A method for treating dyed textiles

By applying silica gel coatings prepared by ethanol, polyvinylpyrrolidone and tetraethyl orthosilicate on dyed textiles, the problem of insufficient sun fastness in dyed textiles is solved, and efficient color fastness improvement is achieved , and avoid the risk of pollution of metal mock agents, and the process is simple and environmentally friendly.

CN115948925BActive Publication Date: 2024-11-15WUHAN TEXTILE UNIV +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310060782.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-17
Publication Date
2024-11-15
Estimated Expiration
2043-01-17

AI Technical Summary

Technical Problem

Traditional natural plant dyed textiles have insufficient sun fastness, and the use of metal mottled agents leads to environmental pollution and human safety threats.

Method used

The silica gel coating is prepared by solvents such as ethanol, polyvinylpyrrolidone and tetraethyl orthosilicate. It is applied to dyed textiles by impregnation to enhance the adhesion and elution resistance of the dye.

Benefits of technology

It effectively improves the sun fastness, water-resistant color fastness and friction color fastness of natural plant dyed textiles, avoids environmental pollution and human safety risks caused by metal mottled agents, and is simple in the process and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004061195400000121
    Figure BDA0004061195400000121
  • Figure BDA0004061195400000131
    Figure BDA0004061195400000131
Patent Text Reader

Abstract

The present invention relates to the field of textiles, and discloses a processing method for dyed textiles, the processing method comprising: (1) mixing ethanol with polyvinyl pyrrolidone to obtain a polyvinyl pyrrolidone-ethanol solution; (2) immersing the dyed textile in the polyvinyl pyrrolidone-ethanol solution, then squeezing out excess solution, and drying to obtain the pretreated textile; (3) mixing ethanol with tetraethyl orthosilicate to obtain tetraethyl orthosilicate-ethanol solution, mixing ethanol with ammonia water to obtain an ammonia water-ethanol mixed solution, dripping the ammonia water-ethanol mixed solution into the tetraethyl orthosilicate solution, and then stirring to obtain a silica gel mixed solution; (4) immersing the pretreated textile in the silica gel mixed solution, stirring, then squeezing out excess solution, and then drying. This method can improve the light fastness, washing color fastness and rubbing color fastness of natural plant dye-dyed fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of textiles, and in particular to a method for treating dyed textiles. Background Art

[0002] The textile printing and dyeing industry is the main industry that produces environmental pollution. As people pay more and more attention to environmental protection issues, they advocate the production concept of green environmental protection and sustainable development. Consumers' requirements for textiles have gradually shifted from the basic requirements of practicality and aesthetics of textiles to the safety and environmental protection of textiles. Therefore, textiles dyed with natural plant dyes and natural fibers have been favored by consumers. Natural fibers include cotton, linen, wool, silk and other fibers. Natural fiber textiles dyed with natural plant dyes have gradually become popular because of their natural degradation properties and their non-toxic, harmless and environmentally friendly properties. Traditional natural plant dyes dye natural fibers. Due to the poor fixation fastness of natural plant dyes to fibers, metal mordants need to be added for complexation, which improves the fixation fastness of natural plant dyes dyed textiles and obtains better color fastness to washing and rubbing, but its light fastness has not been improved. Due to the addition of metal mordants, metal ions are contained in the dyeing wastewater, which makes it possible to potentially pollute the environment. In addition, the complexation of metal ions with natural plant dyes and fibers causes the metal content in textiles to exceed the standard, which also poses a potential threat to human safety. Therefore, it is necessary to develop a new mordant-free finishing process to improve the color fastness of textiles dyed with natural plant dyes, while solving the potential environmental pollution and human safety caused by metal mordants. Summary of the invention

[0003] The purpose of the invention is to overcome the problem of poor color fastness of textiles dyed with natural plant dyes in the prior art, and to provide a method for treating dyed textiles, wherein the method can improve the color fastness to sunlight, color fastness to washing and color fastness to rubbing of the textiles dyed with natural plant dyes.

