Preparation method of large-size amorphous soft magnetic composite powder
Through the preparation method of large-size amorphous soft magnetic composite powder and the use of smelting, atomization and surface treatment technologies, the problems of insufficient frequency stability and corrosion resistance of existing soft magnetic materials in emerging fields have been solved, and a high-performance technology has been achieved. Performance improvements to power device standards.
Patent Information
- Application Number
- CN202310020814.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-06
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-01-06
AI Technical Summary
When existing soft magnetic composite materials are used in emerging fields, their frequency stability and corrosion resistance cannot meet the use standards of integrated inductors, especially in high-power, large-scale applications such as 5G base stations, photovoltaic inverters, and rail transit transformers. There are deficiencies in the capacity equipment.
The preparation method of large-size amorphous soft magnetic composite powder is adopted, including smelting, atomization and surface treatment. The specific steps are: melt the raw materials in a smelting furnace and then crush them in high-pressure water atomization equipment to form powder, and then through plasma surface treatment, pyrophosphate coating and coupling agent surface treatment to form a powder with high frequency stability and Amorphous soft magnetic composite powder with corrosion resistance.
The prepared amorphous soft magnetic composite powder has a particle size distribution of 28-50 μm, and its frequency stability and corrosion resistance meet the standards for use of integrated molded inductors, significantly improving the application performance of equipment in emerging fields.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnetic materials, in particular to a method for preparing large-size amorphous soft magnetic composite powder. Background Art
[0002] Magnetic functional materials are the foundation for the advancement of the new energy industry, but existing ferrite materials are difficult to meet the high power, large capacity and high superposition requirements of industries such as photovoltaic power generation, 5G, energy storage and electric vehicles. Soft magnetic composite materials (SMC) not only have a higher saturation magnetic induction intensity but also a higher frequency of use. The raw material cost is low, and the application scenarios fill the gap between ferrite and silicon steel.
[0003] However, in the construction of "new infrastructure", key supporting equipment or components such as 5G base stations, photovoltaic inverters, rail transit transformers, new energy vehicles and charging piles, big data center substations, and UHV control cabinets have high requirements for related manufacturing materials. When SMC prepared by existing preparation processes is used in emerging fields, there are often many problems. For example, the one-piece molded inductor, which has developed rapidly in recent years, has also put forward higher requirements on the existing soft magnetic alloy powder. The frequency stability and corrosion resistance of the existing SMC are far from meeting the use standards of one-piece molded inductors. Summary of the invention
[0004] The object of the present invention is to provide a method for preparing a large-sized amorphous soft magnetic composite powder whose frequency stability and corrosion resistance performance meet the use standards of an integrally formed inductor.
[0005] In order to solve at least any one of the above technical problems, the present invention provides a method for preparing a large-size amorphous soft magnetic composite powder, including smelting, atomization and surface treatment. Smelting includes adding the raw materials into the smelting furnace one by one, increasing the power to 80-200kW, until the charge is completely melted; when the temperature of the molten steel is ≥1580℃, after refining for several minutes and standing for 1-3min, the molten steel is cleaned of slag, and the temperature of the molten steel is reduced to 1450℃, ensuring that the alloy is overheated by 100-200℃, and atomizing in the atomization equipment after starting the pump; atomization includes using high-pressure water from a high-pressure water pump to impact the molten metal after smelting, breaking it into metal droplets, wherein the water atomization pressure is 105-110MPa, and condensing to form powder; surface treatment includes successively treating the powder with plasma surface treatment, pyrophosphate coating, and coupling agent surface treatment to obtain amorphous soft magnetic composite powder.
[0006] The pyrophosphate coating comprises: the pyrophosphate coating comprises: stirring the powder formed after atomization in a solvent for 2-6 hours, dripping a 10-20wt.% pyrophosphate aqueous solution for 2-4 hours, heating to 35°C-50°C for reaction, and the mass ratio of the powder formed after atomization to the pyrophosphate is 1:(0.1-10);
[0007] The particle size distribution D50 of the amorphous soft magnetic composite powder is 28-50 μm.
