A gradient zirconium oxide ceramic block and preparation method thereof
By molding a single yttria-content zirconia powder in a hypergravity environment, the problem of simultaneous optimization of the optical transparency and mechanical properties of gradient zirconia ceramic blocks in dental restoration materials has been solved, and continuous gradient changes in optical transparency and process simplification have been achieved. It avoids warping phenomenon and is suitable for mass production.
Patent Information
- Application Number
- CN202210279388.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-03-21
AI Technical Summary
It is difficult to simultaneously optimize the optical transparency and mechanical properties of gradient zirconia porcelain blocks in dental restorative materials using existing technology, and the multi-layer laying process is cumbersome and prone to warping.
Zirconia powder with a single yttria content is used for molding in a hypergravity environment. The gradient distribution of the powder in the ceramic block is achieved through the deposition speed of different particle sizes, ensuring the continuous gradient change in the optical transparency of the zirconia ceramic block after sintering. And avoid the problem of inconsistent shrinkage caused by different stabilizer contents.
It achieves the continuity of the optical transparency gradient of the zirconia porcelain blocks in dental restorations, simplifies the process, reduces costs, avoids warping, and has performance close to that of natural teeth.
Smart Images

Figure GDA0004962948950000041 
Figure GDA0004962948950000081 
Figure GDA0004962948950000082
Abstract
Description
Technical Field
[0001] The invention relates to the field of ceramic materials for dental restorations, and in particular to a gradient zirconium oxide ceramic block and a preparation method thereof. Background Art
[0002] Zirconia ceramics have reliable biological stability and excellent mechanical properties. Cutting zirconia ceramics is one of the main methods in the field of dental restorative materials. Pure zirconia ceramics cannot be used directly and stabilizers must be added. Commonly used stabilizers include rare earth metal oxides such as yttrium oxide, and alkaline earth metal oxides such as magnesium oxide and calcium oxide. The stabilizer in zirconia ceramics for dentures is mainly yttrium oxide.
[0003] Related technology Transparent Nanometric Cubic and Tetragonal Zirconia Obtained by High-Pressure Pulsed Electric Current Sintering, Adv. Funct. Mater., 17 (2007), 3267 records that zirconia ceramics mainly have three crystal structures: monoclinic phase, tetragonal phase, and cubic phase, among which tetragonal phase and cubic phase are the two main crystal structures of zirconia ceramics for dentures. The content of yttria will affect the crystal structure of zirconia, and then affect the optical transparency and mechanical strength of the prepared zirconia ceramic blocks for dentures. When the molar percentage of yttria in yttrium-stabilized zirconia powder is about 3%, zirconia is tetragonal; when the molar percentage of yttria in yttrium-stabilized zirconia powder reaches about 8%, all zirconia is cubic; the optical transparency of cubic zirconia ceramics is better than that of tetragonal zirconia ceramics, but the mechanical strength of cubic zirconia is not as good as that of tetragonal zirconia ceramics.
[0004] The optical transparency of natural teeth shows a gradient from the root to the cutting end. The preparation of gradient zirconia ceramic blocks for dentures is one of the important directions in the field of ceramic dentures at this stage. It can simulate the gradient effect of the optical transparency of natural teeth. At present, the relevant technology can realize the preparation of gradient zirconia by stacking yttrium-stabilized zirconia powders with different stabilizer contents multiple times, but the transparency between the obtained porcelain layers is discontinuous, and the sintering power of zirconia with different stabilizer contents between different porcelain layers is different. The warping phenomenon caused by different shrinkage of the material is prone to occur during the stacking sintering, resulting in the need to adjust the overall process flow according to the properties of the porcelain layer. The process is cumbersome and not conducive to actual production. In addition to being affected by the content of yttrium oxide, the transparency of zirconia ceramics is also affected by the grain size in zirconia ceramics. However, the grading of powders of different sizes cannot be achieved by simple powder laying technology. Summary of the invention
[0005] In order to solve the defects existing in the related art, the purpose of the present invention is to provide a gradient zirconia ceramic block and its preparation method. Different from the existing method of laying yttria-stabilized zirconia powder with different contents layer by layer, the present invention uses zirconia with a single yttria content as raw material, and uses the different deposition rates of particles of different sizes in a supergravity environment to achieve a gradient distribution of the particle size of the powder in the ceramic block; after the prepared zirconia ceramic block is crystallized and sintered, a zirconia ceramic with a gradient change in optical transparency in at least one spatial dimension is obtained, and at the same time, the yttria content does not change in the dimension in which the optical transparency changes in a gradient.