[0004] In order to achieve the above object, the present invention provides a method for treating dyed textiles, the method comprising the following steps:

[0005] (1) mixing ethanol and polyvinyl pyrrolidone to obtain a polyvinyl pyrrolidone-ethanol solution;

[0006] (2) immersing the dyed textile in the polyvinyl pyrrolidone-ethanol solution, squeezing out excess solution, and then drying to obtain a pretreated textile;

[0007] (3) mixing ethanol and tetraethyl orthosilicate to obtain a tetraethyl orthosilicate-ethanol solution, mixing ethanol and ammonia water to obtain an ammonia water-ethanol mixed solution, and then dropping the ammonia water-ethanol mixed solution into the tetraethyl orthosilicate solution, followed by stirring to obtain a silica gel mixed solution;

[0008] (4) Immersing the pretreated textile in the silica gel mixed solution, stirring, squeezing out excess solution, and then air-drying.

[0009] Preferably, in step (1), the average molecular weight of the polyvinyl pyrrolidone is ≥ 1,200,000.

[0010] Preferably, the solid-liquid ratio of the polyvinyl pyrrolidone to the ethanol is 2-3 g / L.

[0011] Preferably, in step (2), the method for preparing the dyed textile comprises: immersing the textile in a natural plant dye solution, dyeing at 80-98° C. for 50-70 min, and then air-drying.

[0012] Preferably, the amount of the natural plant dye in the natural plant dye solution is 8-11% owf.

[0013] Preferably, the bath ratio of the natural plant dye solution to the textile is 15-30:1.

[0014] Preferably, the natural plant dye is selected from one or more of gardenia yellow, gardenia red, gardenia blue, turmeric, sodium copper chlorophyllin and alizarin red.

[0015] Preferably, the natural plant dye is sodium copper chlorophyllin.

[0016] Preferably, the textile is pure cotton knitted fabric.

[0017] Preferably, in step (2), the immersion time is 2-5 minutes.

[0018] Preferably, after squeezing out excess solution, the liquid carrying rate of the dyed textile is controlled to be 40-60%.

[0019] Preferably, in step (3), the volume ratio of tetraethyl orthosilicate to ethanol is 10-30:100.

[0020] Preferably, the volume ratio of the aqueous ammonia to the ethanol is 5-30:100.

[0021] Preferably, in step (3), the dropping speed is 0.2-0.5 mL / s.

[0022] Preferably, in step (3), the stirring conditions include: a speed of 1000-1400 rpm and a time of 4-8 min.

[0023] Preferably, in step (4), the stirring conditions include: a speed of 1000-1400 rpm and a time of 150-190 min.

[0024] Preferably, after squeezing out excess solution, the liquid carrying rate of the pretreated textile is controlled to be 80-150%.

[0025] Since the dense silica coating has a protective effect on the dye fixed on the textile, it can weaken the photosensitivity reaction of the dye under the illumination condition, reduce the contact between the dye molecules on the fiber and the active oxygen, and thus protect the dye from being oxidized; and the silica coating has a certain hydrophobicity, which can prevent the dye fixed on the fiber from being dissolved in water and eluted in large quantities in the subsequent washing process to a certain extent. Therefore, the silica coating is prepared by the sol-gel method, which can effectively improve the light fastness, washing fastness and rubbing fastness of the dye on the textile fiber. Due to the poor binding force between silica and the fiber, before the silica coating treatment, the polyvinyl pyrrolidone treatment of the dyed material is first completed by the immersion method. Polyvinyl pyrrolidone is a non-ionic polymer compound, which not only has excellent physiological compatibility and safety, but also has good adhesion, which can make the silica coating more firmly attached to the fiber surface. In addition, the polyvinyl pyrrolidone and silica adsorbed on the dyed textile will not affect the color of the textile. In addition, the method is simple and effective in process and environmentally friendly. DETAILED DESCRIPTION

