A method for preparing self-repairing conductive ion hydrogel
By combining the carbamite-shaped chitosan with electrolyte solution and using centrifugal force to assist, a self-healing conductive ion hydrogel is formed, which solves the problem of low self-healing efficiency of natural polymer conductive hydrogels and achieves the stability of conductivity and biocompatibility.
Patent Information
- Application Number
- CN202211562941.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-07
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2042-12-07
AI Technical Summary
Existing natural polymer conductive hydrogels are susceptible to damage under external forces, and have low self-repair efficiency and speed, making it difficult to take into account both conductivity, biocompatibility and biodegradability.
The combination of chemosaccharide and electrolyte solutions such as LiCl, LiBr, and NaCl is used to form a self-healing conductive ion hydrogel through centrifugal force assistance, and the intramolecular/inter-hydrogen bonding and chain entanglement are used to achieve rapid and efficient self-healing. .
It realizes efficient and fast self-healing of conductive ionic hydrogels, has strong conductivity stability, takes into account both biocompatibility and biodegradability, and breaks through the limitations of traditional low self-healing efficiency.
Smart Images

Figure CN115926199B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of natural polymer conductive ion gel materials, and specifically relates to a preparation method of a self-repairing conductive ion hydrogel, and in particular to a plantago chitosan polysaccharide conductive ion hydrogel. Background Art
[0002] Natural polymer conductive hydrogels are mainly based on natural polysaccharides or polypeptide macromolecular polymers and conductive fillers, and are constructed through intramolecular / intermolecular hydrogen bonds, ionic bonds and other chemical bonds. Compared with traditional metal or semiconductor conductive materials, natural polymer conductive hydrogels have attracted much attention for their biodegradability, green environmental protection and high body affinity. However, natural conductive hydrogels are susceptible to high deformation or structural damage caused by external forces during use, resulting in the loss of the basic functions of conductive hydrogels, and the development of self-healing conductive hydrogels has emerged. The self-healing mechanism of natural polymer hydrogels mainly includes exogenous self-healing materials and intrinsic self-healing materials. Exogenous self-healing materials have high self-healing efficiency and simple repair methods, but are limited by the number of repairs and repair defects; intrinsic self-healing materials mainly rely on the covalent and non-covalent bonds of the material itself to achieve repeatable and highly stable self-healing, but the self-healing efficiency and speed of intrinsic self-healing materials need to be improved with the help of external stimulation.
[0003] Plantain resources have a long history of application in my country. The stems and leaves of plantain have become important Chinese herbal medicine resources because of their expectorant, antitussive, diuretic and dampness-removing effects. Plantain seeds (especially plantain seed coats) contain a large amount of branched arabinoxylan, which has been widely used in the food field as dietary fiber. At present, there are no reports on the use of plantain to prepare self-healing conductive ion hydrogels. Summary of the invention
[0004] Purpose of the invention: In view of the deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a method for preparing a self-healing conductive ion hydrogel.
[0005] Technical solution: In order to solve the above technical problems, the present invention provides a method for preparing a self-healing conductive ion hydrogel, comprising the following steps:
[0006] (1) crushing, purifying, filtering, centrifuging the filtrate to generate a colloid, washing the colloid thoroughly until it is free of impurities, and then freeze-drying to obtain a psyllium husk polysaccharide powder;
[0007] (2) fully mixing the psyllium husk polysaccharide powder and the electrolyte solution to obtain a psyllium husk polysaccharide conductive ion hydrogel precursor solution;
[0008] (3) Centrifuging the psyllium husk polysaccharide conductive ion hydrogel precursor solution and discarding the supernatant to obtain the self-repairing psyllium husk polysaccharide conductive ion hydrogel.
[0009] Furthermore, the psyllium husk material includes large-leaf psyllium husk or ovate-leaf psyllium husk.
[0010] Furthermore, the weight average molecular weight of the psyllium husk polysaccharide conductive ion hydrogel is 2.46×10 6 Da, the number average molecular mass is 6.83×10 5 Da.
[0011] Furthermore, the purification method in step (1) is hot water extraction, the extraction temperature is 30 to 80° C., and the extraction time is 2 to 48 hours.
