Amphiphilic alginic acid particles and method for producing the same
By hydrophobizing calcium alginate, a group of alginate particles is formed, which solves the problem of excessive water absorption, achieves the dual effects of stability and environmental friendliness in cosmetics and industrial materials, and reduces marine pollution risk.
Patent Information
- Application Number
- CN202180041527.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-06-11
- Filing Date
- 2021-05-07
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-05-07
AI Technical Summary
In the prior art, when calcium alginate particles have excessive water absorption, they lead to unstable use of cosmetics, easily collapse, and their performance in industrial materials is reduced, and there is a risk of environmental pollution, making it difficult to find moderate water absorption and Hydrophobic material.
By hydrophobizing calcium alginate, a group of alginate particles is formed, and a hydrophobic agent is used to chemically bond with the polyvalent metal salt of alginate to control the water absorption and oil absorption of the particles, forming a 30° or more than 150° or less Contact angle and maintain solubility and biodegradability in seawater.
It achieves stable particle shape and performance, is suitable for cosmetics, coatings, electronic materials and other fields, while reducing the risk of marine pollution and providing environmentally friendly solutions.
Smart Images

Figure GDA0003989537940000271 
Figure GDA0003989537940000281 
Figure GDA0003989537940000291
Abstract
Description
Technical Field
[0001] The present invention relates to an amphiphilic alginate particle group and a method for producing the same. Background Art
[0002] Microplastics are used as a main material in major industries. Synthetic resins are used as raw materials for microplastics, but in recent years, environmental pollution (marine pollution) and adverse effects on ecosystems caused by microplastics have become a problem, and efforts have been made to reduce the generation of microplastics.
[0003] As a raw material for microparticles, natural polymers such as cellulose are of interest. However, cellulose easily absorbs water and has a relatively high swelling property. When the swelling property is large, it is not preferred from the perspectives of dimensional stability, touch, and moldability. In addition, although the decomposability is high on land such as in soil, it has the disadvantage of low solubility and decomposability in the ocean.
[0004] Alginic acid is a polymer derived from seaweed, and is decomposed relatively quickly in the ocean due to decomposition by marine microorganisms and enzymes released from seaweed and shellfish, etc. However, it has a problem of excessive water absorption, which limits its industrial use.
[0005] As described in non-patent literature 1, by calcium cross-linking alginic acid, swelling can be suppressed, therefore, as long as it is a cosmetic such as an antiperspirant that needs hygroscopic and dehygroscopic properties, the feature can be utilized to the greatest extent, and the superiority is high. On the other hand, for example, in the case of base makeup, point makeup, etc., if the external air humidity rises, water vapor is easily absorbed, and therefore it is possible that a sticky feeling is easily caused by the weather, and discomfort is felt because of the use of customers. In addition, the water absorption of calcium alginate particles is high, and it is high performance, so it is also easy to become the cause of makeup collapse. In addition, when water absorption is too high, in the foundation of liquid system, makeup base, etc., the compatibility with oil agent is poor, and it is possible that product formula and purpose are limited.
[0006] On the other hand, calcium alginate particles are not suitable for fields such as electrical materials because they are not water-absorbent and hygroscopic. If the water absorption is extremely high, there is a risk of performance degradation, so the use of calcium alginate particles in industrial materials is limited. Considering environmental issues such as marine pollution, raw materials that can be used in all industrial materials are sought.
[0007] Prior art literature
[0008] Non-patent literature
[0009] Non-patent document 1: Takaya Sato et al., “Development of calcium alginate microparticles and their application in cosmetics,” Fibers and Industries, Vol. 52, No. 1, 1996, pp. 20-26 Summary of the invention
[0010] Problems to be solved by the invention
[0011] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide amphiphilic polymer particles which can meet the above requirements, are made from natural ingredients, have a moderate water absorption capacity, and have hydrophobicity.
[0012] Means for solving problems
[0013] The present inventors have repeatedly conducted intensive studies to solve the above-mentioned problems, and as a result, have discovered a method for hydrophobizing particles composed of cross-linked alginic acid such as calcium alginate by chemical bonding, and that the locally hydrophobized alginic acid particles have excellent water repellency and tactile properties to a certain extent, and although they are insoluble in water, they dissolve in seawater and are thereby decomposed by microorganisms, which is useful for countermeasures against marine pollution, thereby completing the present invention.
[0014] That is, the present invention provides the following amphiphilic alginic acid particles and a method for producing the same.
[0015] 1. An amphiphilic alginic acid particle group, which is an amphiphilic alginic acid particle group obtained by hydrophobizing an alginic acid polyvalent metal salt using a hydrophobizing agent, wherein:
[0016] The alginate is formed by chemically bonding a portion of the metal ions of the above-mentioned polyvalent metal salt with the above-mentioned hydrophobic agent to perform hydrophobization, and the contact angle of water droplets falling on the particle group after 30 seconds is greater than 30° and less than 150°, and the water absorption per 100 g of the particles is greater than the oil absorption per 100 g of the particles.
[0017] 2.1 The amphiphilic alginate particle group, wherein the hydrophobic agent is a salt compound.
[0018] 3.2 The amphiphilic alginate particle group, wherein the hydrophobic agent is a carboxylate, an amino acid derivative salt, a sulfonate or a sulfate ester salt.
[0019] 4.3 The amphiphilic alginate particle group, wherein the hydrophobic agent is at least one selected from carboxylates and amino acid derivative salts.
[0020] 5. The amphiphilic alginate particles according to any one of 1 to 4, wherein the metal is a metal that becomes a divalent ion.
[0021] 6.5 amphiphilic alginate particle group, wherein the above-mentioned metal is calcium.
[0022] 7. The amphiphilic alginic acid particles according to any one of 1 to 6, which are insoluble in water at 25°C but soluble in a 3% by mass sodium chloride aqueous solution.
[0023] 8. The amphiphilic alginic acid particles according to any one of 1 to 7, wherein the average particle size is 5 mm or less.
[0024] 9. The amphiphilic alginate particle group according to any one of 1 to 8, wherein the amphiphilic alginate particle group is dispersed in a 3% by mass sodium chloride aqueous solution in a manner of 0.1% by mass, and the transmittance of light of a wavelength of 560 nm of the dispersion after 72 hours, 240 hours and 720 hours is set to SD1, SD2 and SD3 (%) respectively; when the amphiphilic alginate particle group is dispersed in water in a manner of 0.1% by mass, and the transmittance of light of a wavelength of 560 nm of the dispersion after 72 hours, 240 hours and 720 hours is set to WD1, WD2 and WD3 (%) respectively, at least one of WD1 / SD1, WD2 / SD2 and WD3 / SD3 is less than 0.9.
[0025] 10. A cosmetic comprising the amphiphilic alginic acid particles according to any one of 1 to 9.
[0026] 11. A coating material comprising the amphiphilic alginate particles according to any one of 1 to 9.
[0027] 12. A resin composition comprising the amphiphilic alginic acid particles according to any one of 1 to 9.
[0028] 13. A molded article comprising the amphiphilic alginic acid particles according to any one of 1 to 9.
[0029] 14. An electronic material comprising the amphiphilic alginate particle group according to any one of 1 to 9.
[0030] 15. A sheet comprising the amphiphilic alginate particles according to any one of 1 to 9.
[0031] 16. A method for producing amphiphilic alginic acid particles, comprising: a step of hydrophobizing alginic acid particles containing a polyvalent metal salt of alginic acid using a hydrophobizing agent without completely dissolving the hydrophobizing agent.
[0032] 17. A method for producing an amphiphilic alginate particle group, comprising: a step of spray-drying a solution containing a monovalent alginate salt and an incompletely dissolved hydrophobic agent to obtain particles; and a step of hydrophobizing the particles while cross-linking them using a polyvalent metal salt.
[0033] 18. A method for producing an amphiphilic alginate particle group, comprising: a step of forming an oil-in-water emulsion containing a monovalent alginate salt and an incompletely dissolved hydrophobic agent in water droplets; and a step of performing a hydrophobic treatment while the hydrophobic agent is not completely dissolved while performing a cross-linking treatment using a polyvalent metal salt.
[0034] Effects of the Invention
[0035] The amphiphilic alginic acid particle group of the present invention also has few foreign matters such as agglomerates, can be stably and efficiently manufactured, and can control the shapes such as small diameter and flattening, and can also stably make cross-linked particles with heat resistance and resistance to (heat) chemicals, so it can be applied to various purposes. In addition, the amphiphilic alginic acid particle group of the present invention is excellent in water repellency and tactile properties to a certain extent, and is environmentally friendly particles, especially particles from natural polymers useful for marine pollution countermeasures, so it can be effectively applied to coatings, inks, molded products, cosmetics, fired hollow molded products and other environmentally required purposes according to the purpose. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is a SEM photograph (2000 times) of the particles obtained in Example 1-1.
[0037] Figure 2 This is a SEM photograph (1000 times) of the particles obtained in Example 1-2.
[0038] Figure 3 This is a SEM photograph (2000 times) of the particles obtained in Example 1-3. DETAILED DESCRIPTION
[0039] [Amphiphilic Alginate Particles]
[0040] The amphiphilic alginic acid particles of the present invention are obtained by subjecting hydrophilic alginic acid multivalent metal salt particles to a hydrophobic treatment.
[0041] Generally speaking, when the solid surface is easily wetted by water, the solid is hydrophilic, and conversely, the solid is hydrophobic when it repels water. With respect to hydrophilic alginate multivalent metal salt particles, the contact angle is less than 10°, which is called a super-hydrophilic region. With respect to the amphiphilic alginate particle group of the present invention, the contact angle after 30 seconds when water drops fall on the particle group is more than 30° and less than 150°. Here, "amphiphilicity" refers to both a hydrophilic part (or hydrophilic group) and a hydrophobic part (or hydrophobic group). Therefore, according to the strength of hydrophobization, if it is close to hydrophilicity, it is less than 90°, and if it is close to hydrophobicity, it exceeds 90°.
[0042] The above-mentioned alginic acid polyvalent metal salt is not particularly limited, and examples thereof include calcium alginate, strontium alginate, magnesium alginate, barium alginate, radium alginate, lead alginate, zinc alginate, nickel alginate, iron alginate, copper alginate, cadmium alginate, cobalt alginate, manganese alginate, etc. Among them, calcium alginate is preferred from the perspectives of environment, safety, crosslinking degree adjustment, versatility, cost, etc.
[0043] As the compound used for the above-mentioned hydrophobic treatment (hereinafter also referred to as a hydrophobic agent), carboxylic acid, carboxylate, amino acid derivative, amino acid derivative salt, organosilicon compound, organosilicon compound (silicone compounds), fluorine compound, sulfate, sulfate salt, sulfonic acid, sulfonate, phosphate, phosphate salt, lactate and lactate salt, etc. can be listed. As for the above-mentioned hydrophobic agent, from the environmental aspect, when it is designed in a manner that fully satisfies the solubility in water and salt water and the microbial decomposition in the environment, a hydrophobic agent with a molecular weight of less than 5000 is preferred, a hydrophobic agent with a molecular weight of 50 to 1000 is more preferred, a hydrophobic agent with a molecular weight of 100 to 600 is further preferred, and a hydrophobic agent with a molecular weight of 200 to 500 is most preferred. It should be noted that in the present invention, in terms of molecular weight, for polymers, it refers to the number average molecular weight (Mn), and Mn is a polystyrene conversion measurement value using gel permeation chromatography. For substances other than polymers, it is the chemical formula weight.
[0044] Among them, as the hydrophobic agent, salt compounds are preferred. As specific salt compounds, carboxylates, amino acid derivative salts, sulfonates, and sulfate ester salts are preferred. These low molecular weight substances are mostly easily decomposed by microorganisms in the environment. It is particularly preferred that the cations of these salts are metal ions.
[0045] As the above-mentioned metal ion, various metal ions such as lithium ion, potassium ion, calcium ion, sodium ion, magnesium ion, aluminum ion, zinc ion, iron ion, nickel ion, tin ion, lead ion, copper ion, cobalt ion, manganese ion, strontium ion, barium ion, cadmium ion, mercury ion, silver ion, platinum ion, gold ion can be enumerated. Wherein, from the viewpoints such as environment, biosafety, versatility, cost, etc., preferably calcium ion, sodium ion, magnesium ion, potassium ion. Particularly preferably, the above-mentioned salt compound is easy to become hydrophilic monovalent metal ion, specifically, preferably potassium ion, sodium ion, from the aspect described later, sodium ion as general metal ion is also excellent.
[0046] These hydrophobic agents are water-soluble and hydrophilic individually, but change to hydrophobicity by chemical bonding with a part of alginic acid polyvalent metal salt. The structure forms a large feature that can control solubility and biodegradability in seawater while maintaining hydrophobicity. It should be noted that the so-called chemical bonding is preferably intramolecular bonding, and more preferably ionic bonding.
[0047] In addition, the hydrophobic treatment will be described in detail later.
[0048] The carboxylic acid is preferably a carboxylic acid having 6 to 30 carbon atoms, more preferably a carboxylic acid having 8 to 25 carbon atoms, and most preferably a carboxylic acid having 10 to 20 carbon atoms. The carboxylic acid may be a monovalent carboxylic acid or a polyvalent carboxylic acid.