[0026] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0027] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0028] The present invention provides a method for treating dyed textiles, the method comprising the following steps:

[0029] (1) mixing ethanol and polyvinyl pyrrolidone to obtain a polyvinyl pyrrolidone-ethanol solution;

[0030] (2) immersing the dyed textile in the polyvinyl pyrrolidone-ethanol solution, squeezing out excess solution, and then drying to obtain a pretreated textile;

[0031] (3) mixing ethanol and tetraethyl orthosilicate to obtain a tetraethyl orthosilicate-ethanol solution, mixing ethanol and ammonia water to obtain an ammonia water-ethanol mixed solution, and then dropping the ammonia water-ethanol mixed solution into the tetraethyl orthosilicate solution, followed by stirring to obtain a silica gel mixed solution;

[0032] (4) Immersing the pretreated textile in the silica gel mixed solution, stirring, squeezing out excess solution, and then air-drying.

[0033] Preferably, in step (1), the average molecular weight of the polyvinyl pyrrolidone is ≥ 1200000. The average molecular weight of the polyvinyl pyrrolidone used is relatively large, so that the polyvinyl pyrrolidone-ethanol solution has good viscosity and can form a film on the surface of the fabric.

[0034] In an excellent embodiment, in step (1), the average molecular weight of the polyvinyl pyrrolidone is 1,300,000.

[0035] In a preferred embodiment, in step (1), the solid-to-liquid ratio of the polyvinyl pyrrolidone to the ethanol is 2-3 g / L, specifically 2 g / L, 2.1 g / L, 2.2 g / L, 2.3 g / L, 2.4 g / L, 2.5 g / L, 2.6 g / L, 2.7 g / L, 2.8 g / L, 2.9 g / L or 3 g / L.

[0036] Preferably, in step (2), the method for preparing the dyed textile comprises: immersing the textile in a natural plant dye solution, dyeing at 80-98° C. for 50-70 min, and then air-drying.

[0037] In a specific embodiment, in step (1), the dyeing temperature can be 80°C, 83°C, 86°C, 89°C, 92°C, 95°C or 98°C, and the dyeing time can be 50 min, 55 min, 60 min, 65 min or 70 min.

[0038] In the present invention, the amount of the natural plant dye in the natural plant dye solution is 8-11% owf, specifically 8% owf, 9% owf, 10% owf or 11% owf.

[0039] In the present invention, the bath ratio of the natural plant dye solution to the textile is 15-30:1, specifically 15:1, 18:1, 21:1, 24:1, 27:1 or 30:1.

[0040] In the present invention, the bath ratio refers to the ratio of the volume (mL) of the natural plant dye solution to the weight (g) of the textile.

[0041] Preferably, the natural plant dye is selected from one or more of gardenia yellow, gardenia red, gardenia blue, turmeric, sodium copper chlorophyllin and alizarin red, and more preferably sodium copper chlorophyllin.

[0042] In the present invention, the textile is selected from loose fibers, yarns or fabrics containing one or more components of cotton, linen, wool and silk.

[0043] Preferably, the textile is selected from cellulose fiber fabrics, and more preferably pure cotton knitted fabrics.

[0044] In a more preferred embodiment, in step (1), in order to fully dissolve polyvinyl pyrrolidone, the specific operation steps of mixing ethanol and polyvinyl pyrrolidone include: adding polyvinyl pyrrolidone to ethanol, and then shaking at 50-70°C for 20-40 minutes.

[0045] In a specific embodiment, the oscillation temperature can be 50°C, 55°C, 60°C, 65°C or 70°C, and the oscillation time can be 20 min, 25 min, 30 min, 35 min or 40 min.

[0046] Preferably, in step (2), the immersion time is 2-5 min, specifically 2 min, 3 min, 4 min or 5 min.

[0047] Preferably, in step (2), after squeezing out excess solution, the liquid carrying rate of the dyed textile is controlled to be 40-60%, specifically 40%, 45%, 50%, 55% or 60%.

