A surface integrity control method for large-size mirror molds manufactured by laser additive manufacturing
Through layer-by-layer laser additive manufacturing and laser surface integral remelting combined with CNC machining and polishing technology, the defect problem in surface processing of large-size mirror molds produced by laser additive manufacturing has been solved, and the surface integrity and hardness uniformity of high-end molds have been improved. .
Patent Information
- Application Number
- CN202111228577.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-21
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-10-21
AI Technical Summary
Existing large-size mirror molds manufactured by laser additive manufacturing have macro- and micro-sized structural defects and periodic performance fluctuations during the surface processing process, resulting in surface roughness and defect problems, making it difficult to meet the surface integrity requirements of high-end molds.
Using layer-by-layer laser additive manufacturing and laser surface overall remelting technology, combined with CNC milling or grinding technology, through laser surface heat treatment and precision polishing, internal metallurgical defects and surface overall remelting are optimized to achieve surface roughness and hardness uniformity. promote.
It effectively suppresses surface cracks, textures, holes and other defects, improves the surface integrity of the mirror mold, the surface roughness reaches less than 30nm, and the hardness uniformity is significantly improved.
Smart Images

Figure CN116000311B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of additive manufacturing, and in particular to a surface integrity control method for a large-size mirror mold manufactured by laser additive manufacturing. Background Art
[0002] Mirror molds are widely used in aerospace, rail transportation, ocean and other fields. The existing mold manufacturing process is to cast / forge the initial steel billet, and then perform complex mechanical processing, including surface processing (such as milling, grinding, polishing, etc.) and internal flow channel structure processing. With the gradual improvement of related industries' requirements for mold size, quality, performance, etc., traditional manufacturing methods are difficult to meet the strong demand of related industries. Especially under the constraints of material constraints, structural constraints, cost and cycle constraints, traditional manufacturing and design methods are no longer applicable in many high-end mold manufacturing occasions.
[0003] Additive manufacturing technology has technical advantages such as direct forming of conformal cooling channels, net size forming of complex structures, functional gradient material structure, unconstrained forming size, and small heat input. It has broad application prospects in the manufacture of large molds and the repair of high-end molds. Compared with other molds, high-gloss mirror molds have higher requirements for their surface integrity, including high surface hardness and hardness uniformity, surface polishing quality, etc.
[0004] Since additive manufacturing technology uses laser to melt powder, the moving molten pool is formed in three-dimensional space through a point-line-surface method. The forming material is martensitic steel or martensitic stainless steel, etc. Its complex spatial thermal process history leads to periodic fluctuations in the organization, defects and performance of the additive forming mold in macro and micro scales. As a result, the martensite content, second phase distribution and defect characteristics in the matrix phase at different positions of the final surface may show characteristics different from those of traditional forging die steel.
[0005] In the subsequent grinding and polishing process, changes in surface morphology (surface roughness, surface defects) will inevitably occur. To control the surface integrity of additively manufactured mirror mold steel, it is necessary to control the solidification structure before machining (that is, from the material perspective) and also from the subsequent precision machining process. At present, compared with traditional manufacturing process mold steel, mirror mold steel manufactured by additive manufacturing is prone to various types of surface defects such as surface cracks, surface holes, surface texture, etc. in the subsequent grinding and polishing process. Summary of the invention
[0006] In view of the above-mentioned shortcomings that occur in the current surface processing process of large-size mirror molds manufactured by laser additive manufacturing, the purpose of the present invention is to provide a surface integrity control method for large-size mirror molds manufactured by laser additive manufacturing. This method realizes surface integrity control of large-size mirror molds by optimizing the internal metallurgical defect control method layer by layer during the additive manufacturing process, the overall laser surface remelting method after additive manufacturing, and the subsequent constant force / constant pressure floating polishing method. This method can improve the surface roughness of the molding surface, improve surface defects, and improve the uniformity of surface hardness.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] A surface integrity control method for a large-size mirror mold manufactured by laser additive manufacturing, the method uses martensitic stainless steel powder as a mold surface material (hardened layer), and manufactures a large-size mirror mold by laser additive manufacturing; the method specifically comprises the following steps:
[0009] (1) Performing layer-by-layer laser additive manufacturing, and performing interlayer remelting using a laser surface remelting process between adjacent layers;
[0010] (2) After laser additive manufacturing, the surface of the additively manufactured parts is rough-machined using CNC milling or grinding technology;
[0011] (3) remelting the sample after rough processing in step (2) by laser surface remelting process;
[0012] (4) After overall remelting, the sample surface is precisely processed using a grinding and polishing process.