[0008] Optionally, the elements of the amorphous soft magnetic composite powder other than iron may include, for example, B, C, N, O, Al, Si, P, S, Ti, V, Cr, Mn, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Cd ..., In, Sn, etc., and a combination of one or two or more thereof. The elements of the amorphous soft magnetic composite powder are determined according to the type of raw materials. In one embodiment, the main components of the amorphous soft magnetic composite powder are shown in Table 1 below, and the main indicators are shown in Table 2.
[0009] Table 1 Main ingredients and proportions
[0010] element Fe Si Ni Cr B C Proportion (weight) margin 2.3-5.8 0-2.5 0-3.5 2.0-4.0 0-1.5
[0011] Table 2 Main indicators of amorphous soft magnetic composite powder
[0012] project Index value Bs ≥145emu / g Ue ≥19 Ploss <![CDATA[≤2900mW / cm 3 ]]> D50 ≥28um DC-bias ≥78%
[0013] The raw materials of the amorphous soft magnetic composite powders shown in Table 1 include industrial pure iron, industrial ferroboron, single crystal silicon, ferrochrome and high carbon iron. In the preparation process of other amorphous soft magnetic composite powders, the raw materials include any one or more of industrial pure iron, industrial ferroboron, single crystal silicon, ferrochrome and high carbon iron, and other rare earth elements may be added as needed.
[0014] Optionally, the coupling agent includes a combination of one or more of a silane coupling agent, a titanium coupling agent, an aluminum coupling agent and a zirconium coupling agent. Preferably, the coupling agent is a silane coupling agent. Optionally, the silane coupling agent is selected from a combination of one or more of trimethylacryloxypropyltrimethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, methacryloxytrimethoxysilane, 3-epoxypropylenetrimethoxysilane, and 3-aminopropyltriethoxysilane.
[0015] Optionally, the plasma surface treatment includes a combination of one or more of oxygen plasma surface treatment, argon plasma surface treatment, and nitrogen plasma surface treatment. Preferably, the plasma surface treatment is oxygen plasma surface treatment.
[0016] Optionally, the pyrophosphate is sodium pyrophosphate or potassium pyrophosphate.
[0017] Optionally, the solvent includes one or more of water, PVP (polyvinyl pyrrolidone), and alcohol.
[0018] Optionally, the coupling agent surface treatment includes: adding 3-aminopropyltriethoxysilane to a mixture of alcohol and water in a mass ratio of (2-10):1; magnetically stirring at a constant temperature of 50-60°C for 20-30 minutes, and then adding the powders after the plasma surface treatment respectively, continuing to stir for 20-30 minutes, and keeping warm at 50-100°C for 30 minutes to 60 minutes.
[0019] Optionally, the plasma surface treatment includes oxygen plasma surface treatment, and the oxygen plasma surface treatment includes: the radio frequency frequency of the plasma instrument is 12-15MHz, the output power range is 0-300W, the gas pressure is 50-100Pa, the oxygen flow rate is set to 100-200mL / mi, and the treatment time is 1min-30min.
[0020] Optionally, the mass ratio of 3-aminopropyltriethoxysilane to the powder after plasma surface treatment is (1-10):100.
[0021] In summary, the preparation method of a large-sized amorphous soft magnetic composite powder provided by the present invention is to treat the powder surface with plasma surface treatment, pyrophosphate coating, and coupling agent surface treatment in sequence, firstly obtain reactive sites with plasma surface treatment, and then respectively perform a binding reaction with the reactive sites obtained with pyrophosphate, coupling agent surface treatment, and plasma surface treatment in sequence. Through such surface treatment, functional groups can be bound to the surface of magnetic particles. Functional groups can cover part or all of the surface of these particles. The final large-sized amorphous soft magnetic composite powder has a particle size distribution D50 of 28-50μm, and the frequency stability and corrosion resistance performance meet the use standards of one-piece molded inductors. DETAILED DESCRIPTION
[0022] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0023] Soft magnetism is a magnetic material with low coercivity and high magnetic permeability. Generally speaking, when magnetization occurs at Hc not greater than 1000A / m, such a material is called a soft magnet.
