A lattice carbon fiber structure battery and preparation method thereof

Through lattice-type cathode material distribution and structural resin curing treatment, the isolation problem caused by cathode material coating in carbon fiber structural batteries is solved, the mechanical and electrical properties are improved, the balance between high energy density and high mechanical properties is achieved, and the process is simplified. production process.

CN115966652BActive Publication Date: 2024-10-25SHANGHAI JIAOTONG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211706005.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-29
Publication Date
2024-10-25
Estimated Expiration
2042-12-29

AI Technical Summary

Technical Problem

The coating method of the cathode material of existing carbon fiber structural batteries leads to isolation between the structural resin and carbon fiber, resulting in a decrease in mechanical properties, and it is impossible to ensure high energy density and high mechanical properties at the same time.

Method used

The lattice cathode material distribution method is adopted, by covering the carbon fiber with an isolation film with lattice holes, and drying it at high temperature under vacuum to form a cathode material covered with lattice distribution, combined with the curing treatment of structural resin and electrolyte to ensure Anti-peeling performance and energy storage effect of carbon fiber layer.

Benefits of technology

It improves the mechanical properties and electrical properties of carbon fiber structure batteries, achieves both high energy density and high mechanical properties, simplifies the production process, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115966652B_ABST
    Figure CN115966652B_ABST
Patent Text Reader

Abstract

The present invention provides a lattice carbon fiber structure battery and a preparation method thereof, wherein the constituent materials of the lattice carbon fiber structure battery include: positive electrode carbon fiber covered with positive electrode material distributed in a lattice, an insulating fiber separator, a negative electrode carbon fiber, an electrolyte and a structural resin; the preparation method is to lay a layer of separator with periodic holes on the desizing carbon fiber, apply the positive electrode slurry on the separator, and dry at high temperature under vacuum to form positive electrode carbon fiber covered with positive electrode material distributed in a lattice, and the desizing carbon fiber is used as negative electrode carbon fiber; each layer is stacked in the order of the positive electrode carbon fiber, the insulating fiber separator, and the negative electrode carbon fiber; in an anhydrous and oxygen-free environment, the electrolyte liquid and the structural resin liquid are mixed in a certain proportion to form a structural electrolyte, and the curing is completed by infusion. The present invention can improve the anti-stripping ability of the positive electrode carbon fiber, and ensure the mechanical properties while having high energy density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of manufacturing multifunctional composite materials, and in particular to a lattice carbon fiber structure battery and a preparation method thereof. Background Art

[0002] In order to further improve the service performance of advanced equipment under more severe loads, integrated energy storage structural composite materials have begun to be proposed. As a typical representative of them, the carbon fiber structure battery is composed of positive electrode carbon fiber-insulating fiber diaphragm-negative electrode carbon fiber loaded with positive electrode materials, as well as electrolyte and structural resin. It fully utilizes the lightweight, high modulus and high strength mechanical properties of carbon fiber and its high conductivity and high specific capacity electrical properties. It can store energy while carrying severe loads and integrate energy into the structure, which saves both mass and space, and provides further development possibilities for the new generation of launch vehicles, manned aircraft, electric vehicles, etc.

[0003] Although the carbon fiber as the negative electrode can simultaneously play multiple roles as a reinforcement, a reaction negative electrode, and a negative electrode current collector, the positive electrode carbon fiber can only play the role of a positive electrode current collector and reinforcement. Carbon fiber structure batteries still need positive electrode active materials for energy storage, and the positive electrode materials are often wrapped on the positive electrode carbon fiber in a slurry coating and drying manner, but this method undoubtedly isolates the contact between the carbon fiber and the structural resin. The weaker positive electrode slurry will become a delamination defect, which is easy to cause the structural resin and the carbon fiber to peel off, causing the fiber to lose its fixed support and buckle, and the mechanical properties will be greatly reduced. The peeled positive electrode material will also lose the energy storage effect, which seriously hinders the further development and application of carbon fiber structure batteries. Therefore, how to change the distribution of the positive electrode material so that it can maintain high energy density while ensuring the anti-peeling performance of its positive electrode carbon fiber layer is an urgent problem to be solved for carbon fiber structure batteries.

