cadmium acetate dihydrate, 0.6mmol oleic acid, 0.6mmol decadecanoic acid and 10mL ODE solution are placed in a 25mL three-necked flask, purged with argon and heated to 150℃ for 10 minutes. Then the temperature is raised to 270℃ and 0.4mL 0.1M octadecanoyl chloride stock solution is added. After reacting for 5 minutes, the purified 5nm CdSe cubic nanocrystal seeds (half the amount of 5nm CdSe cubic nanocrystals prepared in the typical preparation method of CdSe cubic nanocrystals) are added. 0.03M S-ODE precursor solution is added dropwise at a rate of 1.0mL / h until the shell CdS reaches the target number of layers, and the heating and S precursor addition are stopped to stop the reaction. The 0.03M S-ODE solution contains a certain amount of erucic acid, and the molar ratio of erucic acid to sulfur is optimally between 3:1 and 6:1. After 3 hours of growth, the epitaxial CdS shell layer of 5nm CdSe cubic nanocrystals (fluorescence emission peak @ 660nm) reached 20 layers (the size of the cubic nanocrystals was close to 16nm, and the fluorescence emission peak reached 685nm). The reaction progress was quantitatively detected during the reaction. 250μL of the reaction solution was added to a cuvette containing 2mL of toluene for UV-visible absorption spectroscopy, steady-state fluorescence emission spectroscopy, and transient fluorescence spectroscopy.

[0112] The typical preparation method of CdSe8 / CdS cubic core-shell nanocrystals is as follows: 0.4mmol cadmium acetate dihydrate, 1mmol erucic acid, 1mmol decadecanoic acid and 10mL ODE solution are placed in a 25mL three-necked flask, purged with argon and heated to 150℃ for 10 minutes. Then the temperature is raised to 270℃ and 0.6mL 0.1M octadecanoyl chloride stock solution is added. After reacting for 5 minutes, the purified 8nm CdSe cubic nanocrystal seeds (half the amount of 8nm CdSe cubic nanocrystals prepared in the typical preparation method of CdSe cubic nanocrystals) are added. 0.05M S-ODE precursor solution is added dropwise at a rate of 1.5mL / h until the shell CdS reaches the target number of layers, and the heating and S precursor addition are stopped to stop the reaction. The 0.05M S-ODE solution contains a certain amount of fatty acids, and the molar ratio of fatty acids (erucic acid: decadecanoic acid = 1:1) to sulfur is optimally between 3:1 and 6:1. After 4 hours of growth, the 8nm CdSe cubic nanocrystal (fluorescence emission peak @ 695nm) has 20 epitaxial CdS shell layers (the size of the cubic nanocrystal is close to 20nm, and the fluorescence emission peak reaches 705nm). The reaction progress is quantitatively detected during the reaction. 250μL of the reaction solution is added to a cuvette containing 2mL of toluene for UV-visible absorption spectroscopy, steady-state fluorescence emission spectroscopy, and transient fluorescence spectroscopy.

[0113] (6) Quantitative purification method of CdSe and CdS nanocrystals

[0114] Toluene methanol hot centrifugation purification scheme: Place the CdSe (CdS) nanocrystal seed reaction solution in a glass bottle and add twice the volume of ethanol solution, shake well, centrifuge at 4000 rpm for 5 minutes, and discard the upper ODE solution. Add 2mL of toluene to the glass bottle, heat or shake to dissolve the precipitate (nanocrystal seed), add an equal volume of methanol solution and place on a hot plate at 100℃. After heating for 5 minutes, quickly centrifuge at 4000 rpm for 30 seconds and discard the supernatant.

[0115] The operation of dissolving methanol in toluene and hot precipitation was repeated twice to ensure that the residual cadmium salt was completely removed to achieve the purpose of purification. The obtained precipitate (nanocrystal seed) was vacuum dried for 20 minutes and then 2 mL of ODE solution was added and heated to dissolve. The purified nanocrystal seed ODE solution was quantitatively calibrated for concentration and then set aside. The specific quantitative method is as follows: weigh a certain amount of purified nanocrystal seed ODE solution and add it to a known amount of toluene solution, shake well and measure the UV-visible absorption spectrum. Using the extinction coefficient of nanocrystals reported in the literature, the concentration of nanocrystal seeds in the solution can be calculated. It is worth noting that the extinction coefficient reported here is only applicable to spherical nanocrystals and non-cubic nanocrystals because the spherical approximation and non-cubic approximation are used in the process of calculating the size of nanocrystals.

[0116] (7) Purification, separation and quantitative methods of CdSe, CdS and CdSe / CdS cubic nanocrystals

[0117] The products obtained by using the typical synthesis strategy of CdSe or CdS cubic nanocrystals with a size below 10nm include not only the target product (cubic nanocrystals) but also a small amount of by-products (non-cubic nanocrystals). Separating these by-products is the primary task to obtain the target product. The size of the by-products in the synthetic product is much smaller than that of the target product, so the solubility of the by-products in the reaction system is greater than that of the target product. Therefore, the difference in solubility between the two is used to separate and remove the by-products. The specific separation and purification method is as follows: the reaction solution is placed in a glass bottle and placed on a 100℃ hot plate for 5 minutes, shaken and placed in a centrifuge, centrifuged at 4000 rpm for 5 minutes, and then the supernatant is discarded to remove most of the by-products and the reaction solvent (ODE). Add 4mL of toluene to shake or heat to dissolve the precipitate, then add 0.4mL of acetonitrile precipitant, shake and shake, centrifuge at 4000 rpm for 1 minute, and discard the supernatant. The precipitate is the target product-CdSe (CdS) cubic nanocrystals, but it still contains unreacted cadmium salt precursors. The purification operation of using two times of toluene-methanol hot centrifugation can effectively remove the unreacted cadmium salt precursor and achieve the purpose of purification. Finally, the separated and purified CdSe (CdS) cubic nanocrystals are dissolved in 2 mL of hexane for later use.

[0118] Purified CdSe (CdS) cubic nanocrystals are used as seeds for subsequent growth to obtain monodisperse CdSe, CdS and CdSe / CdS cubic nanocrystals. The purification scheme using toluene methanol hot centrifugation can also effectively purify the target product, but this method will greatly affect the optical properties of the cubic nanocrystals. Therefore, a milder precipitant such as isopropanol is used for purification of cubic nanocrystals used for optical property research. The specific purification method is as follows: the reaction solution is placed in a glass bottle and 1.5-2 times the volume of isopropanol solution is added. The mixed solution is placed on a 100°C hot stage and kept for 5 minutes, and then placed in a centrifuge for centrifugation at 4000 rpm for 1 minute and the supernatant is discarded. Add 0.5 mL of hexane and shake or heat to dissolve the precipitate, then add 3 mL of ODE solution and shake well, then add 1.5-2 times the volume of isopropanol solution and place on a 100°C hot plate for 5 minutes, finally centrifuge at 4000 rpm for 1 minute and discard the supernatant, add 2 mL of toluene to dissolve the precipitate for later use.

[0119]

Sample Characterization

[0120] (1) UV-Vis absorption spectrum

[0121] Before testing the sample, first collect the baseline of the blank good solvent (toluene, hexane, chloroform, etc.) and save it as the test method. When testing the sample, take a certain amount of nanocrystal solution and add it to a quartz cuvette containing a certain amount (≥2mL) of good solvent, open the test method of the corresponding solvent, and measure the UV-visible absorption spectrum after zeroing. The UV-visible absorption spectrum obtained in this way has the solvent background subtracted and the absorbance is zeroed at the maximum wavelength. The optical path of the quartz cuvette is 1cm, the commonly used test range of the UV-visible absorption spectrum is 300-800nm, and the spectrum acquisition step is 0.5-1nm.