[0006] The purpose of the present invention is achieved through the following specific technical solutions:
[0007] On the one hand, the present invention provides a gradient zirconia ceramic block for dental use, wherein the zirconia ceramic block is formed by a zirconia slurry through a supergravity method, wherein the zirconia slurry contains yttrium-stabilized zirconia powder, an additive and water, wherein the volume percentage of the yttrium-stabilized zirconia powder in the zirconia slurry is 10 to 55%, the volume percentage of the additive in the zirconia slurry is 0.05 to 10%, and the remainder is water.
[0008] As mentioned above: if too much stabilizer is used, the content of tetragonal zirconium oxide will be reduced, and the mechanical properties of the ceramic block will be insufficient; if too little stabilizer is used, the content of cubic zirconium oxide will be too low, and the light transmittance of the ceramic block will be reduced. For this reason, the present invention uses yttrium oxide as a stabilizer in yttrium-stabilized zirconia powder, and the molar percentage of yttrium oxide in the yttrium-stabilized zirconia powder is 2.5-5.5%.
[0009] On the other hand, the zirconium oxide ceramic block is used to make dental restorations.
[0010] On the other hand, a method for preparing the aforementioned zirconium oxide ceramic block is provided, wherein the zirconium oxide slurry is formed by a supergravity method, and specifically comprises the following steps:
[0011] 1) Yttrium-stabilized zirconium oxide powder with yttrium oxide as a stabilizer is used as a main raw material, mixed with additives and deionized water to prepare zirconium oxide slurry;
[0012] 2) separating the solid phase material in the zirconium oxide slurry under supergravity conditions;
[0013] 3) drying the solid phase material to obtain a zirconia ceramic block blank;
[0014] 4) Performing shape processing on the zirconia ceramic block blank to obtain the zirconia ceramic block.
[0015] Optionally, in step 1), the volume percentage of the yttrium-stabilized zirconia powder in the zirconia slurry is 10-55%. If the volume fraction of the yttrium-stabilized zirconia powder is too low, the thickness of the zirconia ceramic block prepared after gravity-accelerated sedimentation cannot meet the requirements of the actual processing size; if the volume fraction is too high, the yttrium-stabilized zirconia powder in the slurry will be difficult to disperse and prone to sedimentation. For this reason, the volume percentage range of the yttrium-stabilized zirconia powder in the prepared zirconia slurry of the present invention is 10-55%, and more preferably 25-50%.
[0016] Optionally, in step 1), the volume percentage of the additive in the zirconia slurry is 0.05-10%.
[0017] Optionally, the additive is at least one of ethylene glycol, polyethylene glycol, glycerol, glucose, polydextrose, sucrose, ethylene oxide, citric acid, and polyvinyl alcohol.
[0018] Optionally, in step 2), the supergravity condition is: the range of the supergravity coefficient is 1000-10000g, where g is the acceleration of gravity. If the supergravity coefficient is too high, the cost of the required preparation equipment will increase; if the supergravity coefficient is too low, the solid phase components in the slurry cannot be completely settled. For this reason, the range of the supergravity condition in step 2) of the present invention is 1000-10000g, preferably 2000-7000g.
[0019] Optionally, in step 3), the drying conditions are: humidity range is 40-90%, temperature range is 15-80°C. Too high drying temperature will cause the water inside the ceramic block to evaporate too quickly and crack; too low temperature will take a long time to dry, prolonging the process time. Therefore, the humidity range of the drying in step 3) of the present invention is 40-90%, and the temperature range is 15-80°C; the more preferred humidity range is 60-80%, and the temperature range is 20-70°C.
[0020] Optionally, in step 3), the magnification factor of the zirconia ceramic block blank is in the range of 1.195 to 1.255.