[0012] Furthermore, the centrifugation condition in step (1) is 3000-10000×g, and the centrifugation time is 5-60 min.
[0013] Furthermore, the electrolyte solution in step (2) is one or more of LiCl, LiBr, and NaCl, the ion concentration of the electrolyte solution is 0.1% to 5%, and the solid-liquid ratio of the psyllium chitosan powder to the electrolyte solution is 1:20 to 1:500.
[0014] Furthermore, the electrolyte solution in step (2) is LiCl, LiBr or a combination of the two, the electrolyte solution ion concentration is 1% to 5%, and the solid-liquid ratio of the psyllium chitosan powder to the electrolyte solution is 1:20 to 1:300.
[0015] Furthermore, the electrolyte solution described in step (2) is LiCl and LiBr, and the mass ratio of LiCl to LiBr is 30:70 to 70:30.
[0016] Furthermore, the centrifugation condition in step (3) is 5000-12000×g, and the centrifugation time is 5-15 min.
[0017] The present invention also provides a self-repairing conductive ion hydrogel obtained based on the above preparation method.
[0018] Furthermore, the conductivity of the self-healing conductive ion hydrogel is 0.85 to 50 mS / cm.
[0019] Furthermore, the conductivity of the self-healing conductive ion hydrogel is 5 to 50 mS / cm.
[0020] Furthermore, the conductivity detection method of the self-healing conductive ion hydrogel is:
[0021] The self-healing conductive ion hydrogel was cut into gel discs with a diameter of 8 mm and a thickness of 5 mm using a punching machine. Then, a stainless steel disc with a diameter of 8 mm was used as the working electrode and assembled into a button battery (CR2032) with the ion hydrogel disc. The electrochemical impedance spectroscopy was used to measure the open circuit voltage in the range of 1 to 10 5 The bulk resistance of the sample was measured at 0.01 V and the ionic conductivity of the ion conductive gel was calculated using the following formula.
[0022]
[0023] Where: σ is the conductivity of the sample, mS / cm;
[0024] L is the thickness of the sample, cm;
[0025] R is the bulk resistance of the sample obtained from the Nyquist plot, Ω;
[0026] S is the area of the stainless steel electrode, cm 2 ;
[0027] 1000 is the conversion factor between S / cm and mS / cm.
[0028] The present invention also provides a self-repairing method for the self-repairing conductive ion hydrogel obtained based on the above preparation method, adding an electrolyte solution to the self-repairing psyllium chitin polysaccharide conductive ion hydrogel prepared by the above method, fully mixing, and centrifuging to obtain the self-repairing psyllium chitin polysaccharide conductive ion hydrogel; the volume ratio of the supplemented electrolyte solution to the hydrogel is 1:20 to 1:100.
[0029] Furthermore, the centrifugation condition is 5000-12000×g, and the centrifugation time is 5-15 min.
[0030] The present application found in the process of studying psyllium husk polysaccharide that psyllium husk polysaccharide can form a hydrogel structure with the help of intramolecular / intermolecular hydrogen bonds, covalent bonds and entanglement between arabinoxylan chains, and exhibits slow self-repairing properties. Moreover, under the auxiliary effect of centrifugal force, the intramolecular / intermolecular hydrogen bonds and chain entanglements of psyllium husk polysaccharide are rapidly formed, and the self-repairing efficiency of psyllium husk polysaccharide hydrogel is significantly improved, and the structure of the hydrogel before and after self-repair remains highly consistent and repeatedly repeatable. Based on the above characteristics of psyllium husk polysaccharide, the present application proposes to use psyllium husk polysaccharide as a self-repairing hydrogel matrix structure, supplemented by ionic electrolyte solutions such as LiCl, LiBr, and NaCl, while giving the psyllium husk polysaccharide hydrogel conductivity, it will not affect the self-repairing properties of the psyllium husk polysaccharide hydrogel.