[0024] Large size refers to the amorphous soft magnetic composite powder particle size distribution D50 above 28μm, and further, it refers to the particle size distribution D50 between 28-50μm.
[0025] Example 1
[0026] Melting: Add industrial pure iron, industrial ferroboron, single crystal silicon, ferrochrome and high carbon iron into the melting furnace in order according to the burning loss and oxidation difficulty of the elements, increase the power to 80-200kW, until the charge is completely melted; when the temperature of the molten steel is ≥1580℃, refine it for several minutes and let it stand for 1-3 minutes, remove the slag from the molten steel, lower the temperature of the molten steel to 1450℃, ensure that the alloy is overheated by 100-200℃, start the pump and atomize it in the atomization equipment;
[0027] Atomization: High-pressure water from a high-pressure water pump impacts the molten metal to break it into metal droplets. The water atomization pressure is 105-110 MPa, and condenses to form powder.
[0028] Surface treatment: The powder is surface treated with oxygen plasma surface treatment, sodium pyrophosphate coating, and silane coupling agent (3-aminopropyltriethoxysilane) surface treatment to obtain an amorphous soft magnetic composite powder;
[0029] The sodium pyrophosphate coating comprises: the sodium pyrophosphate coating comprises: stirring the powder formed after atomization in water for 4 hours, dripping a 15wt.% sodium pyrophosphate aqueous solution into the water for 3 hours, heating to 42°C for reaction, wherein the amount of the powder formed after atomization and the sodium pyrophosphate added is 1:1 by mass ratio;
[0030] The coupling agent surface treatment includes: adding 3-aminopropyltriethoxysilane to a mixture of alcohol and water in a mass ratio of 5:1; magnetically stirring at a constant temperature of 55°C for 25 minutes, and then adding the powders after the plasma surface treatment respectively, continuing to stir for 25 minutes, and keeping warm at 75°C for 45 minutes.
[0031] Plasma surface treatment includes oxygen plasma surface treatment, which includes: the radio frequency frequency of the plasma instrument is 13 MHz, the output power range is 200 W, the gas pressure is 75 Pa, the oxygen flow rate is set to 150 mL / mi, and the treatment time is 20 min.
[0032] The mass ratio of 3-aminopropyltriethoxysilane to the powder after plasma surface treatment is 5:100.
[0033] The obtained amorphous soft magnetic composite powder has a particle size distribution of D10 of 15 μm, D50 of 30 μm, and D90 of 56 μm. The powder has good sphericity and a smooth surface, a uniform powder structure, and the alloy has a single amorphous structure.
[0034] Example 2
[0035] Melting: Add industrial pure iron, industrial ferroboron, single crystal silicon, ferrochrome and high carbon iron into the melting furnace in order according to the burning loss and oxidation difficulty of the elements, increase the power to 80-200kW, until the charge is completely melted; when the temperature of the molten steel is ≥1580℃, refine it for several minutes and let it stand for 1-3 minutes, remove the slag from the molten steel, lower the temperature of the molten steel to 1450℃, ensure that the alloy is overheated by 100-200℃, start the pump and atomize it in the atomization equipment;
[0036] Atomization: High-pressure water from a high-pressure water pump impacts the molten metal to break it into metal droplets. The water atomization pressure is 105-110 MPa, and condenses to form powder.
[0037] Surface treatment: The powder is surface treated with oxygen plasma surface treatment, sodium pyrophosphate coating, and silane coupling agent (3-aminopropyltriethoxysilane) surface treatment to obtain an amorphous soft magnetic composite powder;
[0038] The sodium pyrophosphate coating comprises: the sodium pyrophosphate coating comprises: stirring the powder formed after atomization in water for 2 hours, dripping a 10wt.% sodium pyrophosphate aqueous solution into the water for 2 hours, heating to 35°C for reaction, and the mass ratio of the powder formed after atomization to the sodium pyrophosphate is 1:0.1;
[0039] The coupling agent surface treatment includes: adding 3-aminopropyltriethoxysilane to a mixture of alcohol and water in a mass ratio of 2:1; magnetically stirring at a constant temperature of 50°C for 20 minutes, and then adding the powders after the plasma surface treatment respectively, continuing to stir for 20 minutes, and keeping at 50°C for 60 minutes.