[0049] Examples of the monocarboxylic acid include caproic acid, heptanoic acid, caprylic acid, octanoic acid, nonanoic acid, capric acid, undecanoic acid, lauric acid, myristic acid, pentadecanoic acid, palmitic acid, palmitoleic acid, heptadecanoic acid, stearic acid, isostearic acid, oleic acid, 11-octadecenoic acid, ricinoleic acid, linoleic acid, linolenic acid, eleostearic acid, hydroxystearic acid, arachidic acid, suberic acid, arachidonic acid, eicosapentaenoic acid, behenic acid, docosahexaenoic acid, lignoceric acid, nervonic acid, hexacosanoic acid, montanic acid, melissic acid, coconut oil fatty acid, and palm oil fatty acid.
[0050] Examples of the polycarboxylic acid include suberic acid, azelaic acid, sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, nonadecanedioic acid, eicosanedioic acid, etc. In addition, these may be isomers having a branched structure, and trivalent or higher polycarboxylic acids may also be used.
[0051] The carboxylate is preferably a carboxylate having 6 to 30 carbon atoms, more preferably a carboxylate having 8 to 25 carbon atoms, and still more preferably a carboxylate having 10 to 20 carbon atoms. The carboxylic acid may be a monovalent carboxylic acid or a polyvalent carboxylic acid.
[0052] Examples of the monovalent carboxylic acid salt include octanoic acid salts such as potassium octanoate, sodium octanoate, and zinc octanoate; octanoic acid salts such as potassium octanoate, sodium octanoate, and zinc octanoate; salt); nonanoic acid salts such as potassium nonanoate and sodium nonanoate; decanoic acid salts such as potassium decanoate and sodium decanoate; undecanoic acid salts such as potassium undecanoate and sodium undecanoate; lauric acid salts such as potassium laurate, sodium laurate, calcium laurate, barium laurate and zinc laurate; myristate salts such as potassium myristate, sodium myristate, zinc myristate and magnesium myristate; pentadecanoic acid salts such as potassium pentadecanoate and sodium pentadecanoate; palmitate salts such as potassium palmitate, sodium palmitate and calcium palmitate; heptadecanoic acid salts such as potassium heptadecanoate and sodium heptadecanoate; stearic acid salts such as lithium stearate, sodium stearate, magnesium stearate, calcium stearate, barium stearate, zinc stearate and aluminum stearate isostearate; isostearate such as potassium isostearate and sodium isostearate; oleate such as potassium oleate and sodium oleate; ricinoleate such as calcium ricinoleate, barium ricinoleate and zinc ricinoleate; linoleate such as potassium linoleate, sodium linoleate and calcium linoleate; linoleate such as potassium linoleate and sodium linoleate; arachidonic acid such as potassium arachidonic acid and sodium arachidonic acid; behenate such as potassium behenate, sodium behenate and calcium behenate; docosahexaenoic acid such as sodium docosahexaenoic acid; coconut oil fatty acid salts such as potassium coconut oil fatty acid and sodium coconut oil fatty acid; palm oil fatty acid salts such as calcium palm oil fatty acid; isopropyl titanium triisostearate, etc. Among them, stearate and myristate are preferred.
[0053] Examples of the polycarboxylate salt include suberates such as disodium suberate and dipotassium suberate; azelates such as disodium azelate and dipotassium azelate; sebacates such as disodium sebacate and dipotassium sebacate; undecanedioates such as disodium undecanedioate and dipotassium undecanedioate; dodecanedioates such as disodium dodecanedioate and dipotassium dodecanedioate; tridecanedioates such as disodium tridecanedioate and dipotassium tridecanedioate; and tetradecanedioates such as disodium tetradecanedioate and dipotassium tetradecanedioate. Tetradecanoic acid salts; pentadecanoic acid salts such as disodium pentadecanedioate and dipotassium pentadecanedioate; hexadecanedioate salts such as disodium hexadecanedioate and dipotassium hexadecanedioate; heptadecanedioate salts such as disodium heptadecanedioate and dipotassium heptadecanedioate; octadecanedioate salts such as disodium octadecanedioate and dipotassium octadecanedioate; nonadecanedioate salts such as disodium nonadecanedioate and dipotassium nonadecanedioate; dicarboxylates such as eicosanedioate salts such as disodium eicosanedioate and dipotassium eicosanedioate. In addition, these branched isomers may be used, and salts of polycarboxylic acids with a valence of 3 or more may also be used. In particular, if a polycarboxylic acid having a carbon number of 6 to 30 as described above is used for hydrophobic treatment, elasticity and softness can be imparted. It is preferably a polycarboxylic acid salt, and more preferably a structure of a diacid disalt.
[0054] As the amino acid derivative, an amino acid derivative having 6 to 30 carbon atoms is preferred, an amino acid derivative having 8 to 25 carbon atoms is more preferred, and an amino acid derivative having 10 to 20 carbon atoms is further preferred. Examples of the amino acid derivative include sarcosine derivatives such as lauroyl sarcosine, myristoyl sarcosine, palmitoyl sarcosine, and coconut oil fatty acid sarcosine; glutamate derivatives such as lauroyl glutamic acid, myristoyl glutamic acid, palmitoyl glutamic acid, stearoyl glutamic acid, coconut oil fatty acid acyl glutamic acid, coconut oil acyl glutamic acid, acyl glutamic acid, and dilauroyl glutamic acid; glycine derivatives such as lauroyl glycine, myristoyl glycine, palmitoyl glycine, palmitoyl methyl glycine, coconut oil fatty acid acyl glycine, and coconut oil acyl glycine; and lauryl methyl alanine, myristyl methyl alanine, coconut oil fatty acid methyl alanine, and coconut oil fatty acid acyl glutamic acid. Alanine derivatives such as alanine; lysine derivatives such as lauroyl lysine, myristoyl lysine, palmitoyl lysine, stearoyl lysine, oleyl lysine, and acylated lysine; aspartic acid derivatives such as lauroyl aspartic acid, myristoyl aspartic acid, palmitoyl aspartic acid, and stearoyl aspartic acid; taurine derivatives such as lauroyl taurine, lauroyl methyl taurine, myristoyl taurine, myristoyl methyl taurine, palmitoyl taurine, palmitoyl methyl taurine, stearoyl taurine, and stearoyl methyl taurine; amino acid derivatives such as proline derivatives such as lauroyl proline, myristoyl proline, and palmitoyl proline.
[0055] As the salt of the amino acid derivative, the salt of the amino acid derivative having 6 to 30 carbon atoms is preferred, the salt of the amino acid derivative having 8 to 25 carbon atoms is more preferred, and the salt of the amino acid derivative having 10 to 20 carbon atoms is further preferred. As the salt of the amino acid derivative, there can be mentioned sarcosinates such as potassium lauroyl sarcosinate, sodium lauroyl sarcosinate, potassium myristoyl sarcosinate, sodium myristoyl sarcosinate, potassium palmitoyl sarcosinate, sodium palmitoyl sarcosinate, potassium coconut oil fatty acid sarcosinate, sodium coconut oil fatty acid sarcosinate; potassium lauroyl glutamate, sodium lauroyl glutamate, potassium myristoyl glutamate, sodium myristoyl glutamate, sodium palmitoyl glutamate, magnesium palmitoyl glutamate, potassium stearoyl glutamate, sodium stearoyl glutamate, coconut oil fat; Fatty acid acyl glutamate potassium, coconut oil fatty acid acyl glutamate sodium, coconut oil acyl glutamate potassium, coconut oil acyl glutamate sodium, acyl glutamate potassium, acyl glutamate sodium, dilauroyl glutamate lysine sodium, sodium polyglutamate and other glutamates; lauroyl glycinate potassium, lauroyl glycinate sodium, myristoyl glycinate potassium, myristoyl glycinate sodium, palmitoyl glycinate sodium, palmitoyl methyl glycinate, coconut oil fatty acid acyl glycinate potassium, coconut oil fatty acid acyl glycinate sodium, coconut oil acyl glycinate potassium, coconut oil acyl glycinate Glycinates such as sodium lauroyl methylalanine; Alanine salts such as potassium lauroyl methylalanine, sodium lauroyl methylalanine, sodium myristoyl methylalanine, sodium cocoyl alanine, and sodium coconut oil fatty acid methylalanine; Aspartates such as potassium lauroyl aspartate, sodium lauroyl aspartate, potassium myristoyl aspartate, sodium myristoyl aspartate, potassium palmitoyl aspartate, sodium palmitoyl aspartate, potassium stearoyl aspartate, and sodium stearoyl aspartate; Sodium lauroyl taurate, calcium lauroyl taurate, etc. Lauroyl taurate; taurates such as sodium lauroyl taurate, calcium lauroyl taurate, sodium lauroyl methyl taurate, potassium myristoyl taurate, sodium myristoyl taurate, sodium myristoyl methyl taurate, potassium palmitoyl taurate, sodium palmitoyl taurate, potassium palmitoyl methyl taurate, sodium palmitoyl methyl taurate, potassium stearoyl taurate, sodium stearoyl taurate, sodium stearoyl methyl taurate; proline salts such as sodium lauroyl proline, sodium myristoyl proline, sodium palmitoyl proline, etc.
[0056] Examples of the organic silicon compound include alkylated silanes having at least one alkyl group having 6 to 30 carbon atoms, alkylated silazanes having at least one alkyl group having 6 to 30 carbon atoms, trialkoxysilanes having at least one alkoxy group having 6 to 30 carbon atoms, octyltrialkoxysilane, triethoxyoctanoylsilane, and 3-methacryloxypropyltrimethoxysilane.
[0057] Examples of the silicone compound include methyl hydrogen polysiloxane, methyl polysiloxane (methicone), dimethyl polysiloxane (dimethicone), triethoxysilylethyl polydimethylsiloxyethyl dimethyl polysiloxane, methylphenyl polysiloxane, triethoxysilylethyl polydimethylsiloxyethyl hexyl dimethyl polysiloxane, cyclic silicone, crosslinked silicone, acrylic-silicone graft polymer, silicone resin partially crosslinked organopolysiloxane polymer, tetramethyltetrahydrocyclotetrasiloxane, trimethylsiloxysilicic acid, amino-modified silicone, carboxylic acid-modified silicone, fluorinated silicone, silicone rubber, acrylic silicone, silicone resin, triethoxysilylethyl polydimethylsiloxyethyl dimethyl polysiloxane, triethoxysilylethyl polydimethylsiloxyethyl hexyl dimethyl polysiloxane, and fluorinated silicone.
[0058] Examples of the fluorine compound include perfluoroalkyl phosphates, perfluoroalkyl silanes, perfluoroalkyl alkoxysilanes, perfluoroalkyl-containing esters, perfluoroalkyl phosphate salts, perfluoropolyethers, fluorosilicones, fluorinated silicone resins, trimethoxy (3,3,3-trifluoropropyl) silane, and tridecafluorooctyl triethoxysilane.
[0059] Examples of the sulfates and sulfate salts include alkyl sulfates, alkyl sulfate salts, polyoxyethylene aryl ether sulfates, polyoxyethylene aryl ether sulfate salts, polyoxyethylene alkyl ether sulfates, polyoxyethylene alkyl ether sulfate salts, polyoxyalkylene alkyl ether sulfate salts, polyoxyalkylene alkenyl ether sulfates, polyoxyethylene castor oil ether sulfates, and polyoxyethylene castor oil ether sulfate salts.
[0060] As the alkyl sulfate ester and alkyl sulfate ester salt, an alkyl sulfate ester and an alkyl sulfate ester salt having an alkyl group with 6 to 30 carbon atoms are preferred, an alkyl sulfate ester and an alkyl sulfate ester salt having an alkyl group with 8 to 25 carbon atoms are more preferred, and an alkyl sulfate ester and an alkyl sulfate ester salt having an alkyl group with 10 to 20 carbon atoms are further preferred. Specific examples of the alkyl sulfate ester and the alkyl sulfate ester salt include alkyl sulfates and salts thereof such as lauryl sulfate, potassium lauryl sulfate, sodium lauryl sulfate, myristyl sulfate, potassium myristyl sulfate, sodium myristyl sulfate, cetyl sulfate, sodium cetyl sulfate, stearyl sulfate, sodium stearyl sulfate, oleyl sulfate, sodium oleyl sulfate, and alkylbenzene sulfates and salts thereof such as dodecylbenzene sulfate, sodium dodecylbenzene sulfate, and potassium dodecylbenzene sulfate.
[0061] As the polyoxyethylene aryl ether sulfate and polyoxyethylene aryl ether sulfate salt, those having an HLB value of 11 or less and those having an HLB value of 6 or less are preferred. Examples thereof include polyoxyethylene polycyclic phenyl ether sulfate salts such as polyoxyethylene polycyclic phenyl ether sulfate and sodium polyoxyethylene polycyclic phenyl ether sulfate; polyoxyethylene aryl ether sulfate and sodium polyoxyethylene aryl ether sulfate; and the like.