[0031] Beneficial effects: Compared with the prior art, the present invention has the following outstanding and significant advantages: The preparation method provided by the present invention uses Plantago asiatica husk as a raw material, mixes and compounds it with an electrolyte solution, and prepares a self-healing conductive ion hydrogel with the aid of centrifugal force. This preparation method breaks through the limitation that the natural polymer hydrogel relies on hydrogen bonds, covalent bonds, and inter-chain entanglements and other intramolecular / inter-molecular effects for self-healing with low efficiency. The prepared self-healing conductive ion hydrogel is completely broken after mixing with the electrolyte solution, and then centrifuged to achieve efficient and rapid self-healing of the conductive ion hydrogel. And the difference in conductivity before and after self-repair is small, and the stability is strong. The preparation method provided by the present invention not only provides a new idea for the high-value-added development of the whole plant resources of Plantago asiatica, but also effectively solves the limitations of the self-healing hydrogel, such as low self-healing efficiency, biocompatibility, biodegradability and poor conductivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 These are pictures of the self-healing conductive ion hydrogel prepared by the present invention before and after self-healing. DETAILED DESCRIPTION
[0033] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.
[0034] The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0035] The present invention is further described in detail below in conjunction with specific embodiments. The embodiments will help to understand the present invention, but the protection scope of the present invention is not limited to the following embodiments.
[0036] Example 1 Effect of different centrifugal forces on the preparation of plantago asiatica polysaccharide conductive ion hydrogel
[0037] (1) The psyllium husk was mechanically crushed to less than 100 mesh, 1.0 g of psyllium husk powder was weighed and mixed with 100 mL of distilled water, extracted in 50°C hot water for 12 h, filtered and the filtrate was collected, centrifuged at a centrifugal force of 10,000 × g for 5 min, and the colloid was collected. The colloid was fully washed with deionized water, and impurities in the colloid were removed after centrifugation. The washing was repeated 3 times, and the washed colloid was freeze-dried to obtain a psyllium husk polysaccharide powder sample. The weight average relative molecular mass of the psyllium husk polysaccharide was determined by gel permeation chromatography to be 2.46 × 10 6 Da, the number average molecular mass is 6.83×10 5 Da.
[0038] (2) Accurately weigh 0.5 g of psyllium husk polysaccharide powder sample, add 50 mL of NaCl solution with a mass concentration of 1%, and the solid-liquid ratio of the system is 1:100. The blade speed of the IKA high-speed disperser is 5000 rpm, and the mixture is fully sheared for 10 minutes. After standing and degassing, the psyllium husk polysaccharide conductive ion hydrogel precursor solution is obtained.
[0039] (3) The psyllium husk polysaccharide conductive ion hydrogel precursor solution was centrifuged at a centrifugal force of 5000, 6000, 7000, 8000, 9000, 10000, 11000, and 12000 × g for 5 min, respectively, and the colloid at the bottom was collected, which was the psyllium husk polysaccharide conductive ion hydrogel, and was recorded as G7000, G8000, G9000, G1000, G11000, and G12000, respectively.
[0040] (4) After wiping clean the liquid on the surface of the conductive ion hydrogel, the volume difference method was used to determine the volume of the psyllium chitosan conductive ion hydrogel under different centrifugal forces, and the volume of the removed supernatant was calculated, which were 23.1, 26.3, 29.3, 31.4, 33.9, 34.5, 34.6, and 34.6 mL, respectively. In addition, the electrochemical impedance spectroscopy method was used to determine the conductivity of the conductive ion gel.
[0041] (5) After the psyllium seed husk polysaccharide conductive ion hydrogel was chopped with a knife, 23.1, 26.3, 29.3, 31.4, 33.9, 34.5, 34.6, and 34.6 mL of 1% NaCl solution were added again, and then placed in an IKA high-speed disperser with a knife head speed of 8000 rpm, and fully sheared for 10 minutes. The mixed solution was then centrifuged at a centrifugal force of 10000×g for 5 minutes, and the bottom colloid was collected. The volume and conductivity of the psyllium seed husk polysaccharide conductive ion hydrogel after centrifugal force assisted self-repair were measured.
[0042] The shape of the psyllium husk polysaccharide conductive hydrogel mainly depends on the shape of the centrifuge tube. In this experiment, a round-bottom centrifuge tube is mainly used for centrifugation, so the prepared hydrogel is mainly a cylindrical structure. The shape of the hydrogel can also be changed by cutting as needed. In addition, the effect of centrifugal force on the volume and conductivity of the psyllium husk polysaccharide conductive hydrogel and the volume and conductivity of the conductive hydrogel before and after self-repair are studied, and the results are shown in Table 1.