[0122] (2) Steady-state fluorescence spectroscopy

[0123] Take a certain amount of nanocrystal solution and add it to a quartz cuvette containing a certain amount (≥2mL) of good solvent (toluene, hexane, chloroform, etc.) to perform steady-state fluorescence spectrum test (fluorescence emission spectrum and fluorescence excitation spectrum). When performing fluorescence spectrum test, the sample concentration should not be too high, and its absorbance usually does not exceed 0.1 to avoid serious reabsorption effect. When performing fluorescence emission spectrum test, the commonly used excitation wavelength of CdSe (CdSe / CdS) nanocrystals is 400nm, and the commonly used excitation wavelength of CdS nanocrystals is 350nm. However, in the fluorescence up-conversion test, the excitation wavelength is greater than the corresponding nanocrystal fluorescence emission peak. The spectrum acquisition step length (0.2-1nm) depends on the situation, such as calculating the fluorescence half-peak width using a smaller step length.

[0124] (3) Transient fluorescence spectroscopy

[0125] Take a certain amount of nanocrystal solution and add it to a quartz cuvette containing a certain amount (≥2mL) of toluene solution for transient fluorescence spectrum test. Due to the great difference in exciton decay dynamics under different medium environments, the solvents used in transient fluorescence tests are all toluene solutions unless otherwise specified. The instrument used for transient fluorescence spectrum is Edinburgh Instruments fluorescence spectrometer (FLS920, Edinburgh Instrument, UK), and the excitation light source is a picosecond laser with a wavelength of 405nm and a repetition rate of 2MHZ. In the transient fluorescence test, the number of photons collected each time is set between 1000-5000. If the single exponential fit goodness of the fluorescence decay curve χ 2 If it is less than or equal to 1.3, the fluorescence of the corresponding nanocrystal decays in a single exponential manner, and the fluorescence lifetime τ is obtained by fitting the decay curve with a single exponential function.

[0126] (4) Infrared absorption spectrum

[0127] The infrared spectroscopy test objects in this paper are mainly carbonyl compounds (RCOO-, RCOOH, R1COOCOR2), and the commonly used solvents for testing are dodecane or ODE solution. The test cuvette is a self-made small optical path cuvette, and the specific construction method is as follows: two calcium fluoride windows (15mm×15mm×1mm) as windows, two alumina ceramics (15mm×2mm×0.5mm) as gaskets, and two dovetail clips with the surface paint removed to clamp the two symmetrical gaskets. Using the surface tension of the liquid, the cuvette can add about 100μL of the solution to be tested. During the test, the test solvent is first used as a blank, and then a 200μL pipette is used to carefully add the solution to be tested into the cuvette for infrared testing, and the obtained infrared spectrum is further subtracted from the solvent background.

[0128] (5) Transmission electron microscopy

[0129] Low-resolution transmission electron microscopy (TEM) test: Take the nanocrystal solution (purified or not) and dilute it into a certain amount of toluene solution, then add it drop by drop onto the ultra-thin carbon film. After the solvent evaporates completely, the TEM test can be carried out.

[0130] High-resolution transmission electron microscopy (HRTEM) test: The purified nanocrystal solution is dissolved in a certain amount of toluene solution, and then dripped onto the ultra-thin carbon film drop by drop. HRTEM test can be performed after the solvent evaporates completely.

[0131] (6) Scanning electron microscopy

[0132] The purified and vacuum dried nanocrystal powder was coated on a conductive adhesive and then glued to a silicon wafer for SEM testing. The main purpose of the SEM test in this paper is the quantitative analysis of elements and the characterization of the self-assembly of cubic nanocrystals.

[0133] (7) X-ray powder diffraction

[0134] The purified and vacuum-dried nanocrystalline powder was evenly spread on a silicon wafer and then placed in a quartz glass sample tank for X-ray powder diffraction testing. Test conditions: 40KV / 30mA, Cu target ( ).

[0135] (8) Small-angle X-ray scattering

[0136] The purified and vacuum-dried nanocrystalline powder was adhered to the KAPTOM film for small angle X-ray scattering (SAXS) testing. The test conditions were: 50KV / 0.6mA, Cu target ( ).

[0137] (9) Single particle spectral test

[0138] The nanocrystal solution was diluted with the toluene solution after dehydration of the sodium sheet (usually the dilution factor was 100,000 times), and then mixed with the toluene solution of polymethyl methacrylate (PMMA, 0.5-1.5wt%). The diluted nanocrystal solution was added dropwise to the cleaned glass slide with a pipette, and then spin-coated on a coating machine to form a film. The single-particle fluorescence spectrum, fluorescence intensity, and fluorescence lifetime were tested using an inverted fluorescence microscope system built by the group.

[0139] (10) Spherical aberration corrected field emission scanning transmission electron microscope

[0140] The purified nanocrystal solution is dissolved in a certain amount of toluene solution, and then dripped onto the ultra-thin carbon film. Once the solvent evaporates completely, the HAADF-STEM test can be performed. The purpose of the STEM test in this article is mainly the atomic characterization of cubic nanocrystals and the elemental mapping analysis of CdSe / CdS core-shell cubic nanocrystals.

[0141]

Figure 1

[0142] The basic synthesis route of large-sized CdE cubic nanocrystals is as follows: Figure 1 (above). In this synthesis route, small-sized (≤10nm) CdE cubic nanocrystals are used as seeds, wherein CdE cubic nanocrystals include CdSe, CdS and CdSe / CdS cubic nanocrystals. The reaction product of cadmium acetate, erucic acid (octadecanoic acid), decadecanoic acid and octadecanoyl chloride (cadmium carboxylate chloride) is used as a cationic precursor and an organic ligand on the surface of the cubic nanocrystal; Se-ODE (S-ODE) is used as an anionic precursor; ODE is used as a solvent; the final CdE cubic nanocrystal product can reach a size of 30nm and maintain monodispersity in size and morphology. As shown Figure 1 As shown, in the synthesis system of large-sized CdE cubic nanocrystals, using CdSe cubic nanocrystals as seeds for growth and using a ligand system consisting of octadecanoate, erucate and decadecate can obtain CdSe cubic nanocrystals with a size of up to 30 nm (bottom) and monodisperse size and morphology. Figure 1 The nanocrystal size is significantly larger than the maximum size of monodisperse CdSe nanocrystals reported in the literature. This fully demonstrates the feasibility of the large-size CdE cubic nanocrystal synthesis system for the synthesis of large-size monodisperse nanocrystals, and also confirms the feasibility of preparing monodisperse CdE large-size cubic nanocrystals under this ligand system.

[0143]

Figure 2

[0144] Figure 2 The characterization results of CdSe cubic nanocrystals with a size of 21 nm are shown, and the CdSe cubic nanocrystals are prepared by the method of the embodiment.

[0145] Figure 2 The TEM images of a are all square two-dimensional projections with regular boundaries, and the relative standard deviation of their size distribution is only 3% ( Figure 2 a upper left graph), which shows that the CdSe nanocrystals have good monodispersity in size and morphology.

[0146] Figure 2 The high-resolution electron microscopy characterization results of (b, c, d) show that the clear single-period lattice fringes without dislocation illustrate the good single crystallinity of CdSe cubic nanocrystals; the atomically flat boundaries illustrate the flatness of the crystal faces of CdSe nanocrystals, that is, the integrity of the cubic morphology; the lattice spacing consistent with the sphalerite lattice parameters indicates that this CdSe cubic nanocrystal has a sphalerite structure.

[0147] Figure 2 The XRD characterization results in (e) that strictly correspond to the standard card diffraction peaks also prove that the CdSe cubic nanocrystals have a zinc blende structure without obvious defects, and the extremely narrow diffraction peaks reflect the larger size of the nanocrystals.