[0062] As the polyoxyethylene alkyl ether sulfates and polyoxyethylene alkyl ether sulfate salts, polyoxyethylene alkyl ether sulfates and polyoxyethylene alkyl ether sulfate salts having an HLB value of 6 or less are preferred, and examples thereof include polyoxyethylene alkyl ether sulfates, polyoxyethylene lauryl ether sodium sulfate, polyoxyethylene myristyl ether sodium sulfate, polyoxyethylene cetyl ether sodium sulfate, polyoxyethylene stearyl ether sodium sulfate, and polyoxyethylene oleyl ether sodium sulfate.
[0063] As the polyoxyalkylene alkyl ether sulfate salt, a polyoxyalkylene alkyl ether sulfate salt having an HLB value of 11 or less is preferred, and a polyoxyalkylene alkyl ether sulfate salt having an HLB value of 6 or less is more preferred. For example, sodium sulfate salts of polyoxyethylene-polyoxypropylene block copolymers, sodium sulfate salts of polyoxyethylene-polyoxybutylene block copolymers, sodium sulfate salts of alkyl ethers of polyoxyethylene-polyoxypropylene block copolymers, etc. are listed. As the above-mentioned polyoxyalkylene alkenyl ether sulfate salt, a polyoxyalkylene alkenyl ether sulfate salt having an HLB value of 11 or less is preferred, and a polyoxyalkylene alkenyl ether sulfate salt having an HLB value of 6 or less is more preferred. For example, sodium sulfate salts of alkenyl ethers of polyoxyethylene-polyoxyalkylene block copolymers, etc. are listed. As the polyoxyethylene castor oil ether sulfate and polyoxyethylene castor oil ether sulfate salt, polyoxyethylene castor oil ether sulfate and polyoxyethylene castor oil ether sulfate salt having an HLB value of 11 or less are preferred, and polyoxyethylene castor oil ether sulfate and polyoxyethylene castor oil ether sulfate salt having an HLB value of 6 or less are more preferred. Examples thereof include polyoxyethylene castor oil ether sulfate and polyoxyethylene castor oil ether sulfate sodium salt.
[0064] The sulfonic acid and sulfonate are preferably those having 6 to 30 carbon atoms, more preferably those having 8 to 25 carbon atoms, and still more preferably those having 10 to 20 carbon atoms. The sulfonic acid and sulfonate may be monovalent or polyvalent and may be an acid. Specific examples of the sulfonic acid and sulfonate include alkyl sulfonic acids and alkyl sulfonates such as lauryl sulfonic acid, sodium lauryl sulfonate, myristic acid, sodium myristic acid, cetyl sulfonic acid, sodium cetyl sulfonate, stearyl sulfonic acid, sodium stearyl sulfonate, oleyl sulfonic acid, sodium oleyl sulfonate; dodecylbenzenesulfonic acids and dodecylbenzenesulfonates such as dodecylbenzenesulfonic acid, sodium dodecylbenzenesulfonate, and calcium dodecylbenzenesulfonate; alkylene disulfonic acids and alkylene disulfonates such as alkylene disulfonic acid and sodium alkylene disulfonate; dialkyl succinate sulfonic acids and dialkyl succinate sulfonates such as dialkyl succinate sulfonic acid and sodium dialkyl succinate sulfonate; monoalkyl succinate sulfonic acids, monoalkyl succinate sulfonates; naphthalenesulfonic acid formaldehyde condensates and naphthalenesulfonic acid formaldehyde condensate salts such as naphthalenesulfonic acid formaldehyde condensate and naphthalenesulfonic acid formaldehyde condensate sodium salt; olefin sulfonates such as sodium olefin sulfonate; isethionate acids such as lauroyl isethionate, myristyl isethionate, palmitoyl isethionate and stearoyl isethionate; isethionate salts such as potassium lauroyl isethionate, sodium lauroyl isethionate, sodium myristyl isethionate, sodium palmitoyl isethionate and sodium stearoyl isethionate; sulfosuccinic acids and sulfosuccinate salts such as sodium dihexyl sulfosuccinate, sodium dioctyl sulfosuccinate, sodium didecyl sulfosuccinate and sodium diisobutyl sulfosuccinate, etc.
[0065] Examples of the phosphate ester and phosphate ester salt include polyoxyalkylene alkyl ether phosphate ester, alkyl phosphate ester, alkyl phosphate ester salt, etc. The polyoxyalkylene alkyl ether phosphate ester preferably has an HLB value of 6 or less, and examples thereof include polyoxyethylene (2) stearyl ether phosphate, etc.
[0066] As the above-mentioned alkyl phosphates and alkyl phosphate salts, alkyl phosphates and alkyl phosphate salts having an alkyl group with 6 to 30 carbon atoms are preferred, alkyl phosphates and alkyl phosphate salts having an alkyl group with 8 to 25 carbon atoms are more preferred, and alkyl phosphates and alkyl phosphate salts having an alkyl group with 10 to 20 carbon atoms are further preferred. Specific examples of the above-mentioned alkyl phosphates and alkyl phosphate salts include octyl phosphate and octyl phosphate salts such as octyl phosphate and potassium octyl phosphate; nonyl phosphate and nonyl phosphate salts such as nonyl phosphate and potassium nonyl phosphate; decyl phosphate and decyl phosphate salts such as decyl phosphate and potassium decyl phosphate; undecyl phosphate and undecyl phosphate salts such as undecyl phosphate and potassium undecyl phosphate; lauryl phosphate and lauryl phosphate salts such as lauryl phosphate and potassium lauryl phosphate; myristyl phosphate and myristyl phosphate salts such as myristyl phosphate and potassium myristyl phosphate; cetyl phosphate and cetyl phosphate salts such as cetyl phosphate, potassium cetyl phosphate, sodium cetyl phosphate, calcium cetyl phosphate, zinc cetyl phosphate; stearyl phosphate and stearyl phosphate salts such as stearyl phosphate and potassium stearyl phosphate, etc.
[0067] As the lactic acid ester and lactic acid ester salt, lactic acid ester and lactic acid ester salt having 6 to 30 carbon atoms are preferred, lactic acid ester and lactic acid ester salt having 8 to 25 carbon atoms are more preferred, and lactic acid ester and lactic acid ester salt having 10 to 20 carbon atoms are further preferred. Specific examples of the lactic acid ester and lactic acid ester salt include lauryl lactate, myristyl lactate, cetyl lactate, oleyl lactate, octyldodecyl lactate, sodium stearoyl lactylate, calcium stearoyl lactylate, sodium isostearyl lactylate, sodium lauroyl lactylate, and the like.
[0068] In addition to the above compounds, oils used as cosmetic additives, acrylic compounds, acrylic resins, titanium coupling agents, inorganic compounds, metal oxides, solid lubricants, and known surfactants can also be used as hydrophobic agents.
[0069] Examples of the oil include vaseline, liquid paraffin, squalane, paraffin, linseed oil, cottonseed oil, coconut oil, castor oil, egg yolk oil, lanolin fatty acid, propylene glycol dicaprate, tricaprylin, cetyl 2-ethylhexanoate, isocetyl stearate, stearyl alcohol, cetyl alcohol, oleyl alcohol, beef tallow, beeswax, spermaceti, wood wax, lanolin, carnauba wax, and candelilla wax.
[0070] Examples of the acrylic compound include alkyl (meth)acrylates, etc. Examples of the acrylic resin include copolymers of (meth)acrylic acid and styrene compounds and salts thereof, copolymers of (meth)acrylic acid and (meth)acrylic acid ester compounds and salts thereof, copolymers of (meth)acrylic acid and vinyl ester compounds and salts thereof, copolymers of (meth)acrylic acid and olefin compounds and salts thereof, copolymers of (meth)acrylic acid and conjugated diene compounds and salts thereof, etc.
[0071] Examples of the titanium coupling agent include alkyl titanates, pyrophosphate-type titanates, phosphorous acid-type titanates, and amino acid-type titanates.
[0072] Examples of the inorganic compound include aluminum oxide, and examples of the metal oxide include titanium oxide.
[0073] Examples of the solid lubricant include polyolefin waxes (e.g., polyethylene waxes), paraffin waxes (e.g., synthetic paraffin waxes, natural paraffin waxes), fluororesin waxes (e.g., polytetrafluoroethylene waxes), fatty acid amide compounds (e.g., stearamide, palmitamide, etc.), metal sulfides (e.g., molybdenum disulfide, tungsten disulfide, etc.), graphite, graphite fluoride, boron nitride, polyalkylene glycol, alkali metal sulfates, and the like.
[0074] For the amphiphilic alginic acid particle group of the present invention, its average particle size is preferably 5 mm or less, preferably 1 mm or less, 500 μm or less, 100 μm or less, 60 μm or less, 30 μm or less, 15 μm or less, 10 μm or less. In addition, its lower limit is preferably 0.1 μm, more preferably 0.5 μm, and further preferably 1.0 μm. It should be noted that in the present invention, the average particle size is a volume average particle size (MV) based on a laser diffraction-scattering method.
[0075] The shape of the amphiphilic alginic acid particle group of the present invention is a spherical, roughly spherical, flat, concave, etc., a physically and chemically controlled product of shape, a physically crushed product, etc., and is not particularly limited, but from the viewpoint of controlling the feel, slippage, and particle size distribution, a spherical, roughly spherical, flat, concave, etc., a physically and chemically controlled product of shape is preferred. Furthermore, irregular particles formed by curves that do not have acute angles such as roughly spherical, flat, concave are preferred because of their good optical properties.
[0076] The water absorption of the amphiphilic alginic acid particles per 100 g of particles (A w , mL / 100g) is the oil absorption per 100g of particles (A o , mL / 100g) or more ((A w / A o )≥1). By satisfying this relationship, the hydrophobic effect is exerted during use, and the particles are kept insoluble in water, gradually dissolved in seawater (salt water), and easily decomposed by microorganisms. w and A o More preferably, A w / A o >1, preferably satisfying A w / A o≥1.05, preferably satisfying A w / A o ≥1.10, preferably A w / A o ≥1.15. In view of the practical hydrophobic effect in industry and environmental aspects such as dissolution in seawater and biodegradability, the particle group preferably satisfies A w / A o ≤20, preferably satisfying A w / A o ≤10, preferably satisfying A w / A o ≤5.
[0077] The water absorption of the amphiphilic alginic acid particle group of the present invention is preferably below 200mL / 100g, more preferably below 160mL / 100g, further preferably below 150mL / 100g, most preferably below 130mL / 100g.If water absorption is below 200mL / 100g, then the dimensional stability produced by the cross-linking effect and the initial water repellent effect produced by the hydrophobic agent as a feature of the present invention can be used without damage in the same manner as the purposes of the existing general polymer particles such as acrylic acid, nylon.It is explained that, with regard to the lower limit of water absorption, from being easy to obtain the above-mentioned effect, it is preferably 30mL / 100g, more preferably more than 60mL / 100g, more preferably more than 80mL / 100g.
[0078] On the other hand, for the amphiphilic alginic acid particle group of the present invention, its oil absorption is preferably more than 10mL / 100g, more preferably more than 20mL / 100g, more preferably more than 30mL / 100g.When oil absorption is more than 10mL / 100g, in the case of cosmetic use, due to the effect of the hydrophobic agent of the present invention, the affinity with oil agent improves, so that dispersibility improves, and in addition, the stability of emulsion and cream improves.From being easy to obtain the above-mentioned effect, the upper limit of oil absorption is preferably less than 150mL / 100g, more preferably less than 125mL / 100g, more preferably less than 100mL / 100g, most preferably less than 80mL / 100g.
[0079] The water absorption and oil absorption can be adjusted by adjusting the type and adhesion amount of the hydrophobic treatment agent described later. It should be noted that in the present invention, the oil absorption is a value measured according to the boiled linseed oil method described in JIS K 5101. The water absorption is a value obtained by the following method. Add 1g of each particle group to a 500mL beaker, then add 200mL of ion exchange water, stir for 30 minutes, then transfer to a 500mL centrifuge tube, and centrifuge using a centrifuge. After centrifugation, discard the supernatant, take out the sample from the centrifuge tube, and measure the weight (W w ), and then dried in a dryer at 105°C until it becomes constant, and the dryness (D w ) weight, and calculate the water absorption according to the following formula.
[0080] Water absorption (mL / 100g) = {(W w -D w ) / D w}×100
[0081] As for the amphiphilic alginic acid particle group of the present invention, the contact angle when water drops on the particle group is 30° or more and 150° or less. If the contact angle is in the above range, the effect of appropriate hydrophobization, solubility in the environment, and decomposability are fully exerted. Considering the above effect is easy to obtain, the lower limit of the contact angle is preferably 40° or more, more preferably 50° or more, and more preferably 60° or more. The upper limit of the contact angle is preferably 140° or less, more preferably 135° or less, and more preferably 125° or less. If it exceeds 150°, the hydrophobic effect is too large, and appropriate water absorption cannot be obtained, which may cause harm to biodegradability in the ocean. It is explained that, considering the practical hydrophobic effect in the industry and the environmental aspects such as dissolution and biodegradability in seawater, the contact angle of the particle group is preferably 40° to 140°, more preferably 50° to 135°, more preferably 60° to 125°, and most preferably 70° to 120°.