[0004] Patent document CN112652737A discloses a composite material structure battery and mobile phone shell based on carbon fiber, wherein the structure battery includes a modified carbon fiber negative electrode and a modified carbon fiber positive electrode; the modified carbon fiber negative electrode is prepared by forming a first modified coating layer as an outer layer on the carbon fiber filaments of the first carbon fiber cloth; the modified carbon fiber positive electrode is prepared by forming a second modified coating layer as an outer layer on the carbon fiber filaments of the second carbon fiber cloth; the modified carbon fiber negative electrode and the modified carbon fiber positive electrode are stacked and laid and completely isolated by a solid electrolyte to form an integral molding structure. This patent only proposes a carbon fiber structure battery structure, and does not consider the mechanical performance degradation caused by the simple coating of the positive electrode slurry on the carbon fiber positive electrode, and cannot simultaneously guarantee high energy density and high mechanical performance. This field still needs to propose a more advanced and more effective design and manufacturing method for high-modulus, high-strength, and high-energy-density carbon fiber structure battery. Summary of the invention

[0005] In view of the defects in the prior art, the object of the present invention is to provide a molding method for a lattice carbon fiber structure battery.

[0006] First aspect:

[0007] The present invention provides a method for preparing a lattice carbon fiber structure battery, comprising the following steps:

[0008] Step S1: mixing the conductive particles, the binder, and the active material, dissolving them in a solvent, and stirring them evenly to form a positive electrode slurry;

[0009] Step S2: laying a separator with lattice holes on the desized carbon fiber, coating the positive electrode slurry described in step S1 on the separator, drying at high temperature under vacuum, and removing the separator to form positive electrode carbon fiber covered with lattice-distributed positive electrode material, and the desized carbon fiber is used as negative electrode carbon fiber;

[0010] Step S3: stacking the layers in the order of the positive electrode carbon fiber, the insulating fiber separator, and the negative electrode carbon fiber;

[0011] Step S4: In an anhydrous and oxygen-free environment, the electrolyte liquid and the structural resin liquid are mixed in a certain proportion to form a structural electrolyte;

[0012] Step S5: In a water-free and oxygen-free environment, the structural electrolyte of step S4 is poured into the preform of step S3 and cured, and after curing, the structural resin is used again to seal the pores; the lattice carbon fiber structure battery is obtained.

[0013] In step S1, the solvent is N-methylpyrrolidone (NMP).

[0014] Preferably, in step S1, the conductive particles include conductive carbon black particles (Super P), acetylene black, the binder includes polyvinylidene fluoride (PVDF), and the active material includes at least one of lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, and ternary lithium metal oxide.

[0015] Preferably, in step S2, the positive electrode carbon fiber and the negative electrode carbon fiber may be woven into a unidirectional fabric, a plain fabric, a twill fabric, a satin fabric or a three-dimensional woven fabric.

[0016] Preferably, in step S2, the holes on the isolation membrane having lattice holes have regular geometric shapes, and the periodic spacing should be determined according to the viscosity of the positive electrode slurry and the permeability of the carbon fiber fabric to avoid the mutual penetration and fusion of the lattice slurries on the carbon fiber fabric surface after coating, thereby losing the lattice structure.

[0017] Preferably, in step S2, the lattice distribution of the positive electrode slurry can be determined according to test results or simulations to ensure that it has the highest utilization rate of mechanical and electrical properties.

[0018] Preferably, the structural resin material includes one or more of epoxy resin, bismaleimide resin, polyimide resin, polyetheretherketone resin, and phenolic resin.

[0019] Preferably, the electrolyte liquid comprises an ionic electrolyte or a solid electrolyte solution. When an ionic electrolyte is used, curing needs to be performed at room temperature or low temperature to avoid volatilization of the organic solvent in the ionic electrolyte. When a solid electrolyte solution is used, curing needs to be performed at medium or high temperature to volatilize the organic solvent in the solid electrolyte solution.

[0020] In step 4, the mixed electrolyte liquid and the structural resin liquid are mixed in equal amounts.

[0021] The lattice carbon fiber structure battery prepared by the above preparation method also belongs to the protection scope of the present invention.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention utilizes dot matrix coating of the positive electrode slurry to avoid the positive electrode carbon fiber being completely wrapped by the positive electrode material, resulting in isolation of the structural resin. The dot matrix distribution method enables each period within the surface of the positive electrode carbon fiber to be wrapped and fixed with a structural resin having higher energy storage and mechanical properties and a positive electrode material.

[0024] 2. The present invention provides a new idea for structural battery design, expands the optimization dimension of in-plane material distribution design, and fully considers the need for carbon fiber structural batteries to meet the requirements of high mechanical properties and high energy density at the same time.