[0040] Plasma surface treatment includes oxygen plasma surface treatment, which includes: the radio frequency frequency of the plasma instrument is 12 MHz, the output power range is 100 W, the gas pressure is 50 Pa, the oxygen flow rate is set to 100 mL / mi, and the treatment time is 15 min.
[0041] The mass ratio of 3-aminopropyltriethoxysilane to the powder after plasma surface treatment is 1:100.
[0042] The obtained amorphous soft magnetic composite powder has a particle size distribution of D10 of 14 μm, D50 of 28 μm, and D90 of 57 μm. The powder has good sphericity and a smooth surface, a uniform powder structure, and the alloy has a single amorphous structure.
[0043] Example 3
[0044] Melting: Add industrial pure iron, industrial ferroboron, single crystal silicon, ferrochrome and high carbon iron into the melting furnace in order according to the burning loss and oxidation difficulty of the elements, increase the power to 80-200kW, until the charge is completely melted; when the temperature of the molten steel is ≥1580℃, refine it for several minutes and let it stand for 1-3 minutes, remove the slag from the molten steel, lower the temperature of the molten steel to 1450℃, ensure that the alloy is overheated by 100-200℃, start the pump and atomize it in the atomization equipment;
[0045] Atomization: High-pressure water from a high-pressure water pump impacts the molten metal to break it into metal droplets. The water atomization pressure is 105-110 MPa, and condenses to form powder.
[0046] Surface treatment: The powder is surface treated with oxygen plasma surface treatment, sodium pyrophosphate coating, and silane coupling agent (3-aminopropyltriethoxysilane) surface treatment to obtain an amorphous soft magnetic composite powder;
[0047] The sodium pyrophosphate coating comprises: the sodium pyrophosphate coating comprises: stirring the powder formed after atomization in water for 6 hours, dripping a 20wt.% sodium pyrophosphate aqueous solution into the water for 4 hours, heating to 50°C for reaction, and the mass ratio of the powder formed after atomization to the sodium pyrophosphate is 1:10;
[0048] The coupling agent surface treatment includes: adding 3-aminopropyltriethoxysilane to a mixture of alcohol and water in a mass ratio of 10:1; magnetically stirring at a constant temperature of 60°C for 30 minutes, and then adding the powders after the plasma surface treatment respectively, continuing to stir for 30 minutes, and keeping warm at 100°C for 30 minutes.
[0049] Plasma surface treatment includes oxygen plasma surface treatment, and oxygen plasma surface treatment includes: the radio frequency frequency of the plasma instrument is 15 MHz, the output power range is 300 W, the gas pressure is 5100 Pa, the oxygen flow rate is set to 200 mL / mi, and the treatment time is 30 min.
[0050] The mass ratio of 3-aminopropyltriethoxysilane to the powder after plasma surface treatment is 10:100.
[0051] The obtained amorphous soft magnetic composite powder has a particle size distribution of D10 of 15 μm, D50 of 29 μm, and D90 of 56 μm. The powder has good sphericity and a smooth surface, a uniform powder structure, and the alloy has a single amorphous structure.
[0052] Example 4
[0053] Melting: Add industrial pure iron, industrial ferroboron, single crystal silicon, ferrochrome and high carbon iron into the melting furnace in order according to the burning loss and oxidation difficulty of the elements, increase the power to 80-200kW, until the charge is completely melted; when the temperature of the molten steel is ≥1580℃, refine it for several minutes and let it stand for 1-3 minutes, remove the slag from the molten steel, lower the temperature of the molten steel to 1450℃, ensure that the alloy is overheated by 100-200℃, start the pump and atomize it in the atomization equipment;
[0054] Atomization: High-pressure water from a high-pressure water pump impacts the molten metal to break it into metal droplets. The water atomization pressure is 105-110 MPa, and condenses to form powder.