[0048] Preferably, in step (3), the volume ratio of tetraethyl orthosilicate to ethanol is 10-30:100, specifically 10:100, 15:100, 20:100, 25:100 or 30:100.

[0049] In a preferred embodiment, in step (3), the volume ratio of tetraethyl orthosilicate to ethanol is 20:100.

[0050] Preferably, in step (3), the volume ratio of the aqueous ammonia to the ethanol is 5-30:100, specifically 5:100, 10:100, 15:100, 20:100, 25:100 or 30:100.

[0051] In a preferred embodiment, in step (3), the volume ratio of the aqueous ammonia to the ethanol is 20:100.

[0052] Preferably, in step (3), the dropping speed is 0.2-0.5 mL / s, specifically 0.2 mL / s, 0.3 mL / s, 0.4 mL / s or 0.5 mL / s.

[0053] Preferably, in step (3), the stirring conditions include: a speed of 1000-1400 rpm and a time of 4-8 min. Specifically, the speed may be 1000 rpm, 1100 rpm, 1200 rpm, 1300 rpm or 1400 rpm, and the time may be 4 min, 5 min, 6 min, 7 min or 8 min.

[0054] In step (4) of the present invention, during the stirring process, the silicon dioxide nanoparticles formed by the hydrolysis of tetraethyl orthosilicate under weak alkaline conditions can gradually adhere to the surface of the fabric fibers.

[0055] Therefore, in a preferred case, in order to obtain a better treatment effect, in step (4), the stirring conditions include: a speed of 1000-1400 rpm, and a time of 150-190 min. Specifically, the speed can be 1000 rpm, 1100 rpm, 1200 rpm, 1300 rpm or 1400 rpm, and the time can be 150 min, 160 min, 170 min, 180 min or 190 min.

[0056] In step (4) of the present invention, after squeezing out excess solution, the liquid carrying rate of the pretreated textile is controlled to be 80-150%, specifically 80%, 90%, 100%, 110%, 120%, 130%, 140% or 150%.

[0057] In a preferred embodiment, in step (4), after squeezing out excess solution, the liquid carrying rate of the pretreated textile is controlled to be 100%.

[0058] In step (4) of the present invention, after the drying is completed, the textile obtained after the drying is rinsed and then continued to be dried.

[0059] In the present invention, the rinsing refers to rinsing the finished fabric with water or ethanol to remove excess finishing agent floating on the surface of the fabric.

[0060] Preferably, ethanol is used for rinsing, and the number of rinsing is two times.

[0061] Preferably, the operations of steps (2), (3) and (4) of the present invention are all carried out at room temperature.

[0062] In the present invention, the normal temperature refers to 20-30°C, and preferably, the normal temperature is 25°C.

[0063] Since the dense silica coating has a protective effect on the dye fixed on the fabric, it can weaken the photosensitivity reaction of the dye under illumination conditions, reduce the contact between the dye molecules on the fiber and the active oxygen, and thus protect the dye from being oxidized; and the silica coating has a certain hydrophobicity, which can prevent the dye fixed on the fiber from being dissolved in water and eluted in large quantities during the subsequent washing process. Therefore, the silica coating is prepared by the sol-gel method, which can effectively improve the light fastness, washing color fastness and rubbing color fastness of the dye on the cellulose fiber. Due to the poor bonding between silica and the fiber, before the silica coating treatment, the treatment of the dyed material with polyvinyl pyrrolidone is first completed by the immersion method. Polyvinyl pyrrolidone is a non-ionic polymer compound, which not only has excellent physiological compatibility and safety, but also has good adhesion. In this scheme, the silica coating can be more firmly attached to the fiber surface.