[0082] In addition, with respect to the amphiphilic alginic acid particle group of the present invention, the amphiphilic alginic acid particle group is dispersed in a 3% by mass sodium chloride aqueous solution in a manner of becoming 0.1% by mass, and the transmittance of the light of the wavelength 560nm of the dispersion liquid after 72 hours, 240 hours and 720 hours is set to SD1 (%), SD2 (%) and SD3 (%) respectively, and the amphiphilic alginic acid particle group is dispersed in water in a manner of becoming 0.1% by mass, and the transmittance of the light of the wavelength 560nm after 72 hours, 240 hours and 720 hours is set to WD1 (%), WD2 (%) and WD3 (%) respectively, at least one of WD1 / SD1, WD2 / SD2 and WD3 / SD3 is preferably 0.9 or less, more preferably 0.8 or less, and further preferably 0.5 or less. If it is 0.9 or less, it is possible to confirm the phenomenon of shape change of the alginic acid particles and transparentization with dissolution. In addition, the lower limits of WD1 / SD1, WD2 / SD2 and WD3 / SD3 are not particularly limited, but are usually about 0.1.
[0083] When the dissolution phenomenon cannot be confirmed in about 720 hours, for example, in the ocean, there is concern about environmental pollution (marine pollution), adsorption of chemical substances, and adverse effects on the ecosystem, so it is sometimes not preferred to maintain the particle shape for a long time exceeding these. Therefore, from the viewpoint of considering environmental impact, it is preferred to satisfy WD3 / SD3≤0.9, more preferably satisfy WD2 / SD2≤0.9, and further preferably satisfy WD1 / SD1≤0.9.
[0084] [Method for producing amphiphilic alginic acid particles]
[0085] As a method for producing the amphiphilic alginic acid particles of the present invention, the following method can be mentioned.
[0086] (1) A method (method 1) comprising: subjecting alginic acid particles containing a polyvalent metal salt of alginic acid to a hydrophobic treatment using a hydrophobic agent without completely dissolving the hydrophobic agent.
[0087] (2) A method (Method 2) comprising: a step of spray-drying a solution containing a monovalent salt of alginate and an incompletely dissolved hydrophobic agent to obtain particles; and a step of simultaneously cross-linking the particles with a polyvalent metal salt and performing a hydrophobic treatment.
[0088] (3) A method (Method 3) comprising: a step of forming a water-in-oil (W / O) emulsion containing a monovalent salt of alginate and an incompletely dissolved hydrophobic agent in water droplets; and a step of performing a hydrophobic treatment while the hydrophobic agent is not completely dissolved while performing a cross-linking treatment using a polyvalent metal salt.
[0089] Method 1 includes: using a hydrophobic agent to hydrophobize a group of alginic acid particles containing a polyvalent metal salt of alginic acid without completely dissolving the hydrophobic agent. The group of alginic acid particles can be manufactured by a known method. For example, as described in Japanese Patent Laid-Open No. 5-222208, a solution in which a monovalent salt of alginic acid is dissolved can be spray-dried and particle-formed, and then cross-linked using a polyvalent metal salt to manufacture the solution. The monovalent salt of alginic acid and the polyvalent metal salt will be described later.
[0090] In addition, the alginate particle group can also be formed by containing a W / O emulsion of alginate monovalent salt in water, and cross-linked using a polyvalent metal salt to manufacture. As the formation method of the W / O emulsion, for example, first, a solution A in which alginate monovalent salt is dissolved in a mixed solvent of water or water and a hydrophilic organic solvent is prepared. At this time, heating can be performed as required. Then, solution A is mixed with a hydrophobic organic solvent and emulsified using a stirring device, a homogenizer, etc. When mixing, solution A can be added to the hydrophobic organic solvent, or the hydrophobic organic solvent can be added to solution A.
[0091] At this time, a solution B prepared by dissolving a surfactant or a polymer stabilizer in a hydrophobic organic solvent in order to control the particle size of water droplets in the W / O emulsion may be used instead of the hydrophobic organic solvent. In this case, solution A and solution B are mixed and emulsified using a stirring device, a homogenizer, etc. During the mixing, solution A may be added to solution B, or solution B may be added to solution A.
[0092] As another example of the method for forming a W / O emulsion, monovalent alginic acid salt, water, a surfactant, a hydrophobic organic solvent, and other necessary components may be placed in a container and emulsified using a stirring device, a homogenizer, or the like.
[0093] The crosslinking treatment can be carried out by adding a solution containing a polyvalent metal salt to the W / O emulsion and stirring. Alternatively, the crosslinking treatment can be carried out by adding a W / O emulsion to a solution containing a polyvalent metal salt and stirring. Regarding the solution containing a polyvalent metal salt, the same solution as that described in the description of method 2 can be used.
[0094] The crosslinking treatment can be carried out while heating as needed. Heating can be carried out when the solution containing the polyvalent metal salt is added to the dispersion, when stirring after the addition, or in both cases. The heating temperature is preferably 10 to 100° C., more preferably 15 to 80° C. The treatment time is preferably 0.5 to 24 hours, more preferably 1 to 12 hours.
[0095] After the cross-linking treatment, the particles are washed and dried as needed to obtain alginate particles. Washing can be carried out by a common method, for example, removing the solvent after the cross-linking treatment, adding water and centrifuging. Drying can be carried out by a common method, for example, spray drying, vacuum drying, freeze drying and the like can be used.
[0096] As the alginic acid particles, commercially available products may be used, and examples thereof include FLAVICA FIINE (registered trademark) manufactured by Nisshinbo Chemika Co., Ltd. and calcium alginate CA series manufactured by Chemika Co., Ltd.
[0097] As a method for hydrophobizing alginic acid particle groups, the following method can be cited: a hydrophobic agent is added to a solvent, and the hydrophobic agent is adjusted in a manner that the solvent is not completely dissolved in the solvent, and the alginic acid particle group is added thereto to disperse it, so that the hydrophobic agent is attached to the surface of the above-mentioned particles or both the surface and the inside. With regard to the state in which the hydrophobic agent is not completely dissolved in the solvent, it can be adjusted by appropriately selecting a solvent or heating or cooling the solvent after the hydrophobic agent is added to the solvent. At this time, if it is further heated and concentrated as needed, it can be efficiently attached. In the case of heating, it is necessary to pay attention to the solubility of the hydrophobic agent, and the temperature is preferably 10 to 100 ° C, and more preferably 30 to 80 ° C. Concentration can be carried out, for example, by heating the reaction system and removing the evaporated solvent. The hydrophobic treatment time is preferably 0.5 to 24 hours, and more preferably 1 to 12 hours.
[0098] Here, the so-called "state in which the hydrophobic agent is not completely dissolved" refers to a state in which the hydrophobic agent is dissolved in the solvent and the dispersed part. That is, it is a state in which at least the emulsified part and the dissolved part are present. In addition, in this state, the appearance is translucent or light white. If it is completely in an emulsified state, it exists and adheres stably as microparticles, so the water absorption of the obtained alginate particle group is high, and it is possible to fail to maintain the contact angle as an index of hydrophobization. On the other hand, when it is completely in a dissolved state, although the contact angle of hydrophobization is fully maintained, there is a tendency for the water absorption to decrease, and sometimes the amphiphilicity is no longer maintained.
[0099] The state in which the hydrophobic agent is not completely dissolved can be determined, for example, by measuring the total light transmittance by pouring a solution into a cell having a cell thickness of 1 cm using a haze meter described in JIS K 7136 and 7361. In this case, the state in which the hydrophobic agent is not completely dissolved is preferably a state in which the total light transmittance is 35 to 85%, more preferably 40 to 80%, and even more preferably 45 to 75%.
[0100] The above-mentioned solvent can be appropriately selected: a solvent capable of dispersing the alginic acid particle group and adding a hydrophobic agent to make it a state in which the hydrophobic agent is not completely dissolved in the solvent. In addition, after adding the hydrophobic agent, the solubility is adjusted by heating or cooling. When adjusting to make it a state in which the hydrophobic agent is not completely dissolved in the solvent, a solvent capable of dispersing the hydrophobic agent can be appropriately selected. Examples of such solvents include water; alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutanol, tert-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, isopentanol, tert-pentanol, 1-hexanol, 2-methyl-1-pentanol, 4-methyl-2-pentanol, 2-ethylbutanol, 1-heptanol, 2-heptanol, 3-heptanol, 2-octanol, 2-ethyl-1-hexanol, benzyl alcohol, and cyclohexanol; ether alcohols such as methyl cellosolve, ethyl cellosolve, isopropyl cellosolve, butyl cellosolve, and diethylene glycol monobutyl ether; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; esters such as ethyl acetate, butyl acetate, ethyl propionate, and cellosolve acetate; pentane, 2-methylbutane, n-hexane, cyclohexane, Aliphatic or aromatic hydrocarbons such as hexane, 2-methylpentane, 2,2-dimethylbutane, 2,3-dimethylbutane, heptane, n-octane, isooctane, 2,2,3-trimethylpentane, decane, nonane, cyclopentane, methylcyclopentane, methylcyclohexane, ethylcyclohexane, p-menthane, bicyclohexyl, benzene, toluene, xylene, ethylbenzene, etc.; halogenated hydrocarbons such as carbon tetrachloride, trichloroethylene, chlorobenzene, tetrabromoethane, etc.; ethers such as diethyl ether, dimethyl ether, trioxane, tetrahydrofuran, etc.; acetals such as methylal, diethyl acetal, etc.; carboxylic acids such as formic acid, acetic acid, propionic acid, etc.; organic compounds containing sulfur and nitrogen such as nitropropylene, nitrobenzene, dimethylamine, monoethanolamine, pyridine, dimethylformamide, dimethyl sulfoxide, N-methyl-2-pyrrolidone, acetonitrile, etc.; ionic liquids, etc. These solvents may be used alone or in combination of two or more.
[0101] As the above-mentioned hydrophobic agent, the above-mentioned hydrophobic agent can be used. When the above-mentioned salt compound is used as the hydrophobic agent in particular, ion exchange occurs with at least a portion of the multivalent metal ions cross-linked by ions, accompanied by chemical bonding with the hydrophobic agent. Therefore, monodisperse cross-linked particles with enhanced hydrophobicity are obtained after treatment, so it is preferred. And then, by carrying out hydrophobization accompanied by chemical bonding, the strength of hydrophilicity can be quantitatively controlled. As the above-mentioned hydrophobic agent, carboxylates, amino acid derivative salts, sulfonates, sulfates are preferred, and carboxylates and amino acid derivative salts from organisms are more preferably. In this way, particles considering the environment can be obtained.
[0102] The hydrophobizing treatment is preferably carried out in a manner such that the mass ratio of the alginate particle group and the hydrophobizing agent in the solvent is alginate particle group: hydrophobizing agent = 99.9:0.1 to 70:30, more preferably 99.5:0.5 to 80:20, further preferably 99:1 to 85:15, and further preferably 98:2 to 90:10.
[0103] After the hydrophobic treatment, the washing and drying of particles are carried out as required, thus the amphiphilic alginic acid particle group can be obtained. The cleaning can be carried out by the usual method, for example, the solvent can be removed after the hydrophobic treatment, and the methods such as centrifugation can be added to water. Drying can be carried out by the usual method, for example, by methods such as spray drying, vacuum drying, freeze drying.
[0104] Method 2 is a method comprising the steps of spray-drying a solution containing a monovalent alginic acid salt and an incompletely dissolved hydrophobic agent to obtain particles, and performing a hydrophobic treatment on the particles while crosslinking them using a polyvalent metal salt.
[0105] The above-mentioned monovalent salt of alginic acid can be an inorganic salt or an organic salt, for example, sodium alginate, potassium alginate, ammonium alginate, etc. can be cited. In addition, the viscosity of 1% by mass or 10% by mass aqueous solution of the above-mentioned monovalent salt of alginic acid is preferably 0.01 to 2000mPa·s, more preferably 0.1 to 1000mPa·s, and most preferably 1.0 to 500mPa·s. Considering productivity, it is more preferred that the viscosity of its 10% by mass aqueous solution meets the above range. It should be noted that the above viscosity is a measured value at 20°C using a B-type viscometer BL type.
[0106] As the solvent used in the above-mentioned solution containing monovalent alginic acid salt and hydrophobic agent, preferably water or a mixed solvent of water and a hydrophilic organic solvent. As water, tap water, ion exchange water, distilled water, etc. can be enumerated. As the hydrophilic organic solvent, methanol, ethanol, 1-propanol, 2-propanol, ethylene glycol, propylene glycol, butylene glycol, dipropylene glycol, methyl cellosolve, ethyl cellosolve, propyl cellosolve, diethylene glycol monobutyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, methyl carbitol, ethyl carbitol, butyl carbitol, ethyl carbitol acetate, formic acid, acetic acid, propionic acid, acetone, tetrahydrofuran, dimethylformamide, dimethyl sulfoxide, trioxane, tetrahydrofuran, N-methyl-2-pyrrolidone, dimethylamine, monoethanolamine, pyridine, acetonitrile, etc. can be enumerated. They can be used alone or in combination of two or more. Among them, water or a mixed solvent of water and a lower alcohol having 1 to 3 carbon atoms is preferred.