[0055] Surface treatment: The powder is surface treated with oxygen plasma surface treatment, potassium pyrophosphate coating, and silane coupling agent (3-aminopropyltriethoxysilane) surface treatment to obtain an amorphous soft magnetic composite powder;
[0056] The potassium pyrophosphate coating comprises: the potassium pyrophosphate coating comprises: stirring the powder formed after atomization in water for 4 hours, dripping a 15wt.% potassium pyrophosphate aqueous solution into the water for 3 hours, heating to 42°C for reaction, and the mass ratio of the powder formed after atomization to the potassium pyrophosphate is 1:1;
[0057] The coupling agent surface treatment includes: adding 3-aminopropyltriethoxysilane to a mixture of alcohol and water in a mass ratio of 5:1; magnetically stirring at a constant temperature of 55°C for 25 minutes, and then adding the powders after the plasma surface treatment respectively, continuing to stir for 25 minutes, and keeping warm at 75°C for 45 minutes.
[0058] Plasma surface treatment includes oxygen plasma surface treatment, which includes: the radio frequency frequency of the plasma instrument is 13 MHz, the output power range is 200 W, the gas pressure is 75 Pa, the oxygen flow rate is set to 150 mL / mi, and the treatment time is 20 min.
[0059] The mass ratio of 3-aminopropyltriethoxysilane to the powder after plasma surface treatment is 5:100.
[0060] The obtained amorphous soft magnetic composite powder has a particle size distribution of D10 of 15 μm, D50 of 30 μm, and D90 of 56 μm. The powder has good sphericity and a smooth surface, a uniform powder structure, and the alloy has a single amorphous structure.
[0061] Example 5
[0062] Melting: Add industrial pure iron, industrial ferroboron, single crystal silicon, ferrochrome and high carbon iron into the melting furnace in order according to the burning loss and oxidation difficulty of the elements, increase the power to 80-200kW, until the charge is completely melted; when the temperature of the molten steel is ≥1580℃, refine it for several minutes and let it stand for 1-3 minutes, remove the slag from the molten steel, lower the temperature of the molten steel to 1450℃, ensure that the alloy is overheated by 100-200℃, start the pump and atomize it in the atomization equipment;
[0063] Atomization: High-pressure water from a high-pressure water pump impacts the molten metal to break it into metal droplets. The water atomization pressure is 105-110 MPa, and condenses to form powder.
[0064] Surface treatment: The powder is surface treated with oxygen plasma surface treatment, sodium pyrophosphate coating, and silane coupling agent (vinyl trimethoxy silane) surface treatment to obtain an amorphous soft magnetic composite powder;
[0065] The sodium pyrophosphate coating comprises: the sodium pyrophosphate coating comprises: stirring the powder formed after atomization in water for 4 hours, dripping a 15wt.% sodium pyrophosphate aqueous solution into the water for 3 hours, heating to 42°C for reaction, and the mass ratio of the powder formed after atomization to the sodium pyrophosphate is 1:1;
[0066] The coupling agent surface treatment includes: adding vinyl trimethoxysilane to a mixture of alcohol and water in a mass ratio of 5:1; magnetically stirring at a constant temperature of 55°C for 25 minutes, and then adding the powders after the plasma surface treatment respectively, continuing to stir for 25 minutes, and keeping warm at 75°C for 45 minutes.
[0067] Plasma surface treatment includes oxygen plasma surface treatment, which includes: the radio frequency frequency of the plasma instrument is 13 MHz, the output power range is 200 W, the gas pressure is 75 Pa, the oxygen flow rate is set to 150 mL / mi, and the treatment time is 20 min.
[0068] The mass ratio of vinyltrimethoxysilane to the powder after plasma surface treatment is 5:100.
[0069] The obtained amorphous soft magnetic composite powder has a particle size distribution of D10 of 15 μm, D50 of 30 μm, and D90 of 56 μm. The powder has good sphericity and a smooth surface, a uniform powder structure, and the alloy has a single amorphous structure.