[0021] The present invention has the following beneficial effects:
[0022] 1. The present invention utilizes the difference in sedimentation speed of powders of different particle sizes under a hypergravity environment to obtain a zirconium oxide ceramic block for dentures with a natural continuous gradient distribution of large particles at the bottom and small particles at the top; the optical transparency gradient of the zirconium oxide ceramic obtained after crystallization and sintering is continuous, and the performance is more consistent with that of natural teeth.
[0023] 2. In the selection of raw materials, each zirconium oxide ceramic block of the present invention uses only one content of yttrium oxide as a stabilizer yttrium stabilized zirconium oxide powder, the raw material composition is simple, and multiple raw material components are not required.
[0024] 3. The present invention not only saves the powder spreading process of multiple layers of raw materials, but also prevents warping caused by different shrinkage due to different stabilizer contents during sintering.
[0025] 4. Compared with the traditional preparation method of gradient zirconia ceramic blocks, the preparation process of the present invention is simple, low-cost, and suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention, but do not constitute a limitation of the present invention.
[0027] Figure 1 This is a sample photo of the dental gradient zirconia ceramic block prepared in Example 1 after crystallization and sintering;
[0028] Figure 2 The electron microscope photograph of the microstructure of the top surface of the zirconia ceramic block obtained in step 4) of Example 1;
[0029] Figure 3 This is an electron microscope photograph of the microstructure of the lower surface of the bottom end of the ceramic block obtained in step 4) of Example 1. DETAILED DESCRIPTION
[0030] Unless otherwise specified, the sources of the reagents used in the specific embodiments of the present invention can be purchased from the market.
[0031] Explanation of the names involved in the present invention:
[0032]
[0033] The yttrium-stabilized zirconia powder involved in the present invention refers to zirconia powder with yttrium oxide as a stabilizer.
[0034] The zirconia ceramic block of the specific embodiment of the present invention is formed by zirconia slurry through a supergravity method. The zirconia slurry contains yttrium-stabilized zirconia powder, additives and water. The volume percentage of the yttrium-stabilized zirconia powder in the zirconia slurry is 10-55%. As an example, it can be 10%, 20%, 30%, 40%, 50%, 55% and the like. When the content is lower than 10% or higher than 55%, the solid phase material is prone to stratification and cracking during the drying process. When the content of the additive is lower than 0.05% or higher than 10%, the solid phase material is prone to cracking during the drying process, and the transparency of the obtained zirconia ceramic block is reduced after sintering. The rest is water, that is, the total volume fraction of the yttrium-stabilized zirconia powder, additives and water is 100%.
[0035] In the zirconia ceramic block of the specific embodiment of the present invention, the yttrium-stabilized zirconia powder uses yttrium oxide as a stabilizer; the total content of the stabilizer in the yttrium-stabilized zirconia powder is 2.5-5.5% by mole percentage.
[0036] The method for preparing a zirconium oxide ceramic block according to a specific embodiment of the present invention specifically comprises the following steps:
[0037] 1) Yttrium-stabilized zirconium oxide powder with yttrium oxide as a stabilizer is used as a main raw material, mixed with additives and deionized water to prepare zirconium oxide slurry;
[0038] 2) separating the solid phase material in the zirconium oxide slurry under supergravity conditions;
[0039] 3) drying the solid phase material to obtain a preformed zirconia ceramic block;
[0040] 4) Performing shape processing on the zirconia ceramic block blank to obtain the dental gradient zirconia ceramic block.
[0041] In some specific embodiments, the method for preparing the zirconium oxide ceramic block may be:
[0042] 1) Yttrium-stabilized zirconia powder with a stabilizer content of 2.5 to 5.5 mol% is used as the main raw material, the volume percentage of the yttrium-stabilized zirconia powder in the zirconia slurry is 10 to 55%, the volume percentage of the additive in the zirconia slurry is 0.05 to 10%, and the rest is deionized water, and they are mixed to prepare a zirconia slurry;
[0043] 2) separating the solid phase material in the zirconia slurry prepared in step 1) under supergravity conditions with a supergravity coefficient of 1000 to 10000 g;
[0044] 3) Drying the solid phase material obtained in step 2) to obtain a zirconia ceramic block blank; the drying humidity range is 40-90% and the temperature range is 15-80° C.;
[0045] 4) The dried zirconia ceramic block blank obtained in step 3) is processed to obtain a gradient zirconia ceramic block for dental use, wherein the magnification factor of the zirconia ceramic block is in the range of 1.195 to 1.255.