[0043] Table 1
[0044]
[0045] With the increase of centrifugal force, the volume of the Psyllium husk polysaccharide conductive hydrogel showed a trend of first decreasing and then remaining unchanged. When the centrifugal force was 10000×g, the volume of the Psyllium husk polysaccharide conductive hydrogel was 15.5cm 3, further increasing the centrifugal force has a weak effect on the volume of the psyllium husk polysaccharide conductive hydrogel. In addition, the conductivity of the psyllium husk polysaccharide conductive hydrogel is less affected by the centrifugal force, which may be closely related to the salt concentration in the electrolyte solution, but has nothing to do with the volume and shape of the psyllium husk polysaccharide conductive hydrogel.
[0046] By comparing the volume change and conductivity change of the psyllium husk polysaccharide conductive ion hydrogel before and after self-repair under different centrifugal forces, it was found that after the psyllium husk polysaccharide conductive ion hydrogel was completely destroyed by the shearing machine, under the action of centrifugal force, the psyllium husk polysaccharide showed excellent self-repair performance. When the centrifugal force reached 7000×g or more, the volume of the psyllium husk polysaccharide remained stable before and after self-repair. In addition, the conductivity of the psyllium husk polysaccharide conductive ion hydrogel before and after self-repair changed little, which fully reflected the conductive stability of the conductive ion hydrogel before and after repair.
[0047] Example 2 Effect of solid-liquid ratio on centrifugal force-assisted self-healing properties of plantago asiatica polysaccharide conductive ion hydrogel
[0048] (1) Accurately weigh 1.0 g of psyllium husk polysaccharide powder sample, add 20, 50, 100, 200, 300, 400, 500 mL of LiCl solution with a mass concentration of 1.5%, and control the solid-liquid ratio of the system to be 1:20, 1:50, 1:100, 1:200, 1:300, 1:400, 1:500, respectively. In an IKA high-speed disperser, the blade speed is 5000 rpm, and the mixture is fully sheared for 10 min. After standing and degassing, the psyllium husk polysaccharide conductive ion hydrogel precursor solutions are obtained, which are respectively recorded as GY20, GY50, GY100, GY200, GY300, GY400, and GY500.
[0049] (2) The psyllium husk polysaccharide conductive ion hydrogel precursor solution was centrifuged at a centrifugal force of 10,000×g for 15 min, the bottom colloid was collected as the psyllium husk polysaccharide conductive ion hydrogel, and the volume of the upper layer liquid was accurately measured. In addition, the volume and conductivity of the psyllium husk polysaccharide conductive ion hydrogel were measured.
[0050] (3) After the psyllium husk polysaccharide conductive ion hydrogel was chopped with a knife, 35.7, 35.6, 35.2, 33.4, 31.3, 29.9, and 21.1 mL of LiCl solution with a mass concentration of 1.5% were re-added, and then placed in an IKA high-speed disperser with a knife head speed of 10,000 rpm. The mixed solution was fully sheared for 10 minutes, and then centrifuged at a centrifugal force of 10,000 × g for 15 minutes. The bottom colloid was collected and recorded as GY20-1, GY50-1, GY100-1, GY200-1, GY300-1, GY400-1, and GY500-1, respectively. The volume and conductivity of the psyllium husk polysaccharide conductive ion hydrogel after centrifugal force assisted self-repair were measured.
[0051] Table 2
[0052]
[0053]
[0054] As shown in Table 2, when the solid-liquid ratio of the system is in the range of 1:20-1:300, the volume and conductivity of the psyllium husk polysaccharide conductive ion hydrogel under the action of centrifugal force maintain good stability before and after repair. When the solid-liquid ratio is further reduced to 1:300-1:500, the volume of the psyllium husk polysaccharide conductive hydrogel before and after self-repair increases significantly. When the solid-liquid ratio is 1:500, the viscosity of the psyllium husk polysaccharide conductive hydrogel decreases significantly, and a hydrogel structure with good mechanical properties cannot be formed. In addition, the solid-liquid ratio of the system has little effect on the conductivity of the psyllium husk polysaccharide conductive hydrogel.