[0070] Example 6
[0071] Melting: Add industrial pure iron, industrial ferroboron, single crystal silicon, ferrochrome and high carbon iron into the melting furnace in order according to the burning loss and oxidation difficulty of the elements, increase the power to 80-200kW, until the charge is completely melted; when the temperature of the molten steel is ≥1580℃, refine it for several minutes and let it stand for 1-3 minutes, remove the slag from the molten steel, lower the temperature of the molten steel to 1450℃, ensure that the alloy is overheated by 100-200℃, start the pump and atomize it in the atomization equipment;
[0072] Atomization: High-pressure water from a high-pressure water pump impacts the molten metal to break it into metal droplets. The water atomization pressure is 105-110 MPa, and condenses to form powder.
[0073] Surface treatment: The powder is surface treated with oxygen plasma surface treatment, sodium pyrophosphate coating, and silane coupling agent (3-aminopropyltriethoxysilane) surface treatment to obtain an amorphous soft magnetic composite powder;
[0074] The sodium pyrophosphate coating comprises: the sodium pyrophosphate coating comprises: stirring the powder formed after atomization in PVP for 4 hours, dripping a 15wt.% sodium pyrophosphate aqueous solution into the powder for 3 hours, heating to 42°C for reaction, wherein the amount of the powder formed after atomization and the sodium pyrophosphate added is 1:1 by mass ratio;
[0075] The coupling agent surface treatment includes: adding 3-aminopropyltriethoxysilane to a mixture of alcohol and water in a mass ratio of 5:1; magnetically stirring at a constant temperature of 55°C for 25 minutes, and then adding the powders after the plasma surface treatment respectively, continuing to stir for 25 minutes, and keeping warm at 75°C for 45 minutes.
[0076] Plasma surface treatment includes oxygen plasma surface treatment, which includes: the radio frequency frequency of the plasma instrument is 13 MHz, the output power range is 200 W, the gas pressure is 75 Pa, the oxygen flow rate is set to 150 mL / mi, and the treatment time is 20 min.
[0077] The mass ratio of 3-aminopropyltriethoxysilane to the powder after plasma surface treatment is 5:100.
[0078] The obtained amorphous soft magnetic composite powder has a particle size distribution of D10 of 15 μm, D50 of 30 μm, and D90 of 56 μm. The powder has good sphericity and a smooth surface, a uniform powder structure, and the alloy has a single amorphous structure.
[0079] Comparative Example 1
[0080] Melting: Add industrial pure iron, industrial ferroboron, single crystal silicon, ferrochrome and high carbon iron into the melting furnace in order according to the burning loss and oxidation difficulty of the elements, increase the power to 80-200kW, until the charge is completely melted; when the temperature of the molten steel is ≥1580℃, refine it for several minutes and let it stand for 1-3 minutes, remove the slag from the molten steel, lower the temperature of the molten steel to 1450℃, ensure that the alloy is overheated by 100-200℃, start the pump and atomize it in the atomization equipment;
[0081] Atomization: High-pressure water from a high-pressure water pump impacts the molten metal to break it into metal droplets. The water atomization pressure is 105-110 MPa, and condenses to form powder.
[0082] Surface treatment: The powder is surface treated with oxygen plasma and silane coupling agent (3-aminopropyltriethoxysilane) to obtain amorphous soft magnetic composite powder;
[0083] The coupling agent surface treatment includes: adding 3-aminopropyltriethoxysilane to a mixture of alcohol and water in a mass ratio of 5:1; magnetically stirring at a constant temperature of 55°C for 25 minutes, and then adding the powders after the plasma surface treatment respectively, continuing to stir for 25 minutes, and keeping warm at 75°C for 45 minutes.
[0084] Plasma surface treatment includes oxygen plasma surface treatment, which includes: the radio frequency frequency of the plasma instrument is 13 MHz, the output power range is 200 W, the gas pressure is 75 Pa, the oxygen flow rate is set to 150 mL / mi, and the treatment time is 20 min.
[0085] The mass ratio of 3-aminopropyltriethoxysilane to the powder after plasma surface treatment is 5:100.
[0086] The particle size distribution D50 of the prepared amorphous soft magnetic composite powder is 20 μm.