[0107] A hydrophobic organic solvent may be further added to the above solvents as required. Examples of the hydrophobic organic solvent include higher alcohols such as 1-butanol, 2-butanol, isobutanol, tert-butanol, 1-pentanol, 2-pentanol, 3-pentanol, 2-methyl-1-butanol, isopentanol, tert-pentanol, 1-hexanol, 2-methyl-1-pentanol, 4-methyl-2-pentanol, 2-ethylbutanol, 1-heptanol, 2-heptanol, 3-heptanol, 2-octanol, 2-ethyl-1-hexanol, benzyl alcohol, and cyclohexanol; ether alcohols such as butyl cellosolve; Ketones such as methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone; esters such as ethyl acetate, butyl acetate, ethyl propionate, cellosolve acetate; pentane, 2-methylbutane, n-hexane, cyclohexane, 2-methylpentane, 2,2-dimethylbutane, 2,3-dimethylbutane, heptane, n-octane, isooctane, 2,2,3-trimethylpentane, decane, nonane, cyclopentane, methylcyclopentane, methylcyclohexane, ethylcyclohexane, p-menthane, dicyclohexyl, Aliphatic or aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, etc.; halogenated hydrocarbons such as carbon tetrachloride, trichloroethylene, chlorobenzene, tetrabromoethane, etc.; ethers such as diethyl ether, dimethyl ether, etc.; acetals such as methylal, diethyl acetal, etc.; hexamethylcyclotrisiloxane (D3), octamethylcyclotetrasiloxane (D4), decamethylcyclopentasiloxane (D5), dodecamethylcyclohexasiloxane (D6), tetradecamethylcycloheptasiloxane (D7), hexamethyldisiloxane, octamethyl Cyclic, linear or branched silicone oils and copolymers thereof such as trisiloxane, dimethylpolysiloxane such as decamethyltetrasiloxane, methylpolytrimethicone, methylphenylpolysiloxane, diphenylpolysiloxane, diphenylsiloxyphenylpolytrimethicone, trimethylsiloxyphenylpolydimethicone, caprylylpolymethicone, hexadecylpolydimethicone, etc.; organic compounds containing sulfur and nitrogen such as nitropropylene and nitrobenzene, etc.
[0108] It should be noted that in the present invention, the hydrophilic organic solvent refers to an organic solvent that maintains a uniform appearance when mixed with water in equal volumes, and the hydrophobic organic solvent refers to an organic solvent that maintains a uniform appearance when mixed with water in equal volumes, and the hydrophobic organic solvent 5 An organic solvent is an organic solvent that is not able to maintain a uniform appearance after the flow of the mixed liquid is stagnant when the mixed liquid is slowly mixed with the same volume of pure water at a temperature of 20°C.
[0109] In method 2, as a hydrophobic agent, the above-mentioned hydrophobic agent can be used, but it is necessary to appropriately select a hydrophobic agent that is not completely dissolved in the above-mentioned solvent. For example, carboxylates, amino acid derivative salts, sulfonates, and sulfates are preferred, and carboxylates and amino acid derivative salts from organisms are particularly preferred. In this way, particles that take the environment into consideration are obtained. It should be noted that as long as the solubility is adjusted by heating and cooling, and the hydrophobic agent is not completely dissolved in the solvent, it can be used as a hydrophobic agent.
[0110] Method 2 is characterized in that, during spray drying, the monovalent alginic acid salt is dissolved by at least any of the solvent and the temperature, and spray drying is performed in a state where the hydrophobic agent is not completely dissolved in the solvent.
[0111] In the above solution, the mixing ratio of monovalent alginate and hydrophobic agent is preferably monovalent alginate: hydrophobic agent = 99.9:0.1 to 70:30, more preferably 99.5:0.5 to 80:20, further preferably 99:1 to 85:15, further preferably 98:2 to 90:10. If the mixing ratio is within the above range, sufficient hydrophobicity can be obtained without reducing the degree of crosslinking.
[0112] In the above solution, the concentration of the solid content (monovalent alginic acid salt and hydrophobic agent) is preferably 1 to 80% by mass, more preferably 5 to 50% by mass.
[0113] Spray drying can be performed by a known method. For example, the above solution can be sprayed into hot air, for example, a conventional disk-type, two-fluid nozzle-type, jet airflow-type spray dryer can be used. The rotation speed of the disk can be about 1000 to 40000 rpm. The temperature of the hot air is preferably 60 to 250° C. at a temperature required for evaporating water. Alternatively, the above solution can be sprayed into the hot air while being heated.
[0114] Next, the particles obtained by spray drying (hereinafter also referred to as pre-crosslinked particles) are crosslinked using a polyvalent metal salt. The crosslinking treatment can be performed, for example, by dispersing the pre-crosslinked particles in a solvent, adding a solution containing a polyvalent metal salt to the dispersion, and stirring. Alternatively, the dispersion can be added to a solution containing a polyvalent metal salt and stirred.
[0115] The above-mentioned pre-crosslinked particles are preferably dispersed in a solvent in a concentration of 1 to 80% by mass, preferably 30 to 60% by mass. As the solvent for dispersing the above-mentioned particles, preferred are lower alcohols such as methanol, ethanol, 1-propanol, and 2-propanol; ether alcohols such as methyl cellosolve, ethyl cellosolve, isopropyl cellosolve, butyl cellosolve, and diethylene glycol monobutyl ether; and hydrophilic organic solvents such as acetone, tetrahydrofuran, dimethylformamide, N-methyl-2-pyrrolidone, and acetonitrile. In particular, a single solvent of a lower alcohol or a mixed solvent containing a lower alcohol is preferred.
[0116] The polyvalent metal salts include calcium salts, strontium salts, magnesium salts, barium salts, radium salts, lead salts, zinc salts, nickel salts, iron salts, copper salts, cadmium salts, cobalt salts, manganese salts, etc., and calcium salts are preferred from the perspectives of environment, safety, and versatility. Specifically, the polyvalent metal salts include calcium chloride, calcium sulfate, calcium carbonate, calcium hydroxide, calcium oxide, etc., and calcium chloride is preferred from the perspectives of solubility in water, handling properties, cost, etc.
[0117] The concentration of the polyvalent metal salt in the solution containing the polyvalent metal salt is preferably 1 to 40% by mass, more preferably 10 to 30% by mass. The solvent of the above solution is preferably water; a lower alcohol solvent such as methanol, ethanol, 1-propanol, 2-propanol; and a mixed solvent thereof, as long as the salt can be dissolved to a target concentration within a range that does not dissolve the particles, or a mixed solvent with other organic solvents.
[0118] The crosslinking treatment can be carried out while heating as needed. Heating can be carried out when a solution containing a polyvalent metal salt is added to the dispersion, or when stirring is carried out after addition, or in both. The temperature at this time is preferably 10 to 100°C, more preferably 20 to 80°C. The treatment time is preferably 0.5 to 24 hours, preferably 1 to 12 hours. By heating, the solubility of the hydrophobic agent can be increased, and the viscosity of the solvent is reduced, so that the hydrophobic agent is easily impregnated into the interior of the particles.
[0119] Since the above-mentioned particles before cross-linking contain the monovalent salt of alginic acid as a hydrophobic agent, the hydrophobic treatment is also performed simultaneously by the cross-linking treatment.
[0120] After the cross-linking treatment, the particles are cleaned and dried as required to obtain the amphiphilic alginic acid particles. The cleaning can be carried out by the usual method, for example, the solvent can be removed after the hydrophobic treatment, and water is added to carry out the methods such as centrifugation. The drying can be carried out by the usual method, for example, by methods such as spray drying, vacuum drying, freeze drying.
[0121] Method 3 is a method comprising the following steps: a step of forming a W / O emulsion containing a monovalent salt of alginic acid and a hydrophobic agent in water droplets; and a step of hydrophobizing the hydrophobic agent without completely dissolving the hydrophobic agent while performing cross-linking treatment using a polyvalent metal salt. As the monovalent salt of alginic acid, the same substance as the monovalent salt of alginic acid described in the description of method 2 can be cited. In addition, the hydrophobic agent needs to be present in the aqueous phase when the W / O emulsion is prepared, preferably the carboxylate, amino acid derivative salt, sulfonate, sulfate ester salt, and particularly preferably carboxylate and amino acid derivative salts from organisms. In this way, particles that take the environment into consideration are obtained.
[0122] An example of a method for forming a W / O emulsion is described. First, a monovalent salt of alginic acid is dissolved in water or a mixed solvent of water and a hydrophilic organic solvent to prepare a solution A in which a hydrophobic agent is not completely dissolved. At this time, the state of the target can also be adjusted by temperature adjustment such as heating and cooling as needed. Next, solution A is mixed with a hydrophobic organic solvent and emulsified using a stirring device, a homogenizer, etc. When mixing, solution A can be added to the hydrophobic organic solvent, or the hydrophobic organic solvent can be added to solution A.
[0123] At this time, a solution B prepared by dissolving a surfactant or a polymer stabilizer in a hydrophobic organic solvent in order to control the particle size of water droplets in the W / O emulsion may be used instead of the hydrophobic organic solvent. In this case, solution A and solution B are mixed and emulsified using a stirring device, a homogenizer, etc. During mixing, solution A may be added to solution B, or solution B may be added to solution A.
[0124] As another example of the method for forming a W / O emulsion, monovalent alginic acid salt, a hydrophobizing agent, water, a surfactant, a hydrophobic organic solvent, and other necessary components may be placed in a container and emulsified using a stirring device, a homogenizer, or the like.
[0125] The mixing ratio of monovalent alginic acid salt to hydrophobic agent is preferably monovalent alginic acid salt: hydrophobic agent = 99.9:0.1 to 70:30, more preferably 99.5:0.5 to 80:20, further preferably 99:1 to 85:15, and further preferably 98:2 to 90:10. If the mixing ratio is within the above range, sufficient hydrophobicity can be obtained without reducing the degree of crosslinking.
[0126] When forming a W / O emulsion, in order to stabilize the state of solution A, heating and cooling operations may be performed. By appropriately adjusting the temperature, the W / O emulsion can be stabilized, and the preferred state of the hydrophobic agent (the state in which the hydrophobic agent is not completely dissolved) can be more stable, so that it can be homogenized with the monovalent salt of alginic acid. As for the temperature when forming the W / O emulsion, although it also varies depending on the composition of the hydrophobic agent, the solvent, etc., it is preferably 5 to 100°C, and more preferably 15 to 80°C.
[0127] After the W / O emulsion is formed, a crosslinking treatment is performed. The crosslinking treatment can be performed by adding a solution containing a polyvalent metal salt to the W / O emulsion and stirring. Alternatively, the W / O emulsion can be added to a solution containing a polyvalent metal salt and stirred. Regarding the solution containing a polyvalent metal salt, the same solution as the solution described above in the description of method 2 can be used.
[0128] The crosslinking treatment can be carried out while heating as needed. Heating can be carried out when a solution containing a polyvalent metal salt is added to the dispersion, or when stirring is carried out after addition, or in both. The heating temperature is preferably 10 to 100° C., more preferably 15 to 80° C. The treatment time is preferably 0.5 to 24 hours, preferably 1 to 12 hours. By heating, the solubility of the hydrophobic agent can be increased, and the viscosity of the solvent is reduced, so that the hydrophobic agent is easily impregnated into the interior of the particles.
[0129] Since the water phase of the W / O emulsion contains a monovalent alginic acid salt and a hydrophobizing agent, the crosslinking treatment also simultaneously performs the intended hydrophobizing treatment.
[0130] After the cross-linking treatment, the particles are washed and dried as required to obtain an amphiphilic alginic acid particle group. Washing can be carried out by a common method, for example, removing the solvent after the cross-linking treatment, adding water and centrifuging. Drying can be carried out by a common method, for example, by spray drying, vacuum drying, freeze drying and the like.
[0131] According to method 2 or method 3, since the water repellent can be impregnated not only on the surface but also inside, the balance between hydrophilicity and hydrophobicity can be further adjusted.
[0132] The obtained amphiphilic alginic acid particles may be surface treated or pulverized by known equipment as needed.
[0133] [Application of amphiphilic alginate particles]
[0134] The amphiphilic alginic acid particles of the present invention can be dispersed in water, a hydrophilic organic solvent, a hydrophobic organic solvent or a mixed solvent thereof and used as a dispersion liquid.
[0135] The amphiphilic alginic acid particle group of the present invention can be used as an additive to liquids, coatings, films, plates, paper and other molded products. For example, it can be widely used in light scattering agents, optical filter materials, colorants, cosmetics, absorbents, adsorbents, inks, adhesives, electromagnetic wave shielding materials, fluorescent sensors, biomarkers, recording materials, recording elements, polarizing materials, drug delivery systems (DDS) drug holders, biosensors, DNA chips, inspection drugs, calcined cavitation molded products, anti-adhesion agents, etc.