[0064] The advantages of this method are: the PVP@SiO2 coating attached to the surface of the dye can weaken the photosensitivity of the dye after being exposed to light, thereby protecting the dye from oxidation. At the same time, the presence of the inorganic silica coating enhances the hydrophobicity of the surface of the dye, which can prevent the dye from being washed away due to being dissolved in water in large quantities during the subsequent washing process. In summary, the coating effectively improves the light fastness, water washing color fastness and rubbing color fastness of fibers dyed with natural plant dyes. In addition, the polyvinyl pyrrolidone and silica adsorbed on the dyed textiles will not affect the color of the textiles. In addition, the process of this method is simple and effective, does not require the addition of mordant, and is environmentally friendly.

[0065] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto.

[0066] The average molecular weight of polyvinyl pyrrolidone used below is 1,300,000, and the room temperature below refers to 25°C.

[0067] Example 1

[0068] (1) mixing sodium copper chlorophyllin with water to obtain a sodium copper chlorophyllin dye solution, immersing 6 g of pure cotton knitted fabric in the sodium copper chlorophyllin dye solution, controlling the bath ratio of the sodium copper chlorophyllin dye solution to the pure cotton knitted fabric to be 20:1, and the amount of the sodium copper chlorophyllin dye in the sodium copper chlorophyllin dye solution to be 10% owf, dyeing at 95° C. for 60 minutes, taking out and drying in the dark, and obtaining a dyed pure cotton knitted fabric;

[0069] (2) adding 0.5 g of polyvinyl pyrrolidone to 250 mL of ethanol, shaking at 60° C. for 30 min, and cooling to room temperature to obtain a polyvinyl pyrrolidone-ethanol solution;

[0070] (3) immersing the dyed pure cotton knitted fabric in the polyvinyl pyrrolidone-ethanol solution for 2 minutes, then taking it out and squeezing out excess solution to control the liquid carrying rate of the dyed pure cotton knitted fabric to 40%, and then drying it in a dark place to obtain the pretreated pure cotton knitted fabric;

[0071] (4) tetraethyl orthosilicate is mixed with ethanol to obtain a tetraethyl orthosilicate-ethanol solution (the volume ratio of tetraethyl orthosilicate to ethanol is 20:100), ammonia water is mixed with ethanol to obtain an ammonia water-ethanol mixed solution (the volume ratio of ammonia water to ethanol is 20:100), and then the ammonia water-ethanol mixed solution is added dropwise to the tetraethyl orthosilicate solution at a dropping rate of 0.3 mL / s. After the dropping is completed, the mixture is stirred at a speed of 1200 rpm for 5 minutes to obtain a silica gel mixed solution;

[0072] (5) immersing the pretreated pure cotton knitted fabric in the silica gel mixed solution, stirring at a speed of 1200 rpm for 180 min, then taking it out, squeezing out excess solution, controlling the liquid carrying rate of the pretreated pure cotton knitted fabric to be 100%, drying it in a dark place, then rinsing it with ethanol twice, and then drying it in a dark place to obtain the treated dyed pure cotton knitted fabric A1;

[0073] The operations of steps (3), (4) and (5) are all carried out at room temperature.

[0074] Example 2

[0075] The operation of Example 1 was followed, except that in step (4), the volume ratio of tetraethyl orthosilicate to ethanol was 10:100, to obtain a treated dyed pure cotton knitted fabric A2.

[0076] Example 3

[0077] The operation of Example 1 was followed, except that in step (4), the volume ratio of tetraethyl orthosilicate to ethanol was 30:100, to obtain a treated dyed pure cotton knitted fabric A3.

[0078] Example 4

[0079] The method of Example 2 is followed, except that in step (4), the volume ratio of ammonia water to ethanol is 5:100, to obtain a treated dyed pure cotton knitted fabric A4.

[0080] Example 5

[0081] The method of Example 2 is followed, except that in step (4), the volume ratio of the ammonia water to the ethanol is 30:100, to obtain a treated dyed pure cotton knitted fabric A5.