[0087] Comparative Example 2
[0088] Melting: Add industrial pure iron, industrial ferroboron, single crystal silicon, ferrochrome and high carbon iron into the melting furnace in order according to the burning loss and oxidation difficulty of the elements, increase the power to 80-200kW, until the charge is completely melted; when the temperature of the molten steel is ≥1580℃, refine it for several minutes and let it stand for 1-3 minutes, remove the slag from the molten steel, lower the temperature of the molten steel to 1450℃, ensure that the alloy is overheated by 100-200℃, start the pump and atomize it in the atomization equipment;
[0089] Atomization: High-pressure water from a high-pressure water pump impacts the molten metal to break it into metal droplets. The water atomization pressure is 105-110 MPa, and condenses to form powder.
[0090] Surface treatment: The powder is surface treated by coating with sodium pyrophosphate and surface treatment with a silane coupling agent (3-aminopropyltriethoxysilane) to obtain an amorphous soft magnetic composite powder;
[0091] The sodium pyrophosphate coating comprises: the sodium pyrophosphate coating comprises: stirring the powder formed after atomization in water for 4 hours, dripping a 15wt.% sodium pyrophosphate aqueous solution into the water for 3 hours, heating to 42°C for reaction, wherein the amount of the powder formed after atomization and the sodium pyrophosphate added is 1:1 by mass ratio;
[0092] The coupling agent surface treatment includes: adding 3-aminopropyltriethoxysilane to a mixture of alcohol and water in a mass ratio of 5:1; magnetically stirring at a constant temperature of 55°C for 25 minutes, and then adding the powders after the plasma surface treatment respectively, continuing to stir for 25 minutes, and keeping warm at 75°C for 45 minutes.
[0093] The mass ratio of 3-aminopropyltriethoxysilane to the powder after plasma surface treatment is 5:100.
[0094] The particle size distribution D50 of the prepared amorphous soft magnetic composite powder is 25 μm.
[0095] Comparative Example 3
[0096] Melting: Add industrial pure iron, industrial ferroboron, single crystal silicon, ferrochrome and high carbon iron into the melting furnace in order according to the burning loss and oxidation difficulty of the elements, increase the power to 80-200kW, until the charge is completely melted; when the temperature of the molten steel is ≥1580℃, refine it for several minutes and let it stand for 1-3 minutes, remove the slag from the molten steel, lower the temperature of the molten steel to 1450℃, ensure that the alloy is overheated by 100-200℃, start the pump and atomize it in the atomization equipment;
[0097] Atomization: High-pressure water from a high-pressure water pump impacts the molten metal to break it into metal droplets. The water atomization pressure is 105-110 MPa, and condenses to form powder.
[0098] Surface treatment: The powder is surface treated with oxygen plasma and then coated with sodium pyrophosphate to obtain amorphous soft magnetic composite powder;
[0099] The sodium pyrophosphate coating comprises: the sodium pyrophosphate coating comprises: stirring the powder formed after atomization in water for 4 hours, dripping a 15wt.% sodium pyrophosphate aqueous solution into the water for 3 hours, heating to 42°C for reaction, wherein the amount of the powder formed after atomization and the sodium pyrophosphate added is 1:1 by mass ratio;
[0100] Plasma surface treatment includes oxygen plasma surface treatment, which includes: the radio frequency frequency of the plasma instrument is 13 MHz, the output power range is 200 W, the gas pressure is 75 Pa, the oxygen flow rate is set to 150 mL / mi, and the treatment time is 20 min.
[0101] The particle size distribution D50 of the prepared amorphous soft magnetic composite powder is 18 μm.
[0102] By comparing the results of each embodiment and the comparative embodiment in Table 4, the anti-corrosion performance and frequency characteristics of the amorphous soft magnetic composite powder in the embodiment are significantly higher than those in the comparative embodiment. Among the various embodiments, the result in Example 6 is the best illustration, and PVP can significantly promote the coating effect of pyrophosphate.
[0103] Table 3 Main components and proportions of amorphous soft magnetic composite powders
[0104]
[0105] Table 4 Parameters of amorphous soft magnetic composite powders in each embodiment
[0106]
[0107] Test conditions: ①100kHz, 100mT ②↓90%u
[0108] Although the present invention has been disclosed as above by the preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make slight changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope of protection required by the claims.