[0046] The present invention takes Example 1 as an example, and provides sample photos of dental gradient zirconia ceramic blocks after crystallization and sintering, as well as electron microscope photos of the microstructure of the upper surface of the top of the zirconia ceramic block obtained by the ultra-gravity forming method, and other embodiments and electron microscope photos of the microstructure of the lower surface of the bottom of the ceramic block. A person skilled in the art can directly and unambiguously determine the contents of other embodiments of the present invention by the same method.
[0047] Example 1
[0048] 1) Yttrium-stabilized zirconia powder with an yttrium oxide content of 2.5 mol% is used as the main raw material, the volume percentage of the yttrium-stabilized zirconia powder in the zirconia slurry is 40%, the volume percentage of the additive in the zirconia slurry is 0.05%, and the rest is deionized water, and they are mixed to prepare a zirconia slurry;
[0049] 2) separating the solid phase material in the zirconia slurry prepared in step 1) under supergravity conditions with a supergravity coefficient of 10000 g;
[0050] 3) Drying the solid phase material obtained in step 2) to obtain a zirconia ceramic block blank; the drying humidity is 80% and the temperature is 20° C.;
[0051] 4) The dried zirconia ceramic block blank obtained in step 3) is processed to obtain a gradient zirconia ceramic block for dental use, with a magnification factor of 1.195.
[0052] Depend on Figure 1 It can be seen that the optical transparency of the cylindrical sample presents a gradient change visible to the naked eye from the top to the bottom, and the gradient change is continuous and natural.
[0053] Depend on Figure 2 and Figure 3 It can be seen that the grain size of the upper surface with better optical transparency is significantly smaller than the grain size of the lower surface with lower optical transparency.
[0054] Example 2
[0055] 1) Yttrium-stabilized zirconia powder with an yttrium oxide content of 2.5 mol% is used as a main raw material, the volume percentage of the yttrium-stabilized zirconia powder in the zirconia slurry is 55%, the volume percentage of the additive in the zirconia slurry is 3.23%, and the rest is deionized water, and they are mixed to prepare a zirconia slurry;
[0056] 2) separating the solid phase material in the zirconia slurry prepared in step 1) under supergravity conditions with a supergravity coefficient of 8500 g;
[0057] 3) Drying the solid phase material obtained in step 2) to obtain a zirconia ceramic block blank; the drying humidity is 80% and the temperature is 35° C.;
[0058] 4) The dried zirconia porcelain obtained in step 3)
[0059] The block blank is processed to obtain a gradient machinable zirconia ceramic block for dental use with an enlargement factor of 1.207.
[0060] Example 3
[0061] 1) Yttrium-stabilized zirconia powder containing 3.5 mol% of yttrium oxide is used as the main raw material, the volume percentage of the yttrium-stabilized zirconia powder in the zirconia slurry is 35%, the volume percentage of the additive in the zirconia slurry is 4.95%, and the rest is deionized water, and they are mixed to prepare a zirconia slurry;
[0062] 2) separating the solid phase material in the zirconia slurry prepared in step 1) under supergravity conditions with a supergravity coefficient of 7200 g;
[0063] 3) Drying the solid phase material obtained in step 2) to obtain a preformed zirconia ceramic block; the drying humidity is 65% and the temperature is 30° C.;
[0064] 4) The dried zirconia ceramic block blank obtained in step 3) is processed to obtain a gradient machinable zirconia ceramic block for dental use, with an enlargement factor of 1.211.
[0065] Example 4
[0066] 1) Yttrium-stabilized zirconia powder containing 4.0 mol% of yttrium oxide is used as the main raw material, the volume percentage of the yttrium-stabilized zirconia powder in the zirconia slurry is 25%, the volume percentage of the additive in the zirconia slurry is 6.72%, and the rest is deionized water, and they are mixed to prepare a zirconia slurry;
[0067] 2) separating the solid phase material in the zirconia slurry prepared in step 1) under supergravity conditions with a supergravity coefficient of 5500 g;
[0068] 3) Drying the solid phase material obtained in step 2) to obtain a zirconia ceramic block blank; the drying humidity is 60% and the temperature is 30° C.;
[0069] 4) The dried zirconia ceramic block blank obtained in step 3) is subjected to shape processing to obtain a gradient machinable zirconia ceramic block for dental use, with an enlargement factor of 1.226.