[0136] Furthermore, in terms of using interior products such as window glass products, curtains, and wall materials to block light or ultraviolet rays (UV) that enter indoors and in cars, it is also useful in not only preventing sunlight exposure and adverse effects on the human body, but also preventing deterioration of indoor and car decorations.
[0137] The amphiphilic alginic acid particles of the present invention are suitable as cosmetic additives. It is the main component from natural polymers, and can be used in a large number of liquid components such as liquid systems while improving lightness, tactility, flow characteristics, solution dispersibility, etc. In addition, in the case of a concave shape, due to its unique shape, it has an adhesion different from the general spherical shape, and obtains an improvement in light scattering, etc., and has the effect of improving the fixing force of molded bodies such as foundations and the retention force after coating. Furthermore, due to its optical properties, the skin looks bright, and the covering power can be improved by a blurring effect. In addition, by the slipperiness of the shape, the ductility on the skin is excellent, and by finely filling the grooves of the texture, wrinkles and pores can be made inconspicuous, or the fluidity of the entire product can be freely controlled. As a preferred addition amount, relative to the product blending amount, it is 0.1 to 50% by mass, preferably 0.5 to 30% by mass. It can be appropriately adjusted according to the uses / purposes such as UV scattering effect, blurring effect, light scattering, fluidity, moldability, adhesion improvement, and finishing feeling. In addition, according to the research of the present inventors, as a cosmetic additive, 1 to 20% by mass is particularly preferred. In addition, it can also be used in combination with commercially available particles after appropriate adjustment.
[0138] Especially as cosmetics with high effects, specifically, they can be skin care products, hair products, antiperspirant products, makeup products, UV defense products, perfume products, etc. For example, emulsions, creams, lotions, color lotions, sunscreens, makeup base materials, sunscreens, after-shave lotions, before-shave lotions, mask materials, cleaning materials, wash fabrics, acne countermeasures cosmetics, basic cosmetics such as essences, foundations, white powder, mascara, eye shadow, eyeliner, eyebrow pencil, blush, nail colors, lipstick, lipstick and other makeup cosmetics, shampoo, conditioner, hair dye, hair tonic, setting agent, talcum powder, hair growth agent, deodorant, depilatory, soap, shower gel, shower agent, hand soap, perfume, etc. In addition, the form of the product is not particularly limited, and can be liquid, emulsion, paste, solid, paste, gel, powder, multi-layer, mousse, spray, etc. As additives for these cosmetics, useful effects can be expected.
[0139] The amphiphilic alginic acid particle group of the present invention can be used as an additive for printing inks used in screen printing, offset printing, color overprinting, gravure printing, flexographic printing, coaters, inkjet, etc., an additive for writing tools such as markers, ballpoint pens, fountain pens, watercolor pens, and all-purpose pens, and an additive for stationery such as crayons, drawing tools, and erasers.
[0140] The amphiphilic alginic acid particles of the present invention are suitable as a coating additive for brush coating, spray coating, electrostatic coating, electrodeposition coating, flow coating, roller coating, dip coating, etc. For example, it is suitable as a coating additive for transportation equipment such as automobiles, trams, helicopters, ships, bicycles, snowmobiles, ropeways, elevators, hovercrafts, motorcycles, window frames, shutters, water storage tanks, doors, balconies, building exterior panels, roofing materials, steps, skylights, concrete walls and other building components, indoor and outdoor exterior walls of buildings, interior decorations, guardrails, pedestrian bridges, soundproof walls, signs, highway side walls, railway viaducts, bridges and other road components, tanks, pipes, towers, chimneys and other equipment components, plastic greenhouses, greenhouses, silos, agricultural equipment such as agricultural sheets, telephone poles, power transmission towers, parabolic antennas and other communication equipment, electrical wiring boxes, lighting fixtures, air conditioner outdoor units, washing machines, refrigerators, microwave ovens and other electrical equipment, and covers thereof, souvenirs, tombstones, paving materials, windproof sheets, water-repellent sheets, building health sheets and other items.
[0141] As the form of the coating, in addition to solvent-based coatings, water-dispersible coatings, non-aqueous dispersion coatings, powder coatings, electrodeposition coatings, etc. can be appropriately selected as needed.
[0142] Example
[0143] The present invention is described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited to the following Examples. In the following Examples and Comparative Examples, the particle size distribution and the volume average particle size (MV) were measured using MICROTRACK MT3000 (manufactured by Nikkiso Co., Ltd.).
[0144] [1] Production of particle swarms
[0145] [Example 1-1] Production of Particle Group A1
[0146] The following components were placed in a 2000 mL flask, and stirred for 1 hour using a stirrer to disperse the components.
[0147]
[0148] Next, slowly heat it in an oil bath, and keep it constant for 3 hours at 35°C, where sodium laurate is not completely dissolved in the above-mentioned mixed solvent. It should be noted that the state in which sodium laurate is not completely dissolved in the above-mentioned mixed solvent at 35°C is confirmed by measuring the total light transmittance in advance (total light transmittance: 74%). Then, slowly heat it in an oil bath, and after heating at 95°C for 2 hours, remove the solvent by distillation, and implement surface treatment while concentrating the reaction solution, thereby performing hydrophobic treatment. After cooling, centrifugal washing is repeatedly performed by ion exchange water, and finally a 10% by mass aqueous dispersion is prepared. The dispersion is spray dried (hot air temperature 220°C) using a spray dryer to obtain the target particle group A1. Particle group A1 is observed with a scanning electron microscope (S-4800 made by Hitachi HiTech Nologis, hereinafter referred to as SEM) to confirm the shape. As a result, the particle size is roughly the same as before the hydrophobic treatment. In addition, the particle size distribution was confirmed by particle size distribution measurement. As a result, the same distribution as before the hydrophobic treatment was shown, so it was confirmed that there was no aggregation and monodispersed particle group. The SEM photo (2000 times) of particle group A1 is shown in Figure 1 .
[0149] [Example 1-2] Production of Particle Group A2
[0150] The following components were placed in a 5000 mL heatable container and dispersed using a stirrer.
[0151] Sodium alginate 313.6g
[0152] (Manufactured by Kimika Co., Ltd.: Trade name: Kimika Algin ULV-L3 (40 mPa·s, 10 mass % aqueous solution))
[0153] Ion exchange water 4260.0g
[0154] Sodium stearoyl glutamate 6.4g
[0155] Then, it was heated to 60°C and dissolved in 2 hours to prepare a 7.0% by mass aqueous solution. Next, the obtained aqueous solution was temperature-adjusted at 20°C, where sodium stearoyl glutamate was not completely dissolved in the above-mentioned solvent, and spray-dried using a spray dryer (hot air temperature 200°C), to obtain a particle group. It should be noted that the state in which sodium stearoyl glutamate was not completely dissolved in the above-mentioned solvent at 20°C was confirmed by measuring the total light transmittance in advance (total light transmittance: 65%). The obtained particle group was observed with SEM to confirm the shape. As a result, it was a flat particle with a depression, and it was a monodisperse particle group with an MV of 7μm in the particle size distribution.
[0156] 300.0 g of the obtained particle group was put into 300.0 g of ethanol and stirred to prepare a 50.0 mass % ethanol dispersion, which was then added dropwise to a pre-made 20.0 mass % calcium chloride aqueous solution while stirring to perform a crosslinking treatment. After the addition was completed, the mixture was further stirred at 50° C. for 2 hours.
[0157] After the stirring is completed, the mixture is repeatedly centrifuged and washed with ion exchange water to finally prepare a 10% aqueous dispersion by mass. The dispersion is spray dried using a spray dryer to obtain the target particle group A2. The particle group A2 is observed with SEM to confirm the shape. As a result, the particle size is roughly the same as before the crosslinking treatment. In addition, the particle size distribution is confirmed by particle size distribution measurement. As a result, the same distribution as before the crosslinking treatment is shown, so it is confirmed to be a monodisperse particle group without agglomeration. The SEM photo (1000 times) of the particle group A2 is shown in Figure 2 .
[0158] [Example 1-3] Production of Particle Group A3
[0159] The following components were placed in a 5000 mL heatable container, and stirred for 5 minutes using a homogenizer (T25 manufactured by IKA Corporation) to emulsify the mixture.
[0160]
[0161] 15.0 mass % calcium chloride aqueous solution was added dropwise thereto, and after the addition was completed, it was stirred at 50°C for 2 hours. After stirring, it was cooled, centrifuged and washed repeatedly by ethanol and ion exchange water, and vacuum dried to obtain a particle group. The obtained particle group was observed by SEM to confirm the shape, and the result was spherical particles. In addition, the result of the particle size distribution measurement was a monodisperse calcium alginate particle group (hereinafter referred to as calcium alginate particle group A) with a MV of 10 μm.
[0162] Next, each component shown below was placed in a 2000 mL flask, and stirred for 1 hour using a stirrer to disperse the components.
[0163]
[0164] Then, slowly heated by an oil bath, the mixture was kept constant for 3 hours at 50°C, where sodium stearate was not completely dissolved in the above-mentioned mixed solvent. It should be noted that, as for the state in which sodium stearate was not completely dissolved in the above-mentioned mixed solvent at 50°C, it was confirmed by measuring the total light transmittance in advance (total light transmittance: 58%). Then, gradually heated by an oil bath, the solvent was removed by distillation at 95°C for 2 hours, and the surface treatment was implemented while concentrating the reaction solution, thereby performing a hydrophobic treatment. After cooling, centrifugal washing was repeatedly performed by ion exchange water, and a 10% by mass aqueous dispersion was finally prepared. The dispersion was spray dried (hot air temperature 200°C) using a spray dryer to obtain a target particle group A3. The particle group A3 was observed with an SEM to confirm the shape, and the result was a particle size roughly the same as before the hydrophobic treatment. In addition, the particle size distribution was confirmed by a particle size distribution measurement, and the result showed the same distribution as before the hydrophobic treatment, so it was confirmed to be a monodisperse particle group without agglomeration. The SEM photograph (2000 times) of particle group A3 is shown in Figure 3 .
[0165] [Example 1-4] Production of Particle Group A4
[0166] 1725.0 g of ion exchange water was placed in a 5000 mL heatable container, the temperature was raised to 50° C., and 148.5 g of sodium alginate (manufactured by Fuji Chemical Industry Co., Ltd.: trade name Snoalgin SSL (40 mPa·s, 1 mass % aqueous solution)) and 1.5 g of sodium myristoyl glutamate were added and completely dissolved. A solution prepared by dissolving 12.0 g of sorbitan trioleate in 1550.0 g of hexane in advance was added thereto, and the mixture was stirred for 5 minutes using a homogenizer (T25 manufactured by IKA Corporation) while maintaining the temperature to emulsify the mixture.
[0167] Then, the mixture was slowly heated in an oil bath, and a 20.0% by mass calcium chloride aqueous solution was slowly added dropwise while the temperature was kept constant at 45° C., which was a state in which sodium myristoyl glutamate was not completely dissolved in the solvent. It should be noted that the state in which sodium myristoyl glutamate was not completely dissolved in the solvent at 45° C. was confirmed by measuring the total light transmittance in advance (total light transmittance: 66%). After the addition was completed, the mixture was stirred at the same temperature for 2 hours, and then the temperature was further slowly raised to 65° C., and the mixture was stirred for another 2 hours while the temperature was maintained.
[0168] After stirring, cool to room temperature, centrifuge repeatedly with ethanol and ion exchange water to finally make 10 mass % aqueous dispersion. Spray dryer is used to spray dry the dispersion (hot air temperature 200 ° C) to obtain target particle group A4. Particle group A4 is observed with SEM to confirm the shape, and the result is spherical particles. In addition, the result of particle size distribution measurement is a monodisperse particle group with MV of 3 μm.
[0169] [Example 1-5] Production of Particle Group A5
[0170] The following components were placed in a 5000 mL flask and stirred for 3 hours using a stirrer to dissolve them.
[0171] Potassium alginate 285.0g
[0172] (Manufactured by Kimika Co., Ltd.: Trade name: Kimika Algin K-ULV-L3 (40 mPa·s, 10 mass % aqueous solution))
[0173] Ion exchange water 3450.0g
[0174] Sodium palmitate 15.0g
[0175] The obtained aqueous solution was temperature-adjusted at 20°C, where the sodium palmitate was not completely dissolved in the above-mentioned solvent, and spray-dried using a spray dryer (hot air temperature 200°C), to obtain a particle group. It should be noted that the state in which the sodium palmitate was not completely dissolved in the above-mentioned solvent at 20°C was confirmed by measuring the total light transmittance in advance (total light transmittance: 61%). The obtained particle group was observed with SEM to confirm the shape, and the result was spherical or approximately spherical particles. In addition, the result of the particle size distribution measurement was a monodisperse particle group with a MV of 33μm.
[0176] 270.0 g of the obtained particle group was put into 330.0 g of ethanol and stirred to prepare a 45.0 mass % ethanol dispersion, which was then added dropwise to a pre-prepared 20.0 mass % calcium chloride aqueous solution while stirring to perform a crosslinking treatment. After the addition was completed, the mixture was further stirred at 50° C. for 3 hours.