Claims
1. A method for preparing large-sized amorphous soft magnetic composite powder, characterized in that: include: Melting: Add the raw materials into the melting furnace one by one, increase the power to 80-200kW, until the charge is completely melted; when the temperature of the molten steel is ≥1580℃, refine for several minutes and let it stand for 1-3min, remove the slag from the molten steel, lower the temperature of the molten steel to 1450℃, ensure that the alloy is overheated by 100-200℃, start the pump and atomize it in the atomizing equipment; Atomization: High-pressure water from a high-pressure water pump impacts the molten metal to break it into metal droplets. The water atomization pressure is 105-110 MPa, and condenses to form powder. Surface treatment: the powder is surface treated by plasma surface treatment, pyrophosphate coating and coupling agent surface treatment to obtain amorphous soft magnetic composite powder; The pyrophosphate coating comprises: stirring the powder formed after atomization in a solvent for 2-6 hours, dripping a 10-20wt.% pyrophosphate aqueous solution into the solvent for 2-4 hours, heating the solution to 35°C-50°C for reaction, wherein the mass ratio of the powder formed after atomization to the pyrophosphate is 1: (0.1-10); The amorphous soft magnetic composite powder has a particle size distribution D50 of 28-50 μm.
2. The method for preparing large-sized amorphous soft magnetic composite powder according to claim 1, characterized in that: The raw materials include any one or more of industrial pure iron, industrial ferroboron, single crystal silicon, ferrochrome and high carbon iron.
3. The method for preparing large-sized amorphous soft magnetic composite powder according to claim 1, characterized in that: The coupling agent includes a combination of one or more of a silane coupling agent, a titanium coupling agent, an aluminum coupling agent and a zirconium coupling agent.
4. The method for preparing large-sized amorphous soft magnetic composite powder according to claim 1, characterized in that: The plasma surface treatment includes one or more of oxygen plasma surface treatment, argon plasma surface treatment, and nitrogen plasma surface treatment.
5. The method for preparing large-sized amorphous soft magnetic composite powder according to claim 1, characterized in that: The pyrophosphate is sodium pyrophosphate or potassium pyrophosphate.
6. The method for preparing large-sized amorphous soft magnetic composite powder according to claim 1, characterized in that: The solvent includes one or more of water, PVP, and alcohol.
7. The method for preparing large-sized amorphous soft magnetic composite powder according to claim 1, characterized in that: The coupling agent surface treatment comprises: adding 3-aminopropyltriethoxysilane to a mixture of alcohol and water in a mass ratio of (2-10):1; magnetically stirring at a constant temperature of 50-60°C for 20-30 minutes, then adding the powders after the plasma surface treatment respectively, continuing to stir for 20-30 minutes, and keeping the temperature at 50-100°C for 30 minutes to 60 minutes.
8. The method for preparing large-sized amorphous soft magnetic composite powder according to claim 1, characterized in that: The plasma surface treatment includes oxygen plasma surface treatment, and the oxygen plasma surface treatment includes: the radio frequency frequency of the plasma instrument is 12-15MHz, the output power range is 0-300W, the gas pressure is 50-100Pa, the oxygen flow rate is set to 100-200mL / mi, and the treatment time is 1min-30min.
9. The method for preparing large-sized amorphous soft magnetic composite powder according to claim 7, characterized in that: The mass ratio of the 3-aminopropyltriethoxysilane to the powder after plasma surface treatment is (1-10):
100.
10. The method for preparing large-sized amorphous soft magnetic composite powder according to claim 3, characterized in that: The silane coupling agent is selected from a combination of one or more of trimethacryloxypropyltrimethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, methacryloxytrimethoxysilane, 3-epoxypropylenetrimethoxysilane and 3-aminopropyltriethoxysilane.
Citation Information
Patent Citations
Soft magnetic composite material and preparation method thereof
CN104036905A
Method for coating metal magnetic powder on soft magnetic ferrites and method for preparing soft magnetic composite materials
CN104550940A