[0082] Example 6

[0083] (1) mixing sodium copper chlorophyllin with water to obtain a sodium copper chlorophyllin dye solution, immersing 6 g of pure cotton knitted fabric in the sodium copper chlorophyllin dye solution, controlling the bath ratio of the sodium copper chlorophyllin dye solution to the pure cotton knitted fabric to be 15:1, and the amount of the sodium copper chlorophyllin dye in the sodium copper chlorophyllin dye solution to be 8% owf, dyeing at 90° C. for 50 minutes, taking out and drying in the dark, and obtaining a dyed pure cotton knitted fabric;

[0084] (2) adding 3 g of polyvinyl pyrrolidone to 1000 mL of ethanol, shaking at 50° C. for 40 min, and cooling to room temperature to obtain a polyvinyl pyrrolidone-ethanol solution;

[0085] (3) immersing the dyed pure cotton knitted fabric in the polyvinyl pyrrolidone-ethanol solution for 4 minutes, then taking it out and squeezing out excess solution to control the liquid carrying rate of the dyed pure cotton knitted fabric to 60%, and then drying it in a dark place to obtain the pretreated pure cotton knitted fabric;

[0086] (4) tetraethyl orthosilicate is mixed with ethanol to obtain a tetraethyl orthosilicate-ethanol solution (the volume ratio of tetraethyl orthosilicate to ethanol is 20:100), ammonia water is mixed with ethanol to obtain an ammonia water-ethanol mixed solution (the volume ratio of ammonia water to ethanol is 20:100), and then the ammonia water-ethanol mixed solution is added dropwise to the tetraethyl orthosilicate solution at a dropping rate of 0.4 mL / s. After the dropping is completed, the mixture is stirred at a speed of 1000 rpm for 8 minutes to obtain a silica gel mixed solution;

[0087] (5) immersing the pretreated pure cotton knitted fabric in the silica gel mixed solution, stirring at a speed of 1400 rpm for 150 min, then taking it out, squeezing out excess solution, controlling the liquid carrying rate of the pretreated pure cotton knitted fabric to be 90%, drying it in a dark place, then rinsing it with ethanol twice, and then drying it in a dark place to obtain the treated dyed pure cotton knitted fabric A6;

[0088] The operations of steps (3), (4) and (5) are all carried out at room temperature.

[0089] Example 7

[0090] (1) mixing sodium copper chlorophyllin with water to obtain a sodium copper chlorophyllin dye solution, immersing 6 g of pure cotton knitted fabric in the sodium copper chlorophyllin dye solution, controlling the bath ratio of the sodium copper chlorophyllin dye solution to the pure cotton knitted fabric to be 30:1, and the amount of the sodium copper chlorophyllin dye in the sodium copper chlorophyllin dye solution to be 11% owf, dyeing at 85° C. for 65 minutes, taking out and drying in the dark, and obtaining a dyed pure cotton knitted fabric;

[0091] (2) adding 0.5 g of polyvinyl pyrrolidone to 200 mL of ethanol, shaking at 70° C. for 20 min, and cooling to room temperature to obtain a polyvinyl pyrrolidone-ethanol solution;

[0092] (3) immersing the dyed pure cotton knitted fabric in the polyvinyl pyrrolidone-ethanol solution for 3 minutes, then taking it out and squeezing out excess solution to control the liquid carrying rate of the dyed pure cotton knitted fabric to 50%, and then drying it in the dark to obtain the pretreated pure cotton knitted fabric;

[0093] (4) tetraethyl orthosilicate is mixed with ethanol to obtain a tetraethyl orthosilicate-ethanol solution (the volume ratio of tetraethyl orthosilicate to ethanol is 20:100), ammonia water is mixed with ethanol to obtain an ammonia water-ethanol mixed solution (the volume ratio of ammonia water to ethanol is 20:100), and then the ammonia water-ethanol mixed solution is added dropwise to the tetraethyl orthosilicate solution at a rate of 0.5 mL / s. After the addition is completed, the mixture is stirred at a speed of 1400 rpm for 4 minutes to obtain a silica gel mixed solution;

[0094] (5) immersing the pretreated pure cotton knitted fabric in the silica gel mixed solution, stirring at a speed of 1000 rpm for 190 min, then taking it out, squeezing out excess solution, controlling the liquid carrying rate of the pretreated pure cotton knitted fabric to be 130%, drying it in a dark place, then rinsing it with ethanol twice, and then drying it in a dark place to obtain the treated dyed pure cotton knitted fabric A7;

[0095] Wherein, the operations of steps (3), (4) and (5) are all carried out at room temperature.