[0148] The above characterization results show that the prepared CdSe cubic nanocrystals are monodisperse in size and morphology and have a zinc blende single crystal structure with excellent crystallinity.

[0149] Figure 2 In (f), the normalized PLE spectra of the 21nm CdSe cubic nanocrystals at different emission positions completely overlap, indicating that they have good size monodispersity and their size distribution will not affect the exciton energy level structure corresponding to the nanocrystals. The fluorescence excitation spectrum reflects the change of the fluorescence emission intensity with the excitation energy (excitation wavelength) under the premise of a fixed fluorescence emission position. In general, only when the size of the nanocrystals is monodisperse can the exciton state of the nanocrystals be monodisperse. Under this condition, the fluorescence contributions of different emission peaks in the fluorescence spectrum come from the same nanoparticle, and the PLE spectra of the nanocrystals at different emission positions will be completely consistent.

[0150] Figure 2(g) is the absorption spectrum and fluorescence emission spectrum corresponding to 21nm CdSe cubic nanocrystals. The absorption spectrum has no obvious discernible exciton absorption peak, showing a quasi-continuous band absorption similar to the bulk phase, and its corresponding fluorescence emission peak reaches 1.69eV, which is very close to the zinc blende CdSe bulk phase band gap of 1.66eV (300K). These bulk-like properties indicate that 21nm CdSe cubic nanocrystals have only a weak quantum confinement effect and belong to weakly confined nanocrystals. In addition, it is worth noting that the half-peak width of the corresponding fluorescence spectrum is not lower than the fluorescence half-peak width of small-sized strongly confined quantum dots as predicted in the literature, but widens to 78meV, and the fluorescence spectrum slightly tails to high energy, showing an asymmetric phenomenon.

[0151]

Figure 3

[0152] Figure 3 The figure is a characterization result of a 21 nm CdS cubic nanocrystal, which is prepared by the method of the embodiment.

[0153] Figure 3 (a) shows a uniform and regular square two-dimensional projection in the TEM image, and the relative standard deviation of its size distribution is only 5% ( Figure 3 a upper left graph), illustrating that the CdS cubic nanocrystals have good monodispersity in size and morphology.

[0154] Figure 3 The high-resolution electron microscopy characterization results of (b, c, d) show that the CdS nanocrystals are sphalerite crystals with good single crystallinity and regular cubic morphology.

[0155] Figure 3 The XRD characterization results in (e) that strictly correspond to the diffraction peaks of the standard card also show the zinc blende structure of the CdS cubic nanocrystals, and the extremely narrow diffraction peaks are consistent with the larger size of the CdS nanocrystals.

[0156] The above characterization results show that the prepared CdS cubic nanocrystals are monodisperse in size and morphology and have a sphalerite single crystal structure with excellent crystallinity.

[0157] Figure 3 The completely overlapping PLE spectra at different corresponding fluorescence emission positions in (f) indicate that the CdS cubic nanocrystals have good size and morphology monodispersity, and their size distribution does not affect the exciton energy level structure corresponding to the nanocrystals.

[0158] Figure 3(g) is the corresponding absorption spectrum and fluorescence emission spectrum. Compared with CdSe cubic nanocrystals, the normalized absorption spectrum corresponding to CdS cubic nanocrystals shows a more bulk-like quasi-continuous band absorption, and its corresponding fluorescence emission peak reaches 2.38eV, which is consistent with the band gap of bulk zinc blende CdS reported in the literature of 2.38eV (300K). This is because the CdS exciton Bohr radius is only about 2.6nm, and the 21nm CdS cubic nanocrystals are in the category of extremely weakly confined nanocrystals, so their spectral properties are extremely similar to those of bulk CdS. Similar to weakly confined CdSe cubic nanocrystals, the fluorescence half-peak width of CdS cubic nanocrystals is also very wide, reaching 95meV, but its corresponding fluorescence spectrum does not have obvious asymmetry. This is because the two lowest emission energy levels of CdS in this size range are very close, resulting in roughly equal double-peak emission intensities, which only broadens the fluorescence spectrum without showing obvious asymmetry.

[0159]

Figure 4

[0160] Figure 4 These are the characterization results of 20 nm CdSe8 / CdS cubic nanocrystals prepared by using 8 nm CdSe cubic nanocrystals as nanocrystal seeds and subsequently adding S-ODE precursor. The CdSe8 / CdS cubic nanocrystals were prepared using the method of the embodiment.

[0161] Figure 4 The TEM images in (a) are all uniform and regular square two-dimensional projections and the standard deviation of the size distribution is only 4%, which indicates that the size and morphology of CdSe8 / CdS cubic nanocrystals maintain a good monodisperse level.

[0162] Figure 4 In the high-resolution electron microscopy characterization results of (c, d, e): clear single-period lattice fringes without dislocation and atomically smooth boundaries indicate that CdSe8 / CdS nanocrystals have good single crystallinity and regular cubic morphology. Figure 4 The element distribution diagram in (b) shows that the nanocrystal is a CdSe / CdS core-shell structure in which CdS completely covers CdSe, and the interplanar spacing of its specific crystal plane is between the interplanar spacing of the corresponding crystal planes of sphalerite CdSe and CdS, which indicates that the nanocrystal is a sphalerite crystal type.

[0163] Figure 4 The XRD characterization results in (f) show that the diffraction peak position is between the sphalerite CdSe and CdS standard cards, which further proves the good sphalerite structure of CdSe8 / CdS core-shell nanocrystals.

[0164] The above structural characterization results show that the prepared CdSe8 / CdS cubic nanocrystals have a zinc blende single crystal structure with monodisperse size and morphology and excellent crystallinity.

[0165] Completely overlapping PLE spectra at different fluorescence emission positions ( Figure 4 g) also illustrates the monodispersity of its size morphology and its monodisperse exciton state. Similar to weakly confined CdSe and CdS, its normalized absorption spectrum also exhibits a bulk-like quasi-continuous band absorption ( Figure 4 h), which shows that 20nm CdSe8 / CdS cubic nanocrystals also belong to the category of weakly confined nanocrystals. Due to the contribution of the epitaxial CdS shell, the absorbance of CdSe8 / CdS at short wavelengths is significantly higher than that of CdSe nanocrystals. In addition, CdSe forms a quasi-type II core-shell structure after epitaxy of CdS, and at this time the epitaxial CdS shell has a certain confinement effect on holes. Therefore, compared with CdSe cubic nanocrystals of the same size, the band edge absorption and emission peak energy corresponding to CdSe8 / CdS cubic nanocrystals are higher. It is worth noting that the half-peak width of the fluorescence spectrum corresponding to the weakly confined CdSe8 / CdS cubic nanocrystals of this size is also wide (70meV) and the fluorescence spectrum tails to high energy, showing obvious asymmetric characteristics.

[0166]

Figure 5

[0167] Figure 5 These are the characterization results of 22 nm CdSe12 / CdS cubic nanocrystals grown by using 12 nm CdSe cubic nanocrystals as seeds and subsequently dropping S-ODE precursor. The CdSe12 / CdS cubic nanocrystals were prepared by the method of the embodiment.

[0168] Similar to large-sized CdSe, CdS, and CdSe8 / CdS cubic nanocrystals, Figure 5 The TEM images in a are uniform and regular square two-dimensional projections and the standard deviation of the size distribution is only 3%, which indicates that the size and morphology of the 22nm CdSe12 / CdS cubic nanocrystals have also reached a monodisperse level.

[0169] Figure 5 In the high-resolution electron microscopy characterization results of (c, d, e): clear single-period lattice fringes without dislocation and atomically smooth boundaries indicate that CdSe12 / CdS nanocrystals have good single crystallinity and regular cubic morphology. Figure 5 The element distribution diagram in (b) shows that the nanocrystal is a CdSe / CdS core-shell structure in which CdS completely covers CdSe, and the interplanar spacing of its specific crystal planes ( Figure 5c) is between the interplanar spacing of the corresponding crystal planes of sphalerite CdSe and CdS, which indicates that the nanocrystal is a sphalerite crystal type.