[0177] After stirring finishes, centrifugal cleaning is repeatedly carried out by ion exchange water, and finally 15 mass % aqueous dispersion is made. Use spray dryer to carry out spray drying to this dispersion, obtain target particle group A5. Observe particle group A5 with SEM, confirm shape, result, be the particle diameter roughly the same as before crosslinking treatment. In addition, confirm particle size distribution by particle size distribution measurement, result, demonstrate the same distribution as before crosslinking treatment, therefore confirm as not cohesive and monodisperse particle group.
[0178] [Example 1-6] Production of Particle Group A6
[0179] The following components were placed in a 5000 mL heatable container and dispersed using a stirrer.
[0180] Sodium alginate 368.0g
[0181] (Manufactured by Kimika Co., Ltd.: Trade name: Kimika Algin ULV-L3 (40 mPa·s, 10 mass % aqueous solution))
[0182] Ion exchange water 3500.0g
[0183] Sodium dodecylbenzenesulfonate 32.0g
[0184] Then, it was heated to 60°C and dissolved in 2 hours to prepare a 10.0 mass % aqueous solution. Next, the temperature was adjusted at 50°C, which is a state where sodium dodecylbenzene sulfonate is not completely dissolved in the above-mentioned solvent, and the above-mentioned aqueous solution was spray-dried using a spray dryer (hot air temperature 200°C) to obtain a particle group. It should be noted that the state where sodium dodecylbenzene sulfonate is not completely dissolved in the above-mentioned solvent at 50°C was confirmed by measuring the total light transmittance in advance (total light transmittance: 70%). The obtained particle group was observed with SEM to confirm the shape. As a result, it was a flat particle with a depression, and it was a monodisperse particle group with a MV of 8μm in the particle size distribution.
[0185] 300.0 g of the obtained particle group was put into 300.0 g of ethanol and stirred to prepare a 50.0 mass % ethanol dispersion, which was then added dropwise to a pre-made 20.0 mass % calcium chloride aqueous solution while stirring to perform a crosslinking treatment. After the addition was completed, the mixture was further stirred at 40° C. for 2 hours.
[0186] After stirring finishes, centrifugal cleaning is repeatedly carried out by ion exchange water, and finally 10 mass % aqueous dispersion is made. Use spray dryer to carry out spray drying to this dispersion, obtain target particle group A6. Observe particle group A6 with SEM, confirm shape, result, be the particle diameter roughly the same as before crosslinking treatment. In addition, confirm particle size distribution by particle size distribution measurement, result, demonstrate the same distribution as before crosslinking treatment, therefore confirm as not cohesive and monodisperse particle group.
[0187] [Example 1-7] Production of Particle Group A7
[0188] The following components were placed in a 5000 mL heatable container and dispersed using a stirrer.
[0189]
[0190] Then, it was heated to 60°C and dissolved in 2 hours to prepare a 10% by mass aqueous solution. Next, the temperature was adjusted at 45°C, which was a state in which the adjusted disodium dodecanedioate was not completely dissolved in the above-mentioned solvent, and the above-mentioned aqueous solution was spray-dried using a spray dryer (hot air temperature 200°C) to obtain a particle group. It should be noted that the state in which disodium dodecanedioate was not completely dissolved in the above-mentioned solvent at 45°C was confirmed by measuring the total light transmittance in advance (total light transmittance: 68%). The obtained particle group was observed with SEM to confirm the shape. As a result, it was a flat particle with a depression, and it was a monodisperse particle group with an MV of 12μm in the particle size distribution.
[0191] 300.0 g of the obtained particle group was placed in 300.0 g of isopropyl alcohol and stirred to prepare a 50.0 mass % isopropyl alcohol dispersion, which was then added dropwise to a pre-prepared 20.0 mass % calcium chloride aqueous solution while stirring to perform a crosslinking treatment. After the addition was completed, the mixture was further stirred at 50° C. for 2 hours.
[0192] After stirring finishes, centrifugal cleaning is repeatedly carried out by ion exchange water, and finally 10 mass % aqueous dispersion is made. Use spray dryer to carry out spray drying to this dispersion, obtain target particle group A7. Observe particle group A7 with SEM, confirm shape, result, be the particle diameter roughly the same as before crosslinking treatment. In addition, confirm particle size distribution by particle size distribution measurement, result, demonstrate the same distribution as before crosslinking treatment, therefore confirm as not cohesive and monodisperse particle group.
[0193] [Comparative Example 1-1]
[0194] The calcium alginate spherical beads (manufactured by Nisshinbo Chemical Co., Ltd.: trade name: Flaviken, MV=20 μm) used in Example 1-1 were designated as particle group B1.
[0195] [Comparative Example 1-2] Production of Particle Group B2
[0196] The following components were placed in a 5000 mL flask and stirred for 2 hours using a stirrer to dissolve them.
[0197] Sodium alginate 400.0g
[0198] (Made by Kimika Co., Ltd.: Trade name: Kimika Algin ULV-L3G (20 mPa·s) 10 mass %)
[0199] Ion exchange water 3600.0g
[0200] The obtained aqueous solution was spray dried using a spray dryer (hot air temperature 200° C.) to obtain particle group B2. The obtained particles were observed using SEM to confirm the shape. As a result, they were spherical or approximately spherical particles. In addition, the result of the particle size distribution measurement was monodisperse particles with a MV of 11 μm.
[0201] [Comparative Examples 1-3]
[0202] The particle group before the crosslinking treatment obtained in the middle of Example 1-2 was designated as particle group B3.
[0203] [Comparative Example 1-4] Production of Particle Group B4
[0204] The following components were added at once to a 2000 mL flask, and a single polymethyl methacrylate spherical polymer particle group B4 having an average particle diameter of 5 μm was prepared by the same method as in Comparative Example 1-3 of International Publication No. 2016 / 181877.
[0205]
[0206] Table 1 shows the shapes, main materials, water repellent agents, and MVs of particle groups A1 to A7 and B1 to B4 in summary.
[0207] [Table 1]
[0208]
[0209] [2] Determination of basic physical properties
[0210] [Examples 2-1 to 2-7, Comparative Examples 2-1 to 2-4]
[0211] For particle groups A1 to A7 and B1 to B4, the contact angle, water absorption, and oil absorption were measured by the following methods, and the heat resistance, chemical resistance, and heat-resistant chemical resistance were evaluated.
[0212] [Measurement of contact angle]
[0213] Particle groups A1 to A7 and B1 to B4 were applied to an acrylic plate with a double-sided tape, and then a water drop was dropped thereon to measure the contact angle after 30 seconds using a contact angle meter (Drop Master 300 manufactured by Kyowa Interface Science Co., Ltd.).
[0214] [Determination of oil absorption]
[0215] The oil absorption was measured according to the boiled linseed oil method described in JIS K 5101. Table 2 shows the results.
[0216] [Determination of water absorption]
[0217] 1 g of each particle group was added to a 500 mL beaker, followed by 200 mL of ion exchange water, and the mixture was suspended and stirred for 30 minutes (150 rpm, 25°C), then transferred to a 500 mL centrifuge tube and centrifuged at 2000 G for 30 minutes using a centrifuge (himac CR20GII, manufactured by Koki Holdecone Co., Ltd.). After centrifugation, the supernatant was discarded, and the sample was taken out from the centrifuge tube and its weight (W) was measured. w ), and then dried in a dryer at 105°C until it becomes constant, and the dry weight (D w ), and the water absorption was calculated according to the following formula. The results are shown in Table 2.
[0218] Water absorption (mL / 100g) = {(W w -D w ) / D w}×100
[0219] [Evaluation of heat resistance]
[0220] 0.5 g of each particle group was added to an aluminum dish and heated in a dryer at 180° C. for 2 hours, then the melting of the particles was visually confirmed, the shape was confirmed by SEM, and the particles were evaluated according to the following evaluation criteria.
[0221] [Evaluation criteria]
[0222] Visual inspection: ○: no major change, △: partial melting, ×: melting
[0223] SEM: 1: Particle shape is produced, 2: Shape is maintained and the surface is partially melted, 3: Partially melted and part of the particle shape is maintained, 4: No particle shape (completely melted)
[0224] [Evaluation of chemical resistance]
[0225] 1 g of each particle group and 99 g (1% by mass) of the solvent shown in Table 3 were added to a 300 mL flask, and after stirring at room temperature (25° C.) for 2 hours, the dispersion state of the particles was confirmed by visual inspection, the shape was confirmed by SEM, and the evaluation was performed according to the following evaluation criteria. The results are shown in Table 3.
[0226] [Evaluation of heat resistance to chemicals]
[0227] 1 g of each particle group and 99 g (1% by mass) of the solvent shown in Table 3 were added to a 300 mL flask, and after stirring at 70° C. for 2 hours, the dispersion state of the particles was visually confirmed, the shape was confirmed by SEM, and the evaluation was performed according to the following evaluation criteria. The results are shown in Table 3.
[0228] [Evaluation criteria]
[0229] ◎: Visually dispersed, SEM shows the shape of the produced particles
[0230] ○: Visually dispersed, shape maintained in SEM, partial surface melting
[0231] △: Partial dispersion observed visually, deformation observed in SEM
[0232] ×: Dissolved visually, no shape in SEM
[0233] [Table 2]
[0234]
[0235] [Table 3]
[0236]
[0237] [3] Functional test and adhesion evaluation
[0238] [Examples 3-1 to 3-7, Comparative Examples 3-1 to 3-4]
[0239] The particle groups A1 to A7 and B1 to B4 were evaluated for skin feel, slip properties, and particle adhesion by the following methods.
[0240] (1) Skin feel
[0241] The touch when each particle group was spread on the skin was evaluated according to the following evaluation criteria.
[0242] (2) Sliding properties
[0243] 1 g of each particle group was placed on black artificial leather, and the length when spread with fingers was evaluated according to the following evaluation criteria.
[0244] (3) Particle Adhesion
[0245] 1 g of each particle group was placed on black artificial leather and evenly spread with a puff. The artificial leather was then tapped three times, and the amount of remaining particles was observed with a digital microscope (VHX200 manufactured by KEYANCE CO., LTD.) and evaluated according to the following evaluation criteria.
[0246] [Evaluation criteria]
[0247] ◎: Very good, ○: Good, △: Standard, ×: Poor
[0248] [Table 4]
[0249]
[0250] For skin feel and slippage, the hydrophobized particle groups A1 to A7 as alginate particle group have properties equal to or above those of polymer particles B4, and with respect to particle adhesion, if the particle size is at the same level, the same adhesion can be maintained. On the other hand, for the particle groups B1 and B2 that are not hydrophobized, there is a tendency that skin feel and slippage are somewhat reduced due to hygroscopicity. In addition, the uncrosslinked hydrophobized particle group B3 also has a tendency that skin feel and slippage are reduced as the hygroscopicity of the base particles deteriorates.
[0251] [4] Sodium chloride aqueous solution dissolution test
[0252] [Examples 4-1 to 4-7, Comparative Examples 4-1 to 4-4]
[0253] The particle groups A1 to A7 and B1 to B4 were each dispersed in water or a sodium chloride aqueous solution (sodium chloride concentration: 3 mass %) to give 0.1 mass %, and a solubility test was conducted.
[0254] (1) Appearance: After dispersion, the state after 72 hours was visually confirmed.
[0255] (2) Shape: After dispersion in a sodium chloride aqueous solution, changes in shape were confirmed by particle size distribution measurement after 72 hours, 240 hours, and 720 hours.
[0256] (3) Transmittance: Each particle group was dispersed in a sodium chloride aqueous solution, and the transmittance of the light of wavelength 560 nm of the dispersion after 72 hours, 240 hours and 720 hours was denoted as SD1 (%), SD2 (%) and SD3 (%), respectively. Each particle group was dispersed in water, and the transmittance of the light of wavelength 560 nm of the dispersion after 72 hours, 240 hours and 720 hours was denoted as WD1 (%), WD2 (%) and WD3 (%), respectively, and WD1 / SD1, WD2 / SD2 and WD3 / SD3 were obtained. The transmittance was measured using an ultraviolet visible spectrophotometer (UV-2450 manufactured by JASCO Corporation).
[0257] The results are shown in Table 5.
[0258] [Table 5]
[0259]
[0260] [5] Preparation and evaluation of optical measurement films
[0261] [Examples 5-1 to 5-7, Comparative Examples 5-1 to 5-4]
[0262] 35.0 g of binder resin (PVA resin manufactured by Kuraray Co., Ltd.) and 75.0 g of purified water were added to 15.0 g of each of particle groups A1 to A7 and B1 to B4, and mixed to prepare a composition for optical measurement sheets. Each of the obtained compositions was applied to one side of a 100 μm thick PET film (E-5000 manufactured by Toyobo Co., Ltd.) using a commercially available bar coater, and then the dryer was set to 60° C. and hot air dried for 20 minutes to prepare optical sheets 1 to 11 with a coating layer thickness of 40 μm.
[0263] Optical sheets 1 to 11 were irradiated with a certain amount of light at an incident angle of 45° using an automatic goniophotometer (GonioPhotometer GP-200 manufactured by Murakami Color Research Laboratory Co., Ltd.), and the light scattering distribution of the reflected light was measured to evaluate the diffusion performance according to the following evaluation criteria.