[0096] Blank Group

[0097] Sodium copper chlorophyllin is mixed with water to obtain a sodium copper chlorophyllin dye solution, 6 g of pure cotton knitted fabric is immersed in the sodium copper chlorophyllin dye solution, the bath ratio of the sodium copper chlorophyllin dye solution to the pure cotton knitted fabric is controlled to be 20:1, the amount of the sodium copper chlorophyllin dye in the sodium copper chlorophyllin dye solution is 10% owf, dyeing is carried out at 95°C for 60 minutes, and the fabric is taken out and dried in the dark to obtain a dyed pure cotton knitted fabric D1.

[0098] Comparative Example 1

[0099] (1) mixing sodium copper chlorophyllin with water to obtain a sodium copper chlorophyllin dye solution, immersing 6 g of pure cotton knitted fabric in the sodium copper chlorophyllin dye solution, controlling the bath ratio of the sodium copper chlorophyllin dye solution to the pure cotton knitted fabric to be 20:1, and the amount of the sodium copper chlorophyllin dye in the sodium copper chlorophyllin dye solution to be 10% owf, dyeing at 95° C. for 60 minutes, taking out and drying in the dark, and obtaining a dyed pure cotton knitted fabric;

[0100] (2) adding 0.5 g of polyvinyl pyrrolidone to 250 mL of ethanol, shaking at 60° C. for 30 min, and cooling to room temperature to obtain a polyvinyl pyrrolidone-ethanol solution;

[0101] (3) immersing the dyed pure cotton knitted fabric in the polyvinyl pyrrolidone-ethanol solution for 2 minutes, then taking it out and squeezing out excess solution to control the liquid carrying rate of the dyed pure cotton knitted fabric to 40%, then drying it in a dark place to obtain the pretreated pure cotton knitted fabric, then rinsing it with ethanol twice, then drying it in a dark place to obtain the treated dyed pure cotton knitted fabric D2;

[0102] Wherein, the operation of step (3) is carried out at room temperature.

[0103] Comparative Example 2

[0104] (1) mixing sodium copper chlorophyllin with water to obtain a sodium copper chlorophyllin dye solution, immersing 6 g of pure cotton knitted fabric in the sodium copper chlorophyllin dye solution, controlling the bath ratio of the sodium copper chlorophyllin dye solution to the pure cotton knitted fabric to be 20:1, and the amount of the sodium copper chlorophyllin dye in the sodium copper chlorophyllin dye solution to be 10% owf, dyeing at 95° C. for 60 minutes, taking out and drying in the dark, and obtaining a dyed pure cotton knitted fabric;

[0105] (2) tetraethyl orthosilicate is mixed with ethanol to obtain a tetraethyl orthosilicate-ethanol solution (the volume ratio of tetraethyl orthosilicate to ethanol is 20:100), ammonia water is mixed with ethanol to obtain an ammonia water-ethanol mixed solution (the volume ratio of ammonia water to ethanol is 20:100), and then the ammonia water-ethanol mixed solution is added dropwise to the tetraethyl orthosilicate solution at a rate of 0.3 mL / s. After the addition is completed, the mixture is stirred at a speed of 1200 rpm for 5 min to obtain a silica gel mixed solution;

[0106] (3) immersing the dyed pure cotton knitted fabric obtained in step (1) in the silica gel mixed solution, stirring at a speed of 1200 rpm for 180 min, then taking it out, squeezing out excess solution, controlling the liquid carrying rate of the dyed pure cotton knitted fabric to be 100%, drying it in a dark place, then rinsing it with ethanol twice, and then drying it in a dark place to obtain the treated dyed pure cotton knitted fabric D3;

[0107] The operations of steps (2) and (3) are both carried out at room temperature.