[0170] Figure 5 In the XRD characterization results of (f), the diffraction peak position is between the zinc blende CdSe and CdS standard cards, indicating that the CdSe12 / CdS core-shell nanocrystals have a good zinc blende structure.

[0171] The above characterization results indicate that the prepared CdSe12 / CdS cubic nanocrystals have reached a level of monodisperse size and morphology and have a sphalerite single crystal structure with excellent crystallinity.

[0172] Completely overlapping PLE spectra at different fluorescence emission positions ( Figure 5 d) illustrates the monodispersity of its size morphology and its monodisperse exciton state. Similar to weakly confined CdSe, CdS, and CdSe8 / CdS cubic nanocrystals, its normalized absorption spectrum also shows a quasi-continuous band absorption similar to the bulk phase, which indicates that the 22nm CdSe12 / CdS cubic nanocrystals also belong to the category of weakly confined nanocrystals, and due to the contribution of the epitaxial CdS shell, the absorbance of CdSe12 / CdS at short wavelengths is significantly higher than that of CdSe nanocrystals. In addition, similar to CdSe8 / CdS cubic nanocrystals, the band edge absorption and emission peak energy corresponding to CdSe12 / CdS cubic nanocrystals are higher than those of CdSe cubic nanocrystals of the same size. It is worth noting that the half-peak width of the fluorescence spectrum corresponding to the weakly confined CdSe12 / CdS cubic nanocrystals of this size is also wide (87meV) and the fluorescence spectrum also tails to high energy and shows obvious asymmetric characteristics.

[0173]

Figure 6

[0174] Normalized UV-visible absorption spectra / fluorescence emission spectra corresponding to CdSe cubic nanocrystals of different sizes are shown in Figure 2. Figure 6 As shown in (a), as the size of the nanocrystal increases, the central peak of the fluorescence spectrum and the band edge of the absorption spectrum gradually move toward the low energy direction, and the exciton absorption peak in the absorption spectrum gradually changes to a shoulder peak until it disappears and becomes a quasi-continuous band absorption feature similar to the bulk phase. When its size increases from 11nm to 13nm, the shoulder peak of the first exciton absorption peak of the corresponding absorption spectrum disappears. This also shows that as the size increases, the quantum confinement effect of CdSe nanocrystals gradually weakens and enters the weak confinement size range.

[0175] like Figure 6As shown in (b), the size of CdSe cubic nanocrystal increases from 5nm to 21nm, and its corresponding fluorescence peak moves from 1.88eV to 1.69eV. However, it is worth noting that the movement speed of the fluorescence peak is different in different size ranges. In the size range of 5nm to 12nm, the fluorescence peak corresponding to the CdSe cubic nanocrystal is monotonically red-shifted; in the size range of about 12nm to 17nm, the fluorescence is almost unchanged; in the range greater than about 17nm, the fluorescence peak is red-shifted again. From the Brus formula, it can be seen that the kinetic energy term (∝D -2 , D is the size of the nanocrystal). As the size of the nanocrystal increases, the kinetic energy brought by the quantum confinement effect gradually decreases and approaches zero, so the band gap of the nanocrystal gradually decreases and the decreasing speed also becomes slower and slower.

[0176] The half-peak width of the fluorescence spectrum of nanocrystals is a common indicator for evaluating the quality of nanocrystals. The half-peak width of the fluorescence of CdSe cubic nanocrystals varies with size. Figure 6 As shown in (c), when the size of CdSe cubic nanocrystals increases from 5nm to 21nm, the corresponding fluorescence half-peak width first gradually decreases to about 50meV, then rapidly increases to about 90meV, and then gradually decreases and fluctuates around 75meV. Considering the good size and morphology monodispersity of the prepared CdSe cubic nanocrystals, the change trend of the half-peak width of the fluorescence spectrum of the CdSe cubic nanocrystal aggregate here can also reflect the change trend of its intrinsic fluorescence half-peak width.

[0177] Figure 6 Some of the fluorescence spectra in (a) have obvious asymmetric characteristics of tailing to high energy, among which the fluorescence spectrum corresponding to the 12nm CdSe cubic nanocrystal has the most obvious asymmetry ( Figure 6 b illustration).

[0178] The calculated results of fluorescence spectra skewness corresponding to CdSe cubic nanocrystals of different sizes are shown in Figure 6 As shown in (c), as the size increases, the skewness of the fluorescence spectrum of CdSe cubic nanocrystals increases sharply and then decreases slightly. The size range where the skewness of the nanocrystal fluorescence peak increases sharply has a high correspondence with the range where the fluorescence half-peak width of the nanocrystal increases rapidly. This shows that the widening of the half-peak width of the fluorescence spectrum of CdSe cubic nanocrystals is caused by the tailing asymmetry of its fluorescence spectrum.

[0179] The exciton Bohr radius of CdSe is about 5.6nm, while the disappearance of the first exciton absorption peak in the absorption spectrum, the rapid increase in the fluorescence half-width and the size of the cubic CdSe nanocrystal corresponding to the maximum skewness of the fluorescence spectrum are all around 12nm, that is, near the CdSe exciton Bohr diameter. This is not a coincidence. It is generally believed that the exciton Bohr diameter is the basic condition for distinguishing the strength of the confinement effect of semiconductor nanocrystals.

[0180]

Figure 7

[0181] Normalized UV-visible absorption spectra / fluorescence emission spectra corresponding to CdS cubic nanocrystals of different sizes are shown in Figure 2. Figure 7 As shown in (a), similar to the size-related optical properties of CdSe cubic nanocrystals, as the size of the nanocrystals increases, the central peak of the fluorescence spectrum and the band edge of the absorption spectrum gradually move toward the low energy direction, and the exciton absorption peak in the absorption spectrum gradually disappears from the shoulder peak and turns into a quasi-continuous band absorption feature similar to the bulk phase.

[0182] like Figure 7 As shown in (b), when the size of CdS cubic nanocrystal increases from 8nm to 20nm, its corresponding fluorescence peak moves from 2.44eV to 2.38eV, the band gap of zinc blende CdS. This shows that the 20nm CdS cubic nanocrystal has already behaved as a bulk absorption material. In addition, its fluorescence peak also moves rapidly at first and then basically stops moving, which is basically consistent with the phenomenon of CdSe. In addition, when the size of CdS cubic nanocrystal reaches 8nm, its corresponding absorption spectrum band edge no longer has obvious exciton absorption peak but shows shoulder peak. This is because the CdS exciton Bohr radius is small, and the absorption band edge of 8nm CdS nanocrystal already has a higher energy level state density. When its size increases from 10nm to 12nm, the shoulder peak of the first exciton absorption peak of the corresponding absorption spectrum disappears completely. This also shows that with the increase of size, the quantum confinement effect gradually weakens, and the corresponding CdS cubic nanocrystal enters the category of weakly confined nanocrystals.

[0183] The fluorescence half-peak width of CdS cubic nanocrystals varies with size. Figure 7 As shown in (c), when the size of CdS cubic nanocrystal increases from 8nm to 20nm, its corresponding fluorescence half-peak width first increases rapidly to about 100meV and then decreases slightly. This is different from the change trend of the fluorescence half-peak width of CdSe nanocrystal with size.