[0025] 3. The present invention designs a distribution mode of the positive electrode material in the positive electrode carbon fiber layer. Since the carbon fiber layers are interconnected and highly conductive, the electrical performance of the positive electrode energy storage layer is less affected.

[0026] 4. The lattice carbon fiber structure battery formed by the present invention has simple steps, low cost, good effect, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0028] Figure 1 This is a schematic diagram of the structure of a lattice high-modulus high-strength high-energy-density carbon fiber structure battery;

[0029] Figure 2Schematic diagram of the lattice distribution of the positive electrode material in the positive electrode carbon fiber layer in Example 2. DETAILED DESCRIPTION

[0030] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several changes and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0031] like Figure 1 As shown, the present invention provides a lattice carbon fiber structure battery.

[0032] The carbon fiber structure battery includes negative electrode carbon fiber, insulating fiber separator, positive electrode carbon fiber, positive electrode material, structural resin and electrolyte.

[0033] Positive carbon fiber and negative carbon fiber are laid on both sides of the insulating fiber diaphragm respectively; the surface of the positive carbon fiber is coated with a dot matrix positive electrode material; the insulating fiber diaphragm with positive carbon fiber and negative carbon fiber laid on both sides is immersed in a mixed solution of structural resin and electrolyte (ionic electrolyte or solid electrolyte polymer), and solidified.

[0034] The structural resin can be selected from epoxy resin, bismaleimide resin, polyimide resin, polyetheretherketone resin or phenolic resin.

[0035] The method for preparing the carbon fiber structure battery comprises the following steps:

[0036] Step S1: mixing a conductive agent, a binder and an active material in a certain proportion, dissolving them in N-methylpyrrolidone (NMP), and stirring to form a positive electrode slurry;

[0037] The conductive agent in the present invention can be selected from acetylene black, conductive carbon black (Super P), and carbon nanotubes.

[0038] The binder may be polyvinylidene fluoride (PVDF).

[0039] The active material may be selected from one or more of ternary lithium metal oxide, lithium iron phosphate, lithium manganese oxide, and lithium cobalt oxide.

[0040] Ternary lithium metal oxides include LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811), LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523), LiNi 0.3 Co 0.3 Mn0.3 O2(NCM111).

[0041] Step S2: Lay a layer of separator with lattice holes on the desized carbon fiber. The desized carbon fiber is obtained by calcining the carbon fiber in air, and the lattice holes of the separator can be obtained by cutting. The positive electrode slurry in step S1 is coated on the separator, and quickly dried at high temperature under vacuum to form positive electrode carbon fiber covered with lattice distributed positive electrode material, and the desized carbon fiber is used as negative electrode carbon fiber;

[0042] The lattice holes described in the present invention refer to holes that are cut and arranged in a geometric shape according to a certain periodic rule.

[0043] Step S3: stacking the layers in the order of the positive electrode carbon fiber, the insulating fiber separator, and the negative electrode carbon fiber to form a preform;

[0044] Step S4: In an anhydrous and oxygen-free environment, the electrolyte liquid is mixed with the structural resin liquid to form a structural electrolyte;

[0045] The electrolyte liquid can be an ionic electrolyte or a solid electrolyte solution; the ionic electrolyte is an ester or ether electrolyte in which LiPF6 or lithium bistrifluoromethanesulfonyl imide (LiTFSI) is dissolved; the solid electrolyte solution is an N-methylpyrrolidone (NMP) solution in which LiTFSI and polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP) or polyethylene oxide (PEO) are dissolved.

[0046] Step S5: In a water-free and oxygen-free environment, the structural electrolyte of step S4 is poured into the preform of step S3 and cured, and after curing, the structural resin is used again to seal the pores;

[0047] Step S6: Conduct mechanical and electrical performance test verification to complete performance experimental verification.

[0048] The lattice distribution of the positive electrode slurry can be determined based on test results or simulations to ensure that it has the highest utilization rate of mechanical and electrical properties.

[0049] In the following embodiments:

[0050] Electrical performance test standard: Use a battery testing system to perform single-rate constant current charge and discharge on the obtained structural battery to test the battery energy density; use an electrochemical workstation to test the structural battery impedance, the AC voltage amplitude is 0.01V, and the frequency range is: 0.01Hz-100kHz.