[0264] [Evaluation criteria]
[0265] Based on the optical sheet 11 (polymer particle group B4)
[0266] A: Good diffusion
[0267] B: Diffusion is roughly the same
[0268] C: Poor diffusion
[0269] [Table 6]
[0270]
[0271] It was confirmed that the hydrophobic treatment can provide performance equal to or better than that of general-purpose polymer particles.
[0272] [6] Water repellency evaluation
[0273] [Examples 6-1 to 6-7, Comparative Examples 6-1 to 6-4]
[0274] Particle groups A1 to A7 and B1 to B4 were added to a commercially available oil-based paint (Protach manufactured by Lock Paint Co., Ltd.) at 5% by mass, applied to an aluminum substrate, and dried to form a film having a thickness of 2 μm after drying, thereby producing coated sheets 1 to 11.
[0275] The reflectivity of light and the presence of gloss of the obtained coating film were visually evaluated, and the sensory evaluation of the tactile effect was performed. As for the tactile effect, the coating film was traced with a finger, and the softness was evaluated according to the following evaluation criteria. As a blank, an aluminum substrate without a film was used. The results are shown in Table 7.
[0276] [Evaluation criteria]
[0277] ○: Yes, △: Somewhat (felt), ×: No
[0278] [Table 7]
[0279]
[0280] The coating sheets 1 to 7 including the particle groups A1 to A7 showed high hiding power and could be used as matting agents.
[0281] [7] Preparation and evaluation of skin cleansing compositions
[0282] [Examples 7-1 to 7-3, Comparative Example 7-1]
[0283] Using particle group A1, A5, A7 or B1, skin cleansing compositions (cleansing compositions 1 to 4) were prepared according to the compositions shown in Table 8 below.
[0284] [Table 8]
[0285]
[0286] Each of the prepared cleaning compositions was evaluated by the following method. The results are shown in Table 9.
[0287] Ten people were selected as evaluation panelists, and a use test of the skin cleansing composition by face washing was carried out. The six items of feeling 1, feeling 2, foaming property, skin dirt, keratin removal effect, massage effect, and irritation were evaluated according to the following evaluation criteria, and based on the evaluation, a comprehensive evaluation as a scrub was performed.
[0288] · Usage experience 1: Good application feeling and affinity with skin during use
[0289] · User experience 2: There is less residual feeling of scrub after rinsing off the cleanser, and less discomfort on the skin
[0290] Foaming property: Good foaming and foam retention when using cleaning agent
[0291] · Effect of removing dirt and dead skin cells from the skin: How makeup falls off after use
[0292] Massage effect: After washing, can you feel the effects of massage, such as the reduction of dullness, improvement of skin color, and promotion of blood circulation?
[0293] Irritation: Less redness, stinging, etc. after rinsing off the detergent
[0294] [Evaluation criteria for each item]
[0295] ◎: Effective (good feeling) [8 or more people give a high rating]
[0296] ○: The effect was confirmed (slightly better feeling) [6-7 people rated it highly]
[0297] □: The effect was confirmed (slightly better feeling) [4-5 people rated it highly]
[0298] △: Not very effective (slightly poor feeling) [2-3 people rated it highly]
[0299] ×: No effect (no feeling) [1 or less is a high rating]
[0300] [Score Evaluation]
[0301] ◎: 8 points ○: 6 points □: 4 points △: 2 points ×: 0 points
[0302] [Overall evaluation]
[0303] A: 36 points or more
[0304] B: 28-35 minutes
[0305] C: 20-27 points
[0306] D: 19 points or less
[0307] [Table 9]
[0308]
[0309] As shown in Table 9, it can be seen that the amphiphilic alginic acid particles of the present invention can also be used as an additive (raw material) for a body cleansing composition from the viewpoints of touch and foaming properties.
[0310] [8] Production and evaluation of skin cosmetics 1
[0311] [Examples 8-1 to 8-4, Comparative Examples 8-1 to 8-2]
[0312] Using particle group A2, A3, A4, A7, B1 or B4, cosmetic compositions (foundations 1 to 6) were prepared according to the compositions shown in Table 10 below.
[0313] [Table 10]
[0314]
[0315] 15 people were selected as the evaluation panel members to comprehensively evaluate the five items of "adhesion to the skin", "fitting feeling when applied", "feeling of use", "soft focus", and "duration of makeup effect (4 hours)" for foundations 1 to 6 in terms of usage feeling and the difference before and after use. Regarding whether the foundations 1 to 6 can be combined with cosmetics, they were evaluated using the following A to G.
[0316] A: Foundation 1 is good
[0317] B: Foundation 2 Good
[0318] C: Foundation 3 Good
[0319] D: Foundation 4 Good
[0320] E: Foundation 5 Good
[0321] F: Foundation 6 Good
[0322] G: All the same
[0323] As a result, the evaluation team members' evaluation was
[0324] A: 4 people
[0325] B: 3 people
[0326] C: 5 people
[0327] D: 2 people
[0328] E: 0
[0329] F: 1 person
[0330] G: 0.
[0331] It should be noted that regarding Foundation 1 and Foundation 3, "adhesion to the skin", "soft focus", and "duration of the makeup effect (4 hours)" are particularly excellent, and most people give a good overall evaluation. Regarding "feel of fit during application" and "feel of use", there are preferences for Foundations 1 to 4, and although opinions vary, there are many opinions that the performance is equal to or better than that of the polymer component of Foundation 6 due to particle size reduction and hydrophobic treatment, and that it can be used without damage. In addition, regarding Foundation 4, many people feel that it has elasticity (softness). On the other hand, regarding Foundation 6, many people say that it is slightly lacking in "adhesion to the skin" and "feel of use". Therefore, it is confirmed that the alginate particle group of the present invention can also exert characteristics equal to or better than those of the alginate particle group known so far as a cosmetic raw material.
[0332] [9] Production and evaluation of skin cosmetics 2
[0333] [Examples 9-1 to 9-4, Comparative Examples 9-1 to 9-2]
[0334] Using particle group A2, A3, A4, A7, B1 or B4, cosmetic compositions (liquid foundations 7 to 12) were prepared according to the compositions shown in Table 11 below.
[0335] [Table 11]
[0336]
[0337] 15 people were selected as the evaluation panel members to comprehensively evaluate the five items of "adhesion to the skin", "fitting feeling when applied", "feeling of use", "soft focus", and "duration of makeup effect (4 hours)" for foundations 7 to 12 in terms of usage feeling and the difference before and after use. The following A to G were used to evaluate whether they can be combined with cosmetics.
[0338] A: Foundation 7 Good
[0339] B: Foundation 8 Good
[0340] C: Foundation 9 Good
[0341] D: Foundation 10 Good
[0342] E: Foundation 11 Good
[0343] F: Foundation 12 Good
[0344] G: All the same
[0345] As a result, the evaluation team members' evaluation was
[0346] A: 4 people
[0347] B: 3 people
[0348] C: 3 people
[0349] D: 4 people
[0350] E: 0
[0351] F: 1 person
[0352] G: 0.
[0353] It should be noted that regarding foundations 7 to 10, there are many opinions that give good comprehensive evaluations on "adhesion to the skin", "fitting feeling when applying", "feeling when using", "soft focus", and "duration of makeup effect (4 hours)". In particular, there are preferences for foundations 7 to 10. Although opinions vary, from the perspective of imparting smoothness due to hydrophobic treatment, there are many opinions that are good about "fitting feeling when applying" and "feeling when using". In addition, there are opinions that the emulsified handling, stability, and dispersibility are excellent, and there are many opinions that the performance is equal to or better than that of the polymer component of the previous foundation 12 and can be used without damage. In addition, for foundation 10, there are many opinions that elasticity (softness) is felt. On the other hand, for foundation 11, there are many opinions that "adhesion to the skin", "fitting feeling when applying", and "feeling when using" are slightly lacking. As a result, it is confirmed that the alginate particle group of the present invention can also exert characteristics equal to or better than those of the alginate particle group so far as a liquid-based cosmetic raw material.
[0354] As described above, the amphiphilic alginic acid particles of the present invention have few foreign matters such as aggregates, can be produced stably and efficiently, and can also stably produce heat-resistant, (thermal) chemical-resistant and cross-linked particles, and can therefore be used in various applications.
[0355] In addition, the amphiphilic alginate particle group of the present invention has a controlled particle size and is environmentally friendly. In particular, as a soluble component from natural polymers that can be used to counter marine pollution, it can be effectively applied to applications required for environmental response such as coatings, inks, molded products, cosmetics, and calcined hollow molded products depending on the application.
Claims
1. An amphiphilic alginic acid particle group, which is an amphiphilic alginic acid particle group formed by hydrophobizing an alginic acid multivalent metal salt using a hydrophobizing agent, wherein: The particles are formed by chemically bonding a part of the metal ions of the polyvalent metal salt of alginic acid to the hydrophobic agent to be hydrophobic, the contact angle of water droplets falling on the particle group after 30 seconds is 30° or more and 150° or less, the water absorption per 100g of the particles is equal to or greater than the oil absorption per 100g of the particles, The hydrophobic agent is a carboxylate having 6 to 30 carbon atoms, an amino acid derivative salt having 6 to 30 carbon atoms, a sulfonate having 6 to 30 carbon atoms, an alkyl sulfate having 6 to 30 carbon atoms, a polyoxyethylene aryl ether sulfate having an HLB value of 11 or less, a polyoxyethylene alkyl ether sulfate having an HLB value of 6 or less, a polyoxyalkylene alkyl ether sulfate having an HLB value of 11 or less, a polyoxyalkylene alkenyl ether sulfate having an HLB value of 11 or less, or a polyoxyethylene castor oil ether sulfate having an HLB value of 11 or less.
2. The amphiphilic alginate particles according to claim 1, wherein The hydrophobic agent is at least one selected from carboxylate salts and amino acid derivative salts.
3. The amphiphilic alginate particles according to claim 1 or 2, wherein The metal is a metal that becomes a divalent ion.
4. The amphiphilic alginate particles according to claim 3, wherein The metal is calcium.
5. The amphiphilic alginate particles according to claim 1 or 2, wherein At 25°C, it is insoluble in water but soluble in a 3% by mass sodium chloride aqueous solution.
6. The amphiphilic alginate particles according to claim 1 or 2, wherein The average particle size is less than 5 mm.
7. The amphiphilic alginate particles according to claim 1 or 2, wherein: The amphiphilic alginate particles are dispersed in a 3% by mass sodium chloride aqueous solution in a manner of 0.1% by mass, and the transmittances of the dispersion at a wavelength of 560 nm after 72 hours, 240 hours and 720 hours are set to SD1, SD2 and SD3, respectively. When the amphiphilic alginate particles are dispersed in water in a manner of 0.1% by mass, and the transmittances of the dispersion at a wavelength of 560 nm after 72 hours, 240 hours and 720 hours are set to WD1, WD2 and WD3, respectively, at least one of WD1 / SD1, WD2 / SD2 and WD3 / SD3 is less than 0.
9.
8. The amphiphilic alginate particles according to claim 1, wherein The cation of the salt of the hydrophobic agent is a metal ion.
9. The amphiphilic alginate particles according to claim 1, wherein The cation of the salt of the hydrophobic agent is a monovalent metal ion. 10 . A cosmetic comprising the amphiphilic alginate particles according to claim 1 .
11. A coating comprising the amphiphilic alginate particles according to any one of claims 1 to 9. 12 . A resin composition comprising the amphiphilic alginate particles according to claim 1 .
13. A molded article comprising the amphiphilic alginate particles according to any one of claims 1 to 9. 14 . An electronic material comprising the amphiphilic alginate particles according to claim 1 . 15 . A sheet comprising the amphiphilic alginate particles according to claim 1 .
16. A method for producing the amphiphilic alginate particles according to claim 1, comprising: A step of hydrophobizing a group of alginic acid particles containing a polyvalent metal salt of alginic acid using a hydrophobizing agent without completely dissolving the hydrophobizing agent, The state in which the hydrophobic agent is not completely dissolved means a state having both a portion in which the hydrophobic agent is dissolved and a portion in which the hydrophobic agent is dispersed in the solvent.
17. A method for producing the amphiphilic alginate particles according to claim 1, comprising: A step of spray drying a solution containing monovalent alginate and an incompletely dissolved hydrophobic agent to obtain particles; and a step of performing a hydrophobic treatment while cross-linking the particles using a polyvalent metal salt, The state in which the hydrophobic agent is not completely dissolved means a state having both a portion in which the hydrophobic agent is dissolved and a portion in which the hydrophobic agent is dispersed in the solvent.
18. A method for producing the amphiphilic alginate particles according to claim 1, comprising: A step of forming a water-in-oil emulsion containing monovalent alginic acid salt and an incompletely dissolved hydrophobic agent in water droplets; and a step of performing a hydrophobic treatment while the hydrophobic agent is not completely dissolved while performing the crosslinking treatment using a polyvalent metal salt, The state in which the hydrophobic agent is not completely dissolved means a state having both a portion in which the hydrophobic agent is dissolved and a portion in which the hydrophobic agent is dispersed in the solvent.