[0055] Example 3 Effects of different electrolyte concentrations on the centrifugal force-assisted self-healing properties of psyllium husk polysaccharide conductive ion hydrogel
[0056] (1) Accurately weigh 1.0 g of psyllium husk polysaccharide powder sample, add 100 mL of LiBr solution with mass concentrations of 0.1%, 1%, 2%, 3%, 4%, and 5%, and control the solid-liquid ratio of the system to be 1:100, respectively. In an IKA high-speed disperser, the blade speed is 5000 rpm, and the mixture is fully sheared for 10 min. After standing and degassing, the psyllium husk polysaccharide conductive ion hydrogel precursor solution is obtained, which is recorded as ND0.1%, ND1%, ND2%, ND3%, ND4%, and ND5%, respectively.
[0057] (2) The psyllium husk polysaccharide conductive ion hydrogel precursor solution was centrifuged at a centrifugal force of 10,000×g for 5 minutes, the bottom colloid was collected as the psyllium husk polysaccharide conductive ion hydrogel, and the volume of the upper layer liquid was accurately measured. In addition, the volume and conductivity of the psyllium husk polysaccharide conductive ion hydrogel were measured.
[0058] (3) After the psyllium husk polysaccharide conductive ion hydrogel was chopped with a knife, 34.7, 34.9, 34.5, 34.6, 34.7, 34.7, 34.7, 34.1, 34.6, 34.7, 34.7, 34.2, and 34.9 mL of LiBr solution with mass concentrations of 0.1%, 1%, 2%, 3%, 4%, and 5% were added respectively, and then placed in an IKA high-speed disperser with a knife head speed of 10000 rpm, and fully sheared for 10 minutes. Then the mixed solution was centrifuged at a centrifugal force of 10000×g for 5 minutes, and the bottom colloid was collected and recorded as ND0.1%-1, ND1%-1, ND2%-1, ND3%-1, ND4%-1, and ND5%-1, respectively. The volume and conductivity of the psyllium husk polysaccharide conductive ion hydrogel after centrifugal force assisted self-repair were measured.
[0059] Table 3
[0060]
[0061]
[0062] As shown in Table 3, the volume change of the psyllium husk polysaccharide conductive ion hydrogel before and after self-repair is less affected by the mass concentration of LiBr, and mainly depends on the solid-liquid ratio of the psyllium husk polysaccharide conductive ion hydrogel precursor solution. In addition, as the mass concentration of LiBr increases from 0.1% to 5%, the conductivity of the psyllium husk polysaccharide conductive hydrogel gradually increases. When the mass concentration of LiBr is 0.1%, the conductivity of the psyllium husk polysaccharide conductive hydrogel before and after centrifugal force-assisted self-repair is close to the conductivity of tap water, which are 0.45mS / cm and 0.40mS / cm, respectively.
[0063] Example 4 Effects of different electrolytes on the centrifugal force-assisted self-healing properties of psyllium husk polysaccharide conductive ion hydrogel
[0064] (1) Accurately weigh 1.0 g of psyllium husk polysaccharide powder sample, 50 mL of LiCl, LiBr, NaCl and electrolyte solutions with different LiCl:LiBr addition ratios (mass ratios of 30:70, 40:60, 50:50, 60:40, and 70:30, respectively), the mass concentration (w / v) of the electrolyte in the electrolyte solution was controlled at 5%, and the solid-liquid ratio of the control system was 1:50. The blade speed of the IKA high-speed disperser was 5000 rpm, and the mixture was fully sheared for 10 min. After standing and degassing, the psyllium husk polysaccharide conductive ion hydrogel precursor solution was obtained, which was recorded as LiCl, LiBr, NaCl, LiCl:LiBr, respectively. 30:70 、LiCl:LiBr 40:60 、LiCl:LiBr 50:50 、LiCl:LiBr 60:40、LiCl:LiBr 70:30 .