[0051] Mechanical properties test standards: The tensile test refers to ASTM D3039 Standard Test Method for Tensile Properties of Polymer Matrix Composites; the bending test refers to ASTM D790 Standard Test Method for Bending Properties of Unreinforced and Reinforced Plastics and Electrical Insulating Materials.

[0052] Example 1

[0053] The carbon fiber structure battery of this embodiment includes a negative electrode carbon fiber unidirectional tape, a high-strength plain glass fiber separator, a positive electrode carbon fiber unidirectional tape, a positive electrode material, a structural epoxy resin and a LiPF6 ion electrolyte; both sides of the high-strength glass fiber separator are respectively paved with a dotted LiNi 0.8 Co 0.1 Mn 0.1 The positive electrode carbon fiber unidirectional tape and the negative electrode carbon fiber unidirectional tape of the O2 (NCM811) positive electrode material form a preform, and the preform is entirely impregnated with a mixed solution of a structural resin and an ion electrolyte or a solid electrolyte polymer, and then cured. Figure 2 The figure shows a schematic diagram of the dot distribution of the positive electrode material in the positive electrode carbon fiber layer. The plain fabric substrate in the figure is only for illustration. The carbon fiber used in Example 2 is in the form of a unidirectional tape.

[0054] The specific steps are as follows:

[0055] T1, conductive carbon black particles (Super P): polyvinylidene fluoride (PVDF): LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811) was mixed in a mass ratio of 1:1:8, dissolved in N-methylpyrrolidone (NMP), and stirred for 20 hours to form a positive electrode slurry;

[0056] T2, a T700 carbon fiber unidirectional tape desizing after calcination at 400°C for 1.5h in air is used as the negative electrode carbon fiber, a portion of the desizing carbon fiber is taken, and a layer of an isolating film with lattice holes is laid on it, wherein the specific structure of the isolating film with lattice holes is a circular array with a diameter of 15mm and a period of 20mm, and the positive electrode slurry described in T1 is coated, and dried at 120°C in vacuum for 12h, and the NMP is dried to obtain a positive electrode carbon fiber 3 with a lattice positive electrode material distribution;

[0057] T3, lay out a 10 micron thick stainless steel foil as the positive electrode current collector, a 0.1 mm thick positive electrode carbon fiber unidirectional tape containing a dot matrix NCM811 positive electrode material distribution in T2 as the positive electrode, a 0.1 mm thick high-strength plain glass fiber separator, and another 0.1 mm thick carbon fiber unidirectional tape in T2 as the negative electrode 1, and lay out the stainless steel foil again as the negative electrode current collector;

[0058] T4. In a glove box, under an argon atmosphere, mix a commercial room temperature curing structural resin (epoxy resin) and a LiPF6 ion electrolyte of equal mass, inject them into the preform stacked in T3, seal and evacuate, and cure at 40°C. After curing, use the structural resin again to seal the holes;

[0059] T5. Conduct electrical and mechanical performance tests on the structural battery obtained in T4 to complete performance verification.

[0060] The resulting structural battery has a tensile modulus of 37.5 GPa, a tensile strength of 394.2 MPa, a flexural modulus of 30.9 GPa, a flexural strength of 272.5 MPa, an energy density of 94.2 Wh / kg, and an impedance of 561 Ω. It also has high mechanical and electrical properties.

[0061] Example 2

[0062] This embodiment provides a structural battery, and its preparation method is basically the same as that of embodiment 1, except that: in step T2, an isolation film having another form of lattice holes is laid, such as Figure 3 As shown, the specific structure of the isolation film of the lattice holes is a square array with a period of 10 mm and a side length of 8 mm.

[0063] The resulting structural battery has a tensile modulus of 34.9 GPa, a tensile strength of 407.1 MPa, a flexural modulus of 32.7 GPa, a flexural strength of 311.2 MPa, an energy density of 101.9 Wh / kg, and an impedance of 486 Ω. It also has high mechanical and electrical properties.