[0013] The particle size of the martensitic stainless steel powder is 100-200 meshes, and the contents of elements such as S, P, and O in the martensitic stainless steel must be strictly controlled.
[0014] In step (1), the laser additive manufacturing process parameters are: laser power 2000-3000W, scanning speed 3-4.5mm / s, powder feeding rate <10g / min, and powder feeding gas flow rate 4-5L / min.
[0015] In the additive manufacturing process, high power density and low powder feeding rate should be used as much as possible to ensure that the powder fed into the molten pool is completely melted. Incomplete melting of the powder will inevitably cause internal shrinkage defects, which will be exposed in the subsequent mechanical processing process, thus affecting its surface integrity.
[0016] During the interlayer remelting in step (1), the Nth remelting and the N-1th remelting use different scanning paths, and the center point of the Nth remelting scanning path is the fusion line (overlap area) of the N-1th remelting, so that the defects distributed on the fusion line (overlap line position) can be remelted again.
[0017] During the interlayer remelting in step (1), powder is not fed, and surface remelting is performed layer by layer. The heat input during the interlayer remelting is lower than the heat input during laser additive manufacturing. The scanning speed during the interlayer remelting is higher than the scanning speed during laser additive manufacturing. The same circular spot size is used during the interlayer remelting and laser additive manufacturing.
[0018] In step (2), rough machining uses as little cutting depth and lower feed speed as possible to avoid excessive plastic deformation of the surface and subsurface layers. It is worth noting that excessive damage caused by rough machining of parts (such as plastic deformation) will affect the integrity of the final surface.
[0019] In step (3), the overall surface remelting is performed by laser surface heat treatment, wherein: a long strip-shaped spot is used, and the remelting thickness is greater than 100 μm; and the scanning rate used for remelting should be greater than the scanning speed during interlayer remelting.
[0020] Step (4) surface grinding and polishing process is as follows: first, the existing mold surface grinding method is adopted, that is, 400#, 1000#, 1500#, 2000# sandpaper is used, and the surface of the part is ground by fixing the tool and moving the sandpaper; after grinding, a pneumatic polishing tool is used for grinding and polishing, and diamond polishing paste (9μm, 6μm, 1μm) is used in the grinding process. The polishing process should ensure that a relatively low rotation speed and contact force are used, and a pneumatic grinding tool is used. Precision polishing is performed through a grinding and polishing system. Polishing to a mirror surface state.
[0021] The surface roughness Ra value of the mirror mold prepared by the method is less than 30nm, and the Sa value and Sq value thereof are both less than 20nm as tested by AFM.
[0022] The advantages and beneficial effects of the present invention are:
[0023] 1. The surface integrity control method of the mirror mold proposed in the present invention can realize the manufacture of large-size mirror molds (effective mold surface size is at the level of plane surface), breaking through the bottleneck of the existing technology in the manufacture of large-size and super-large-size mirror molds.
[0024] 2. The surface roughness of the final mirror mold can reach below 30nm, and the hardness uniformity and hardness value of the mold surface can be improved.
[0025] 3. It can effectively suppress various surface defects such as cracks, textures, holes, etc. that occur in the subsequent surface fine processing process of additive manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 Flowchart of the surface integrity control method for additively manufactured mirror molds. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0028] The present invention adopts martensitic stainless steel material as the material of the profile area (hardened layer), firstly performs layer-by-layer laser additive manufacturing, and adopts a laser surface remelting process to perform interlayer remelting between adjacent layers, wherein the second remelting and the first remelting use different scanning paths, and the center point of the remelting scanning path is the fusion line (overlapping area) of the first remelting. After the above-mentioned method is used for additive manufacturing; a CNC milling / grinding process is used for surface rough machining, and then a second overall remelting is performed. After remelting, the surface is finely machined by a grinding and polishing process ( Figure 1 ). The method of the present invention specifically comprises the following steps:
[0029] 1. Additive manufacturing optimizes the internal metallurgical defect control method layer by layer: For mirror mold steel additive manufacturing, the surface area requires extremely high density, so the additive process needs to ensure a high power density. The overlap area is usually the gathering place of microscopic defects in additive forming. For the mirror mold surface area additive, after the additive layer is formed, the first remelting can be performed by laser remelting without powder feeding to ensure the internal metallurgical quality.