[0065] (2) The psyllium husk polysaccharide conductive ion hydrogel precursor solution was centrifuged at a centrifugal force of 12000×g for 5 min, and the bottom colloid was collected as the psyllium husk polysaccharide conductive ion hydrogel, and the volume of the upper layer liquid was accurately measured, which was 12.3, 13.2, 15.6, 12.7, 12.9, 12.6, 12.3, and 12.4 mL, respectively. In addition, the volume and conductivity of the psyllium husk polysaccharide conductive ion hydrogel were measured.
[0066] (3) After the psyllium chitosan polysaccharide conductive ion hydrogel was chopped with a knife, 12.3, 13.2, 15.6, 12.7, 12.9, 12.6, 12.3, and 12.4 mL of electrolyte solutions with a mass concentration of 5% LiCl, LiBr, and NaCl and different LiCl and LiBr addition ratios (mass ratios of 30:70, 40:60, 50:50, 60:40, and 70:30, respectively) were added, and then placed in an IKA high-speed disperser with a knife head speed of 10,000 rpm, fully sheared for 10 minutes, and then the mixed solution was centrifuged at a centrifugal force of 10,000×g for 5 minutes, and the bottom colloid was collected and recorded as Y LiCl , Y LiBr , Y NaCl , Y LiCl:LiBr30:70 , Y LiCl:LiBr40:60 , Y LiCl:LiBr50:50 , Y LiCl:LiBr60:40 , Y LiCl:LiBr70:30 , the volume and conductivity of the psyllium husk polysaccharide conductive ion hydrogel after centrifugal force-assisted self-repair were determined.
[0067] Table 4
[0068]
[0069] It can be seen from Table 4 that at the same electrolyte concentration, the type and proportion of salt in the electrolyte have a greater impact on the stability of the volume and conductivity of the psyllium husk polysaccharide conductive ion hydrogel before and after repair. Compared with NaCl electrolyte solution, LiCl and LiBr and different ratios of the two are more conducive to the preparation of high conductivity and high self-healing psyllium husk polysaccharide conductive hydrogel.
Claims
1. A method for preparing a self-healing conductive ion hydrogel, It is characterized in that The following steps are involved: (1) crushing, purifying, filtering, centrifuging the filtrate to generate a colloid, washing the colloid thoroughly until it is free of impurities, and then freeze-drying to obtain a psyllium husk polysaccharide powder; (2) fully mixing the psyllium husk polysaccharide powder and the electrolyte solution to obtain a psyllium husk polysaccharide conductive ion hydrogel precursor solution; The electrolyte solution is one or more of LiCl or LiBr, the electrolyte solution ion concentration is 5%, and the solid-liquid ratio of the psyllium chitosan powder to the electrolyte solution is 1:20 to 1:400; when the electrolyte solution is LiCl and LiBr, the mass ratio of LiCl to LiBr is 30:70 to 70:30; (3) Centrifuging the psyllium husk polysaccharide conductive ion hydrogel precursor solution and discarding the supernatant to obtain the self-repairing psyllium husk polysaccharide conductive ion hydrogel.
2. The preparation method according to claim 1, It is characterized in that The purification method in step (1) is hot water extraction, the extraction temperature is 30 to 80° C., and the extraction time is 2 to 48 h.
3. The preparation method according to claim 1, It is characterized in that The centrifugation conditions in step (1) are 3000-10000×g, and the centrifugation time is 5-60 min.
4. The preparation method according to claim 1, It is characterized in that The centrifugation conditions described in step (3) are 5000-12000×g and the centrifugation time is 5-15 min.
5. A self-healing conductive ion hydrogel obtained by the preparation method according to any one of claims 1 to 4.
6. The self-healing conductive ion hydrogel according to claim 5, It is characterized in that The conductivity of the self-healing conductive ion hydrogel is 0.85-50 mS / cm.
7. A self-repairing method for a self-repairing conductive ion hydrogel obtained by the preparation method of claim 1, It is characterized in that Add electrolyte solution to the self-repairing psyllium husk polysaccharide conductive ion hydrogel prepared in claim 1, mix thoroughly, and centrifuge to obtain the self-repairing psyllium husk polysaccharide conductive ion hydrogel; the volume ratio of the supplemented electrolyte solution to the hydrogel is 1:20 to 1:
100.