[0184] The calculated results of fluorescence spectra skewness corresponding to CdS cubic nanocrystals of different sizes show that ( Figure 7d), when the size of CdSe cubic nanocrystals increases from 8nm to 20nm, the skewness of the fluorescence spectrum of CdS cubic nanocrystals gradually decreases. This is different from the trend of the skewness of the fluorescence spectrum of CdSe nanocrystals changing with size, which shows that the size-related optical properties corresponding to CdSe and CdS are different. This is because the exciton Bohr radius of the two is different, and the intensity of the confinement effect of the two is different within the same size range. The exciton Bohr radius of CdSe nanocrystals is about twice that of CdS nanocrystals, which means that the confinement effect of 8nm CdS nanocrystals is roughly equivalent to the confinement effect of 16nm CdSe nanocrystals. From this perspective, the spectral behavior corresponding to CdS cubic nanocrystals with a size of more than 8nm should be close to that of CdSe cubic nanocrystals with a size of more than 16nm, which is basically consistent with the experimental results. The calculation results of the skewness show that the fluorescence spectrum corresponding to CdS cubic nanocrystals is also asymmetric and the fluorescence spectrum is also more biased towards high energy. This is consistent with the phenomenon of the fluorescence spectrum of CdSe cubic nanocrystals. This shows that as the size of nanocrystals increases, the fluorescence spectrum becomes asymmetric, which is a common feature of CdSe and CdS nanocrystals.

[0185]

Figure 8

[0186] CdSe8 / yCdS (y is the number of CdS monomolecular shells) cubic nanocrystals prepared by epitaxial CdS shells in the synthesis route of large-sized CdE cubic nanocrystals with 8nm CdSe cubic nanocrystals as nanocrystal seeds are studied. The normalized absorption spectra of CdSe8 / yCdS cubic nanocrystals with different CdS shell thicknesses are shown in Figure 2. Figure 8 As shown in (a), as the thickness of the CdS shell increases, the absorbance at high energy in the corresponding absorption spectrum gradually increases and the exciton absorption peak characteristics in the corresponding absorption spectrum gradually disappear and show a quasi-continuous band absorption feature similar to the bulk phase. This shows that the edge state density of the absorption band of CdSe8 / yCdS cubic nanocrystals gradually increases and shows weak confinement characteristics.

[0187] The normalized fluorescence spectra of CdSe8 / yCdS cubic nanocrystals with different CdS shell thicknesses are shown in Figure 2. Figure 8 As shown in (b), as the thickness of the CdS shell increases, the corresponding fluorescence peak moves about 20 meV to a lower energy. Figure 8d), after 8nm CdSe cubic nanocrystals were epitaxially grown with 5 layers of CdS, their fluorescence peak moved from 1.78eV to 1.76eV. After further epitaxial growth of CdS, its overall fluorescence peak slightly moved to higher energy. From the Brus formula, we can see that as the size of the nanocrystal increases, its band gap gradually decreases, and its fluorescence peak should also move to lower energy. For CdSe / CdS quasi-type II core-shell nanocrystals, although only electrons can be delocalized in the entire nanocrystal, it should still have a size-related quantum confinement effect. From this perspective, even if the CdSe8 / yCdS nanocrystals are in the weak confinement range, their corresponding fluorescence peak should not move to higher energy as the thickness of the CdS shell increases.

[0188] The fluorescence spectra of CdSe8 / yCdS cubic nanocrystals with different CdS shell thicknesses were analyzed. Figure 8 As shown in (e), with the increase of CdS shell thickness, the skewness of the fluorescence spectrum corresponding to CdSe8 / yCdS gradually increases and the half-peak width of the fluorescence spectrum also gradually increases. Figure 8 It can also be seen in (b) that as the thickness of the CdS shell increases, the high energy of the fluorescence spectrum corresponding to CdSe8 / yCdS gradually rises. This shows that the fluorescence spectrum corresponding to CdSe8 / yCdS cubic nanocrystals also has asymmetric characteristics. In addition, it is worth noting that Figure 8 In (b), although the peak of the fluorescence spectrum slightly moves toward the high energy direction with the increase of the CdS shell thickness, the low energy falling edge of the fluorescence spectrum basically coincides. This shows that the peak of the fluorescence spectrum moves toward the high energy direction because the fluorescence spectrum gradually tails toward the high energy, that is, this abnormal phenomenon is also caused by the asymmetry of the fluorescence peak.

[0189] The transient fluorescence spectra of CdSe8 / yCdS cubic nanocrystals with different CdS shell thicknesses are shown in Figure 2. Figure 8 As shown in (c), as the thickness of the CdS shell increases, the corresponding fluorescence lifetime of CdSe8 / yCdS gradually increases. Figure 8 f shows that after epitaxial 2 CdS shell layers, the corresponding fluorescence lifetime of CdSe8 / 2CdS is about 38ns, while after epitaxial 18 CdS shell layers, the corresponding fluorescence lifetime of CdSe8 / 18CdS reaches 73ns. In addition, although the goodness of fit of transient fluorescence increases with the increase of CdS shell layers, 2 It gradually increases, but its value is still lower than 1.3, so the transient fluorescence spectrum corresponding to CdSe8 / yCdS cubic nanocrystals has the characteristics of composite single-channel attenuation. From this perspective, the CdSe8 / yCdS cubic nanocrystals synthesized under the weak confinement CdE cubic nanocrystal synthesis strategy have good optical properties.

[0190]

Fig. 9

[0191] CdSe12 / yCdS cubic nanocrystals prepared by epitaxial CdS shell with 12nm CdSe cubic nanocrystals as nanocrystal seeds are used as research objects. The normalized absorption spectra of CdSe12 / yCdS cubic nanocrystals with different CdS shells are shown in Figure 2. Fig. 9 As shown in (a), with the increase of CdS shell thickness, similar to CdSe8 / yCdS cubic nanocrystals, the absorbance at high energy in its corresponding absorption spectrum also gradually increases. And its corresponding absorption spectrum always shows a quasi-continuous band absorption feature similar to the bulk phase. This shows that CdSe12 / yCdS cubic nanocrystals also belong to the category of weakly confined nanocrystals.

[0192] The normalized fluorescence spectra of CdSe12 / yCdS cubic nanocrystals with different CdS shell thicknesses are shown in Figure 2. Fig. 9 As shown in (b), as the thickness of the CdS shell increases, its corresponding fluorescence peak continues to move toward higher energy. Fig. 9 d), after 19 layers of CdS were epitaxially added to the 12nm CdSe cubic nanocrystal, its fluorescence peak moved from 1.725eV to 1.739eV. This is the same trend as the movement of the fluorescence position of some CdSe8 / yCdS cubic nanocrystals, indicating that with the increase of the thickness of the CdS shell, it is not accidental that the fluorescence peak of CdSex / yCdS cubic nanocrystals moves to higher energy, but it is more likely a common feature of weakly confined CdSex / yCdS nanocrystals. In addition, similar to CdSe8 / yCdS cubic nanocrystals, Fig. 9 In (b), although the peak position of the fluorescence spectrum of CdSe12 / yCdS cubic nanocrystals slightly moves toward the high energy direction with the increase of CdS shell thickness, the low energy falling edge of the fluorescence spectrum is basically coincident. This shows that the peak position of the fluorescence spectrum moves toward the high energy direction because the fluorescence spectrum gradually tails toward the high energy.

[0193] The fluorescence spectra of CdSe12 / yCdS cubic nanocrystals with different CdS shell thicknesses were analyzed. Fig. 9 As shown in (e), with the increase of CdS shell thickness, the skewness and half-peak width of the fluorescence spectrum of CdSe12 / yCdS cubic nanocrystals also gradually increase. Fig. 9 It can be seen more clearly in (b) that with the increase of CdS shell thickness, the fluorescence spectrum corresponding to CdSe12 / yCdS tails more and more seriously towards high energy. This shows that the fluorescence spectrum corresponding to CdSe12 / yCdS cubic nanocrystals also has obvious asymmetric characteristics.