[0030] In the forming mirror mold steel material, in order to avoid the appearance of oxide impurities inside, the oxygen content in the forming atmosphere must be controlled at 20-50ppm. At the same time, the content of elements such as O, S, and P in the mold steel powder material must also be strictly controlled.
[0031] At the same time, in the specific forming process, a lower powder feeding rate and scanning rate are often used to ensure that all the powder fed into the molten pool is melted and the reactive and involved gases are fully released. Through process parameter control, external field, atmosphere control, multiple remelting and other treatments, defects with a scale of 50 to 200 μm are avoided.
[0032] For the first laser remelting, the scanning rate used is greater than that of the synchronous powder feeding additive process.
[0033] 2. Use a long strip light spot to scan the entire surface for a second overall surface remelting: Different from the circular light spot used in laser additive manufacturing, after the second surface remelting, the light spot change is achieved by changing the optical path. The use of a long strip light spot can greatly reduce the overlap area (fusion line) between adjacent paths. Multiple long strip light spots can be operated in parallel, so that the structure of the entire surface can be homogenized. The thickness of the second surface remelting layer is on the order of hundreds of microns, so it is necessary to perform the second surface remelting after mechanical processing of the part, that is, after CNC milling or initial grinding. Laser surface heat treatment can also improve the unevenness of the internal structure of the surface, especially due to the differences in the heat-affected zone structure and the structure at the fusion line position between adjacent scanning paths, which can significantly improve its surface hardness value and uniformity.
[0034] 3. Surface grinding and mirror polishing: Different from the traditional forging state organization, the additive manufacturing organization is a solidified organization, and there may be metallurgical defects of the μm level (generally 10-50μm) inside (possibly pores, shrinkage, oxides, etc.). During the fine grinding and polishing of the mold surface to a mirror state, it is necessary to ensure that excessive removal during the grinding and polishing process should be avoided as much as possible to avoid plastic deformation of the surface. In the subsequent polishing process, try to use a constant contact pressure or a constant pressure method.
[0035] In the subsequent mechanical processing (milling, grinding, etc.), the defects are exposed on the surface. In the actual polishing process, the defects are mostly part of the pores. As the subsequent polishing process proceeds, the polishing medium will enter the defect position. During the contact between the polishing medium and the deposition substrate, the defects will expand in the horizontal direction shown in the figure, and the final defect shape is flat. In addition, some second phases are also prone to fracture and separation from the substrate under high strain rate and large plastic deformation conditions, resulting in defects at this position.
[0036] The grinding process uses a moving grinding tool and a fixed mold surface to be machined. During the grinding process, it is necessary to avoid continuous processing at a local location, which may cause a rise in the temperature of the local location, and to avoid using excessive mechanical loads, which may cause a serious deterioration layer on the material surface.
[0037] Embodiment 1:
[0038] 1. Material composition (mass percentage) of martensitic stainless steel for mirror mold steel: Cr 15%, Ni 4.0%, Mo1.4%, Mn 0.6%, Si 1.3%, C 0.14%, B 0.7%, Fe as the balance. Powder particle size is 100-200 mesh. It should be noted that the content of S, P, O and other elements in the powder should be strictly controlled (the content of S, P, O is less than 0.15wt.%).
[0039] 2. Additive forming process parameter range: laser power: 2000-3000W; scanning speed: 3-4.5mm / s, powder feeding rate <10g / min, powder feeding gas flow: 4-5L / min. In the additive manufacturing process, high power density and low powder feeding rate should be used as much as possible to ensure that the powder fed into the molten pool is completely melted. Incomplete melting of the powder will inevitably cause shrinkage defects inside, which will be exposed in the subsequent mechanical processing process, thus affecting its surface integrity.