[0064] Comparative Example 1

[0065] Comparative Example 1 provides a structural battery, and the preparation method is as follows:

[0066] T1, conductive carbon black particles (Super P): polyvinylidene fluoride (PVDF): LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811) was mixed in a mass ratio of 1:1:8, dissolved in N-methylpyrrolidone (NMP), and stirred for 20 hours to form a positive electrode slurry;

[0067] T2, calcining the T700 carbon fiber unidirectional tape at 400°C for 1.5 hours in air for desizing to obtain negative electrode carbon fiber, taking a portion of the negative electrode carbon fiber and uniformly coating it with the positive electrode slurry described in T1, drying it at 120°C in vacuum for 12 hours, drying the NMP, and obtaining positive electrode carbon fiber covered with energy storage material;

[0068] T3, lay out a 10 μm thick stainless steel foil as the positive electrode current collector, a portion of the positive electrode carbon fiber unidirectional tape containing NCM811 positive electrode material in T2 as the positive electrode, a portion of 0.1 mm thick high-strength plain glass fiber, and another portion of the carbon fiber unidirectional tape in T2 as the negative electrode on the concave mold, and lay out the stainless steel foil again as the negative electrode current collector;

[0069] T4. In a glove box, under an argon atmosphere, mix the structural epoxy resin and the LiPF6 ion electrolyte in equal amounts, pour them into the preform stacked in T3, seal and evacuate, and cure at 40°C. After curing, use the structural resin to seal the holes again;

[0070] T5. Conduct electrical and mechanical performance tests on the structural battery obtained in T4 to complete performance verification.

[0071] The obtained structural battery has a tensile modulus of 24.50 GPa, a tensile strength of 260.8 MPa, a flexural modulus of 16.1 GPa, a flexural strength of 235.2 MPa, an energy density of 107.7 Wh / kg, and an impedance of 523 Ω. The electrical properties are similar, but the mechanical properties are significantly worse than those of Comparative Example 1.

[0072] In this comparative example, a uniform coating method is adopted, which blocks the infiltration of the resin and the positive electrode fiber, is easy to be delaminated, and has poor mechanical properties.

[0073] In the description of the present application, it should be understood that the terms "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating orientations or positional relationships, are based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.

[0074] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art can make various changes or modifications within the scope of the claims, which does not affect the essence of the present invention. In the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other arbitrarily.

Claims

1. A method for preparing a lattice carbon fiber structure battery, characterized in that: The following steps are involved: Step S1: mixing the conductive particles, the binder, and the active material, dissolving them in a solvent, and stirring them evenly to form a positive electrode slurry; Step S2: laying a separator with lattice holes on the desized carbon fiber, coating the positive electrode slurry in step S1 on the separator, drying at high temperature under vacuum, and then removing the separator to form positive electrode carbon fiber covered with lattice-distributed positive electrode material; the desized carbon fiber is used as negative electrode carbon fiber; Step S3: stacking the layers in the order of the positive electrode carbon fiber, the insulating fiber separator, and the negative electrode carbon fiber; Step S4: in an anhydrous and oxygen-free environment, mixing the electrolyte liquid and the structural resin liquid in a certain proportion to form a structural electrolyte; mixing the mixed electrolyte liquid and the structural resin liquid in equal amounts; Step S5: In a water-free and oxygen-free environment, the structural electrolyte of step S4 is poured into the preform of step S3 and cured, and after curing, the structural resin is used again to seal the pores; the lattice carbon fiber structure battery is obtained.

2. The method for preparing a lattice carbon fiber structure battery according to claim 1, characterized in that: In step S1, the solvent is N-methylpyrrolidone.

3. The method for preparing a lattice carbon fiber structure battery according to claim 1, characterized in that: In step S1, the conductive particles include conductive carbon black particles and acetylene black, and the binder includes polyvinylidene fluoride (PVDF).

4. The method for preparing a lattice carbon fiber structure battery according to claim 1, characterized in that: In step S2, the positive electrode carbon fiber and the negative electrode carbon fiber are respectively woven into one of unidirectional fabric, plain fabric, twill fabric, satin fabric, and three-dimensional woven fabric.

5. The method for preparing a lattice carbon fiber structure battery according to claim 1, characterized in that: In step S2, the holes on the isolation film having lattice holes include regular geometric shapes.

6. The method for preparing a lattice carbon fiber structure battery according to claim 1, characterized in that: In step S2, the structural resin material includes epoxy resin, bismaleimide resin, polyimide resin, polyetheretherketone resin or phenolic resin.

7. The method for preparing a lattice carbon fiber structure battery according to claim 1, characterized in that: In step S4, the electrolyte liquid includes an ionic electrolyte or a solid electrolyte solution.

8. The method for preparing a lattice carbon fiber structure battery according to claim 1, characterized in that: In step S1, the active material includes at least one of lithium iron phosphate, lithium manganese oxide, lithium cobalt oxide, and ternary lithium metal oxide.

9. A lattice carbon fiber structure battery prepared by the preparation method according to any one of claims 1 to 8.