[0194] The fluorescence spectrum of the aggregate corresponding to CdSe12 / 20CdS cubic nanocrystals and the fluorescence spectrum of a single particle completely overlap ( Fig. 9 d), which indicates that it has good monodispersity and its aggregate fluorescence spectrum can reflect its intrinsic fluorescence properties. Combined with the above CdSe, CdS and CdSe8 / yCdS cubic nanocrystal fluorescence spectra, they also have different degrees of asymmetric characteristics, indicating that the asymmetry of the fluorescence spectrum is an intrinsic commonality of weakly confined CdE cubic nanocrystals.

[0195] The transient fluorescence spectra of CdSe12 / yCdS cubic nanocrystals with different CdS shell thicknesses are shown in Figure 2. Fig. 9 As shown in (c), as the thickness of the CdS shell increases, the corresponding fluorescence lifetime of CdSe12 / yCdS also gradually increases. Fig. 9 f), after epitaxial 6 layers of CdS shell, the corresponding fluorescence lifetime of CdSe12 / 6CdS reaches about 75ns, while after epitaxial 19 layers of CdS shell, the corresponding fluorescence lifetime of CdSe12 / 19CdS is close to 200ns. However, with the increase of CdS shell, the single exponential of the transient fluorescence spectrum corresponding to CdSe12 / yCdS cubic nanocrystals becomes significantly worse. Specifically, after epitaxial 19 layers of CdS shell, the fitting goodness of the transient fluorescence of CdSe12 / 19CdS is 2 It is close to 2.0, which indicates that there are multiple channels in the fluorescence decay process of CdSe12 / 19CdS cubic nanocrystals. It is worth noting that for CdSe12 / 19CdS cubic nanocrystals with a fluorescence lifetime close to 200ns, their exciton decay rate is orders of magnitude different from that of CdSe3 / CdS nanocrystals with a common fluorescence lifetime of about 20ns.

[0196]

Fig.10

[0197] Fig.10 The power-related fluorescence spectrum of 15nm CdSe cubic nanocrystals. As the excitation intensity increases, the corresponding fluorescence intensity continues to increase. Further integration calculation of the fluorescence spectrum, the excitation power increases from 4μW to 3430μW, and the linear fit goodness of fluorescence intensity and excitation power reaches 0.9999, which shows that when the excitation power ranges from 4μW to 3430μW, the fluorescence emission process of 15nm CdSe cubic nanocrystals is a single exciton emission process.

[0198] In the conventional steady-state fluorescence spectrum measurement process (low excitation power, tens of μW), an electron in the corresponding valence band of the nanocrystal is excited to the energy level of the conduction band, and a hole is generated in the valence band. Then the conduction band electron quickly relaxes to the bottom of the conduction band and recombine with the hole at the top of the valence band to emit a photon to produce single exciton fluorescence. The fluorescence intensity of the single exciton state increases linearly with the increase of the excitation power. However, when the excitation power is large, multiple pairs of photogenerated excitons will be generated in the nanocrystal, and then multi-exciton emission will occur, and at this time the fluorescence intensity of the multi-exciton state will no longer increase linearly with the excitation power.

[0199] Considering that the excitation power in the conventional fluorescence spectrum measurement process is only tens of microwatts, the following conclusion can be drawn: for the conventional fluorescence measurement of 15nm CdSe cubic nanocrystals, their fluorescence spectra are all single exciton state fluorescence emission spectra without the interference of multi-exciton state emission.

[0200] The normalized fluorescence spectra of CdSe cubic nanocrystals at different powers are shown in Figure 2. Fig.10 As shown in the inset of (a), their fluorescence spectra completely overlap and both have obvious asymmetric characteristics of tailing to high energy. This shows that the fluorescence spectra corresponding to CdSe cubic nanocrystals at different powers are only different in fluorescence intensity, and the fluorescence peak shape does not change significantly. This once again proves that the double-peak emission of CdE weakly confined cubic nanocrystals in this power range is single exciton state fluorescence emission.

[0201]

Fig.11

[0202] Fig.11 The power-dependent fluorescence spectrum of CdSe8 / 20CdS cubic nanocrystals. When the excitation power increases from 1μW to 1600μW, the linear fit goodness of the fluorescence intensity and the excitation power reaches 0.9999, which means that when the excitation power ranges from 1μW to 1600μW, the fluorescence emission process of CdSe8 / 20CdS cubic nanocrystals is a single exciton emission process. Considering that the excitation power in the conventional fluorescence spectrum measurement process is only tens of microwatts, the following conclusion can be drawn: For the conventional fluorescence measurement of CdSe8 / 20CdS cubic nanocrystals, its fluorescence spectrum is a single exciton state fluorescence emission spectrum.

[0203] Normalized fluorescence spectra of CdSe8 / 20CdS cubic nanocrystals at different powers ( Fig.11 The inset in a) completely overlap and both have obvious asymmetric characteristics of tailing to high energy. This shows that the fluorescence spectra corresponding to CdSe8 / 20CdS cubic nanocrystals at different powers are only different in fluorescence intensity, and the fluorescence peak shape does not change significantly. This once again proves the conclusion that CdSe8 / 20CdS cubic nanocrystals are in the same single exciton state fluorescence emission within this power range.

[0204] Single particle spectroscopy is a common method to characterize the intrinsic optical properties of nanocrystals. The corresponding aggregate spectrum and single particle fluorescence spectrum of CdSe8 / 20CdS cubic nanocrystals ( Fig.11 c) overlap and both have asymmetric characteristics of tailing to high energy. This fully proves that the spectrum of CdSex / yCdS cubic nanocrystal aggregates with monodisperse size and morphology can truly reflect its intrinsic optical properties, and this proves that the fluorescence spectrum of CdE cubic nanocrystals of a certain size has asymmetric characteristics.

[0205] The fluorescence spectra of nanocrystals with different charge states are also different, and the fluorescence lifetimes of nanocrystals with different charges will be significantly different. Fig.11 (d) shows that there is no short-lived charged state emission. Fig.11 (d) The upper part shows the fluorescence emission spectrum of CdSe8 / 20CdS cubic nanocrystals and its double Gaussian fitting result. The perfect fitting result indicates that the apparent asymmetric fluorescence spectrum may contain two fluorescence emission peaks with different energies. Fig.11 (d) The lower part is the transient fluorescence spectra corresponding to the two fitting peaks and the intrinsic fluorescence spectrum peak. The almost completely overlapping transient fluorescence spectra indicate that there is no obvious difference in the fluorescence lifetime of the nanocrystals at different emission positions, that is, there is no obvious difference in the decay rate of the exciton decay process corresponding to the high energy fitting peak and the apparent fluorescence peak and the low energy fitting peak. This also excludes the possibility that the nanocrystal is in a charged state, resulting in the asymmetry of its fluorescence spectrum.

[0206] The power-related experiments of CdSe and CdSe8 / 20CdS cubic nanocrystals ruled out the possibility that the nanocrystals were in a multi-exciton state during conventional fluorescence testing; the transient fluorescence tests of CdSe8 / 20CdS cubic nanocrystals at different emission positions ruled out the possibility that the nanocrystals were in a charged state during conventional fluorescence testing; the comparison of the fluorescence spectra of single particles and the fluorescence spectra of the aggregate of CdSe8 / 20CdS cubic nanocrystals proved the intrinsic nature of its fluorescence spectrum. These experimental results fully prove that the fluorescence spectrum of the aggregate of CdE cubic nanocrystals with monodispersed size and morphology under conventional testing conditions can reflect its intrinsic fluorescence spectrum properties, that is, the asymmetry of the fluorescence spectrum within a certain size range is its intrinsic characteristic.