[0040] 3. First surface remelting process parameters: Surface remelting is performed layer by layer, using a lower heat input (power 1000-1500W) than the deposition process, and a higher scanning speed (scanning speed is 1.5 times the scanning speed of synchronous powder feeding additive manufacturing), and the same spot size. In order to remelt the defects distributed on the fusion line (overlap line position), the center point of the scanning path is the original overlap line position when the laser is remelted.
[0041] 4. Rough machining of part surface: Use CNC milling, grinding and other methods to rough machine the surface of the part after additive manufacturing. Rough machining (milling, etc.) should use as little cutting depth and lower feed speed as possible to avoid excessive plastic deformation of the surface and subsurface layers. It is worth noting that excessive damage caused by rough machining of parts (such as plastic deformation, etc.) will affect the integrity of the final surface.
[0042] 5. Surface remelting after machining: Use laser surface heat treatment, that is, use a long strip spot (the spot size used in this test is a 30mm*1mm long strip spot) to perform laser heat treatment (remelting) on the surface after milling and grinding, and the remelting thickness is 100-500μm. The scanning rate during the long strip spot remelting should be greater than the scanning speed of laser deposition and the first laser remelting (circular spot).
[0043] 6. Surface grinding and polishing: First, the existing mold surface grinding method is used, that is, 400#, 1000#, 1500#, 2000# sandpaper is used, and the surface is ground by fixing the tool and moving the sandpaper. After grinding, a pneumatic polishing tool is used for grinding and polishing. Diamond polishing paste (9μm, 6μm, 1μm) is used in the grinding process. The polishing process should ensure a relatively low speed and contact force, and pneumatic grinding tools are used. Precision polishing is performed by installing a force feedback controlled grinding and polishing system. Polish to a mirror surface state.
[0044] The surface roughness of the mirror mold prepared by the above method was tested by a handheld hardness tester. The surface roughness Ra value was in the range of 15 to 30 nm. The local Sa value and Sq value tested by AFM were both 5 to 16 nm.
Claims
1. A method for controlling the surface integrity of a large-size mirror mold manufactured by laser additive manufacturing, characterized in that: The method uses martensitic stainless steel powder as the mold surface material and manufactures a large-size mirror mold by laser additive manufacturing. The method specifically includes the following steps: (1) A synchronous powder feeding additive process is used for layer-by-layer laser additive manufacturing, and a laser surface remelting process is used between adjacent layers to perform interlayer remelting. The Nth remelting and the N-1th remelting use different scanning paths, and the center point of the Nth remelting scanning path is the fusion line of the N-1th remelting, so that the defects distributed on the fusion line can be remelted; (2) After laser additive manufacturing, the surface of the additively manufactured parts is rough-machined using CNC milling or grinding technology; (3) The parts rough-machined in step (2) are subjected to overall remelting by laser surface remelting process; (4) After overall remelting, the surface of the parts is precisely processed by grinding and polishing; In step (1), during interlayer remelting, powder is not fed, and surface remelting is performed layer by layer. The heat input during interlayer remelting is lower than the heat input during the synchronous powder feeding additive process. The scanning speed during interlayer remelting is higher than the scanning speed during the synchronous powder feeding additive process. The same circular spot size is used during interlayer remelting and the synchronous powder feeding additive process. In step (3), the overall surface remelting is performed by laser surface heat treatment, wherein: a long strip-shaped spot is used, the remelting thickness is greater than 100 μm; and the scanning rate used for remelting is greater than the scanning speed during interlayer remelting.
2. The surface integrity control method for laser additive manufacturing of a large-size mirror mold according to claim 1, characterized in that: The particle size of the martensitic stainless steel powder is 100-200 meshes.
3. The surface integrity control method for laser additive manufacturing of a large-size mirror mold according to claim 1, characterized in that: In step (1), the synchronous powder feeding additive process parameters are: laser power 2000~3000W, scanning speed 3~4.5mm / s, powder feeding rate <10g / min, and powder feeding gas flow rate 4~5L / min.
4. The surface integrity control method for laser additive manufacturing of a large-size mirror mold according to claim 1, characterized in that: Step (4) The surface grinding and polishing process is as follows: after grinding, a pneumatic polishing tool is used to perform grinding and polishing. Diamond polishing paste is used in the polishing process. Precision polishing is performed through a grinding and polishing system until the surface is in a mirror state.