[0108] Test Example 1

[0109] A1-A7 and D1-D3 were tested for color fastness to washing (ISO 105C06: C2S), color fastness to rubbing (ISO105-X12) and color fastness to sunlight (ISO 105B02).

[0110] The results are shown in Table 1.

[0111] Table 1

[0112]

[0113]

[0114] It can be seen from the results in Table 1 that the treatment method of the present invention improves the light fastness, washing fastness and rubbing fastness of fibers dyed with natural plant dyes. This process is simple and effective, does not require the addition of mordant, and is environmentally friendly.

[0115] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A method for treating dyed textiles, characterized in that: The processing method comprises the following steps: (1) mixing ethanol and polyvinyl pyrrolidone to obtain a polyvinyl pyrrolidone-ethanol solution; (2) immersing the dyed textile in the polyvinyl pyrrolidone-ethanol solution, squeezing out excess solution, and then drying to obtain a pretreated textile; (3) mixing ethanol and tetraethyl orthosilicate to obtain a tetraethyl orthosilicate-ethanol solution, mixing ethanol and ammonia water to obtain an ammonia water-ethanol mixed solution, and then dropping the ammonia water-ethanol mixed solution into the tetraethyl orthosilicate-ethanol solution, followed by stirring to obtain a silica gel mixed solution; (4) immersing the pretreated textile in the silica gel mixed solution, stirring, squeezing out excess solution, and then drying; In step (2), the method for preparing the dyed textile comprises: immersing the textile in a natural plant dye solution, dyeing at 80-98° C. for 50-70 min, and then air-drying; The textile is pure cotton knitted fabric.

2. The processing method according to claim 1, characterized in that: In step (1), the average molecular weight of the polyvinyl pyrrolidone is ≥ 1,200,000.

3. The processing method according to claim 2, characterized in that: In step (1), the solid-to-liquid ratio of the polyvinyl pyrrolidone to the ethanol is 2-3 g / L.

4. The processing method according to any one of claims 1 to 3, characterized in that: In step (2), the amount of natural plant dye in the natural plant dye solution is 8-11% owf.

5. The processing method according to claim 4, characterized in that: The bath ratio of the natural plant dye solution to the textile is 15-30:

1.

6. The processing method according to claim 4, characterized in that: The natural plant dye is selected from one or more of gardenia yellow, gardenia red, gardenia blue, turmeric, sodium copper chlorophyllin and alizarin red.

7. The processing method according to claim 6, characterized in that: The natural plant dye is sodium copper chlorophyllin.

8. The processing method according to claim 1, characterized in that: In step (2), the immersion time is 2-5 minutes.

9. The processing method according to claim 8, characterized in that: In step (2), after squeezing out excess solution, the liquid carrying rate of the dyed textile is controlled to be 40-60%.

10. The processing method according to claim 1, characterized in that: In step (3), the volume ratio of tetraethyl orthosilicate to ethanol is 10-30:

100.

11. The processing method according to claim 10, characterized in that: In step (3), the volume ratio of the aqueous ammonia to the ethanol is 5-30:

100.

12. The processing method according to claim 1 or 11, characterized in that: In step (3), the dropping speed is 0.2-0.5 mL / s.

13. The processing method according to claim 1, characterized in that: In step (3), the stirring conditions include: a speed of 1000-1400 rpm and a time of 4-8 min.

14. The processing method according to claim 1, characterized in that: In step (4), the stirring conditions include: a speed of 1000-1400 rpm and a time of 150-190 min.

15. The processing method according to claim 14, characterized in that: In step (4), after squeezing out excess solution, the liquid carrying rate of the pretreated textile is controlled to be 80-150%.

Citation Information

Cited By

  • Preparation method of high-color-rendering textile composite coating and coating

    CN122039454A