[0207] Through the fitting analysis of the spectra of CdSe and CdS cubic nanocrystals, it is proved that within a certain size range, the fluorescence spectra of CdSe and CdS cubic nanocrystals both contain fluorescence emission peaks of two exciton states at the same time. The energy levels of the two exciton states of the two fluorescence spectra are further attributed in combination with the theoretical energy level calculation results of cubic nanocrystals. The experimental results show that CdS and CdSe cubic nanocrystals have similar size-related optical properties, and both have dual-level emission fluorescence properties.

[0208]

Fig.12

[0209] The fluorescence lifetime of CdSex / yCdS cubic nanocrystals with different sizes of CdSe epitaxy and different CdS thickness varies with temperature. Fig.12 As shown. The fluorescence lifetimes of different types of CdSex / yCdS cubic nanocrystals at different temperatures are different. Under the same temperature conditions, considering the degree of exciton confinement effect, the fluorescence lifetime of CdSex / yCdS cubic nanocrystals should increase gradually with the increase of nanocrystal size. Taking room temperature as an example, Fig.12 The size-related fluorescence lifetime of CdSex / yCdS cubic nanocrystals in (a) roughly conforms to this trend. However, the fluorescence lifetimes of CdSe3 / 10CdS and CdSe3 / 15CdS do not conform to this trend. Specifically, the fluorescence lifetime of CdSe3 / 10CdS (9nm) is higher than that of CdSe5 / 10CdS (11nm) and CdSe5 / 15CdS (14nm), and the fluorescence lifetime of CdSe3 / 15CdS (11nm) is even higher than that of CdSe8 / 10CdS (14nm) and CdSe5 / 15CdS (14nm). This shows that the fluorescence lifetime of CdSex / yCdS cubic nanocrystals is not simply proportional to the size of the nanocrystal. For quasi-type II CdSex / yCdS nanocrystals, in general, the hole wave function is effectively confined in the CdSe core, while the electron is delocalized throughout the nanocrystal. The Bohr diameter of CdSe holes is 2.2nm. In a 3nm CdSe core, the hole wave function is effectively confined to the core space, while in a 5nm or even larger 8nm CdSe core, its wave function will no longer be significantly confined and will have a larger spatial range. Therefore, under the same conditions of the spatial distribution of the electron wave function (the same size of CdSex / yCdS nanocrystals), the larger the size of the CdSe core, the higher the probability that the electron and hole will meet and recombine to emit photons, and the corresponding fluorescence lifetime will be lower.

[0210] On the other hand, the fluorescence lifetimes of different types of CdSex / yCdS cubic nanocrystals change at different rates with temperature. Fig.12As shown in (a), when the temperature increases from 280K to 358K, the fluorescence lifetime of CdSe3 / 5CdS only increases from 21ns to 26ns, while the fluorescence lifetime of CdSe5 / 15CdS increases from 37ns to 72ns.

[0211] In order to further compare the change rate of the fluorescence lifetime of different types of CdSex / yCdS cubic nanocrystals with temperature, the temperature starting point (279.15K) was unified and the relative change rate of the corresponding fluorescence lifetime was calculated ( Fig.12 b). The relative rate of change of lifetime with temperature has obvious size correlation. Specifically, within the same temperature range, when the size range of CdSex / yCdS cubic nanocrystals is 6-9nm, the relative rate of change of fluorescence lifetime increases from 1 to about 1.3; when the size range of CdSex / yCdS cubic nanocrystals is 11-14nm, the relative rate of change of fluorescence lifetime increases from 1 to about 1.6; when the size range of CdSex / yCdS cubic nanocrystals is 14-17nm, the relative rate of change of fluorescence lifetime increases from 1 to about 2. This should be related to the exciton binding energy related to the size of CdSex / yCdS cubic nanocrystals. As the size of CdSex / yCdS cubic nanocrystals increases, the corresponding confinement effect gradually decreases, and the exciton binding energy gradually decreases. As the temperature increases, the proportion of electron holes in the form of free carriers in weakly confined CdSex / yCdS cubic nanocrystals increases, so the corresponding rate of change of fluorescence lifetime with temperature gradually increases. Fig.12 In (b), the three CdSex / yCdS cubic nanocrystal size ranges should correspond to three size ranges with different confinement effects. Compared with CdSe and CdS nanocrystals, which can directly distinguish the strength of their corresponding confinement effects based on their exciton Bohr radius, the strength of the confinement effect of CdSex / yCdS cubic nanocrystals can also be distinguished based on the temperature change rate of their corresponding fluorescence lifetime.

[0212]

Fig.13

[0213] like Fig.13As shown in the figure, both CdSe8 / 20CdS and CdSe12 / 20CdS exhibit excellent photostability, and the single particle fluorescence corresponding to the CdSe12 / 20CdS cubic nanocrystals does not show fluorescence flickering for a period of up to 1000 seconds. The biexciton fluorescence yield of CdSe8 / 20CdS reaches 79%, and the biexciton fluorescence yield corresponding to CdSe12 / 20CdS is even as high as 99%, which means that there is almost no interference from the Auger process during the biexciton emission process. This is great news for high-power devices (such as LEDs, lasers, etc.) whose device efficiency has been restricted by the Auger effect. Considering that the corresponding fluorescence lifetime reaches hundreds of nanoseconds and the regular cubic morphology is conducive to close-packed assembly to increase the electron-hole transfer rate, the weakly confined CdSex / yCdS cubic nanocrystals also have great application value in the photovoltaic field.

[0214] The above describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention to be protected. The scope of protection claimed by the present invention is defined by the attached claims and their equivalents.

Claims

1. A weakly confined semiconductor nanocrystal, characterized in that: The size of the nanocrystal is larger than its exciton diameter. The nanocrystal is a cubic nanocrystal with a size larger than 10 nm. The synthesis of the nanocrystal uses a cubic nanocrystal with a size ≤10 nm as a seed. The ligands in the synthesis process include fatty acids with a carbon number of not less than 22. The size of the nanocrystal is the average value of its diameter or the average value of its centroid length. The exciton of the nanocrystal is a dynamic exciton. At the operating temperature, the electron-hole Coulomb interaction of the dynamic exciton is not sufficient to bind each other to form a stable combined exciton. The electrons and holes of the dynamic exciton are constrained by the boundary of the nanocrystal. The operating temperature includes room temperature. The transmission electron microscope photograph of the nanocrystal shows that the nanocrystal has a square two-dimensional projection. The high-resolution transmission electron microscope photograph shows that the nanocrystal has a single-period lattice stripe without dislocation and an atomically flat boundary.

2. A weakly confined semiconductor nanocrystal, characterized in that: The size of the nanocrystal is larger than its exciton diameter, the nanocrystal is a cubic nanocrystal with a size larger than 10 nm, the synthesis of the nanocrystal uses cubic nanocrystals with a size ≤10 nm as seeds, the ligands of the synthesis process include fatty acids with a carbon number of not less than 22, the size of the nanocrystal is the average value of its diameter or the average value of the length through its center of mass, under room temperature test conditions, the ultraviolet-visible absorption spectrum of the nanocrystal exhibits quasi-continuous band absorption, the transmission electron microscope photograph of the nanocrystal shows that the nanocrystal has a square two-dimensional projection, and the high-resolution transmission electron microscope photograph shows that the nanocrystal has single-period non-dislocated lattice fringes and atomically smooth boundaries.

3. A weakly confined semiconductor nanocrystal, characterized in that: The size of the nanocrystal is larger than its exciton diameter, the nanocrystal is a cubic nanocrystal with a size larger than 10 nm, the synthesis of the nanocrystal uses cubic nanocrystals with a size ≤10 nm as seeds, the ligands of the synthesis process include fatty acids with a carbon number of not less than 22, the size of the nanocrystal is the average value of its diameter or the average value of the length through its center of mass, under room temperature test conditions, the fluorescence spectrum of the nanocrystal has an asymmetric feature of tailing to high energy, the transmission electron microscope photograph of the nanocrystal shows that the nanocrystal has a square two-dimensional projection, and the high-resolution transmission electron microscope photograph shows that the nanocrystal has single-period non-dislocated lattice stripes and atomically smooth boundaries.

4. A weakly confined semiconductor nanocrystal, characterized in that: The size of the nanocrystal is larger than its exciton diameter, the nanocrystal is a cubic nanocrystal with a size larger than 10 nm, the synthesis of the nanocrystal uses cubic nanocrystals with a size ≤10 nm as seeds, the ligands of the synthesis process include fatty acids with a carbon number of not less than 22, the size of the nanocrystal is the average value of its diameter or the average value of the length through its center of mass, and under room temperature test conditions, the double Gaussian fitting results of the fluorescence emission spectrum of the nanocrystal show that the fluorescence emission spectrum of the nanocrystal contains two fluorescence emission peaks with different energies, that is, the nanocrystal has a fluorescence property of dual-level emission, the transmission electron microscope photograph of the nanocrystal shows that the nanocrystal has a square two-dimensional projection, and the high-resolution transmission electron microscope photograph shows that the nanocrystal has single-period non-dislocated lattice fringes and atomically smooth boundaries.

5. A weakly confined semiconductor nanocrystal, characterized in that: The size of the nanocrystal is larger than its exciton diameter, the nanocrystal is a cubic nanocrystal with a size larger than 10 nm, the synthesis of the nanocrystal uses cubic nanocrystals with a size ≤10 nm as seeds, the ligands of the synthesis process include fatty acids with a carbon number of not less than 22, the size of the nanocrystal is the average value of its diameter or the average value of the length through its center of mass, the biexciton fluorescence quantum yield of the nanocrystal is not less than 50%, the transmission electron microscope photograph of the nanocrystal shows that the nanocrystal has a square two-dimensional projection, and the high-resolution transmission electron microscope photograph shows that the nanocrystal has single-period non-dislocated lattice fringes and atomically smooth boundaries.

6. The weakly confined semiconductor nanocrystal according to claim 5, characterized in that: The biexciton fluorescence quantum yield of the nanocrystal is not less than 70%.

7. The weakly confined semiconductor nanocrystal according to claim 6, characterized in that: The biexciton fluorescence quantum yield of the nanocrystal is not less than 80%.

8. The weakly confined semiconductor nanocrystal according to claim 7, characterized in that: The biexciton fluorescence quantum yield of the nanocrystal is not less than 90%.

9. The weakly confined semiconductor nanocrystal according to claim 8, characterized in that: The biexciton fluorescence quantum yield of the nanocrystal is not less than 95%.

10. The weakly confined semiconductor nanocrystal according to any one of claims 1 to 9, characterized in that: The size of the nanocrystal is 1 to 20 times of its exciton diameter.

11. The weakly confined semiconductor nanocrystal according to claim 10, characterized in that: The size of the nanocrystal is 1 to 6 times the diameter of its exciton.

12. The weakly confined semiconductor nanocrystal according to any one of claims 1 to 9, characterized in that: The size of the nanocrystals is greater than 15 nm.

13. The weakly confined semiconductor nanocrystal according to claim 12, characterized in that: The size of the nanocrystal is greater than 20 nm.

14. The weakly confined semiconductor nanocrystal according to claim 13, characterized in that: The size of the nanocrystals is greater than 25 nm.

15. The weakly confined semiconductor nanocrystal according to claim 14, characterized in that: The size of the nanocrystal is greater than or equal to 30 nm.

16. The weakly confined semiconductor nanocrystal according to any one of claims 1 to 9, characterized in that: The relative standard deviation of the size distribution of the nanocrystals does not exceed 10%.

17. The weakly confined semiconductor nanocrystal according to claim 16, characterized in that: The relative standard deviation of the size distribution of the nanocrystals does not exceed 6%.

18. The weakly confined semiconductor nanocrystal according to claim 17, characterized in that: The relative standard deviation of the size distribution of the nanocrystals does not exceed 5%.

19. The weakly confined semiconductor nanocrystal according to claim 18, characterized in that: The relative standard deviation of the size distribution of the nanocrystals does not exceed 4%.

20. The weakly confined semiconductor nanocrystal according to claim 19, characterized in that: The relative standard deviation of the size distribution of the nanocrystals does not exceed 3%.

21. The weakly confined semiconductor nanocrystal according to any one of claims 1 to 9, characterized in that: The nanocrystals are CdS or CdSe cubic nanocrystals.

22. The weakly confined semiconductor nanocrystal according to any one of claims 1 to 9, characterized in that: The nanocrystal is a II-IV semiconductor or a III-V semiconductor.

23. The weakly confined semiconductor nanocrystal according to any one of claims 1 to 9, characterized in that: The nanocrystal is a zinc blende single crystal structure.

24. The weakly confined semiconductor nanocrystal according to any one of claims 1 to 9, characterized in that: The excitation spectra of the nanocrystals at different fluorescence emission positions substantially overlap.

25. The weakly confined semiconductor nanocrystal according to any one of claims 1 to 9, characterized in that: The fluorescence emission peak position of the nanocrystal is substantially consistent with the band gap width of its bulk material.

26. A method for preparing a weakly confined semiconductor nanocrystal according to any one of claims 1 to 25, characterized in that: The following steps are involved: Synthesis of nanocrystal seeds: a cationic precursor reacts with a first fatty acid at a first temperature, and then a first anionic precursor is added to react to obtain nanocrystal seeds, wherein the size of the nanocrystal seeds is smaller than the exciton diameter thereof, and the size of the nanocrystal seeds is the average value of the diameter thereof or the average value of the length passing through the center of mass thereof; Growth of cubic nanocrystals with a size of less than 10 nm: reacting a cationic precursor, a first fatty acid and a fatty acid chloride, and then sequentially adding the nanocrystal seed and a second anionic precursor for growth to obtain cubic nanocrystals with a size of less than 10 nm; Growth of cubic nanocrystals with a size of more than 10 nm: a cationic precursor, a first fatty acid, a second fatty acid and a fatty acid chloride are mixed and reacted, and then the cubic nanocrystals with a size of less than 10 nm and a second anionic precursor are added in sequence for growth to obtain nanocrystals with a size greater than 10 nm, wherein the size of the nanocrystal is not less than its exciton diameter, and the size of the nanocrystal is the average value of its diameter or the average value of its center of mass length; Among them, the first fatty acid is a fatty acid with a carbon number of not less than 10 and not more than 18, and the second fatty acid is a fatty acid with a carbon number of not less than 22.

27. The method for preparing weakly confined semiconductor nanocrystals according to claim 26, characterized in that: The cation precursor is cadmium carboxylate, and the first anion precursor is a Se precursor or a S precursor.

28. The use of the weakly confined semiconductor nanocrystal according to any one of claims 1 to 25, characterized in that: Used for lighting.

29. The use of the weakly confined semiconductor nanocrystal according to any one of claims 1 to 25, characterized in that: For display.

30. The use of the weakly confined semiconductor nanocrystal according to any one of claims 1 to 25, characterized in that: Used in photovoltaic solar devices.

31. The use of the weakly confined semiconductor nanocrystal according to any one of claims 1 to 25, characterized in that: For photodetectors.

32. The use of the weakly confined semiconductor nanocrystal according to any one of claims 1 to 25, characterized in that: For lasers.

33. The use of the weakly confined semiconductor nanocrystal according to any one of claims 1 to 25, characterized in that: For quantum light sources.

34. The use of the weakly confined semiconductor nanocrystal according to any one of claims 1 to 25, characterized in that: Used in photochemical catalysis.