[0070] Example 5
[0071] 1) Yttrium-stabilized zirconia powder containing 4.5 mol% of yttrium oxide is used as the main raw material, the volume percentage of the yttrium-stabilized zirconia powder in the zirconia slurry is 20%, the volume percentage of the additive in the zirconia slurry is 8.45%, and the rest is deionized water, and they are mixed to prepare a zirconia slurry;
[0072] 2) separating the solid phase material in the zirconia slurry prepared in step 1) under supergravity conditions with a supergravity coefficient of 4300 g;
[0073] 3) Drying the solid phase material obtained in step 2) to obtain a preformed zirconia ceramic block; the drying humidity is 45% and the temperature is 40° C.;
[0074] 4) The dried zirconia ceramic block blank obtained in step 3) is subjected to shape processing to obtain a gradient machinable zirconia ceramic block for dental use, with an enlargement factor of 1.235.
[0075] Example 6
[0076] 1) Yttrium-stabilized zirconia powder containing 5.0 mol% of yttrium oxide is used as the main raw material, the volume percentage of the yttrium-stabilized zirconia powder in the zirconia slurry is 25%, the volume percentage of the additive in the zirconia slurry is 9.27%, and the rest is deionized water, and they are mixed to prepare a zirconia slurry;
[0077] 2) separating the solid phase material in the zirconia slurry prepared in step 1) under ultra-gravity conditions with an ultra-gravity coefficient of 2900 g;
[0078] 3) Drying the solid phase material obtained in step 2) to obtain a zirconia ceramic block blank; the drying humidity is 40% and the temperature is 30° C.;
[0079] 4) The dried zirconia ceramic block blank obtained in step 3) is subjected to shape processing to obtain a gradient machinable zirconia ceramic block for dental use, with an enlargement factor of 1.248.
[0080] Example 7
[0081] 1) Yttrium-stabilized zirconia powder containing 5.5 mol% of yttria is used as the main raw material, the volume percentage of the zirconia powder in the zirconia slurry is 10%, the volume percentage of the additive in the zirconia slurry is 10%, and the rest is deionized water, and they are mixed to prepare a zirconia slurry;
[0082] 2) separating the solid phase material in the zirconia slurry prepared in step 1) under supergravity conditions with a supergravity coefficient of 1000 g;
[0083] 3) Drying the solid phase material obtained in step 2) to obtain a preformed zirconia ceramic block; the drying humidity is 40% and the temperature is 80° C.;
[0084] 4) The dried zirconia ceramic block blank obtained in step 3) is subjected to shape processing to obtain a gradient machinable zirconia ceramic block for dental use, with an enlargement factor of 1.255.
[0085] The dosage of raw materials and process parameters of each embodiment are shown in Table 1.
[0086] Table 1 Amounts of raw materials and process parameters of Examples 1 to 7
[0087]
[0088] The additives in each embodiment of the present invention are at least one or a combination of polyethylene glycol, ethylene glycol, glycerol, glucose, polydextrose, sucrose, citric acid, ethylene oxide, and polyvinyl alcohol. The composition and content of the additives in each embodiment are shown in Table 2.
[0089] Table 2 Composition and content of additives in Examples 1 to 7
[0090]
Claims
1. A gradient machinable zirconia ceramic block for dental use, characterized in that: The zirconia ceramic block is formed by a zirconia slurry through a supergravity method, wherein the zirconia slurry contains yttrium-stabilized zirconia powder, an additive and water, wherein the volume percentage of the zirconia powder in the zirconia slurry is 10-55%, the volume percentage of the additive in the zirconia slurry is 0.05-10%, and the rest is water; The method for preparing the zirconium oxide ceramic block comprises the following steps: 1) Yttrium-stabilized zirconium oxide powder is used as the main raw material, mixed with additives and deionized water to prepare zirconium oxide slurry; 2) separating the solid phase material in the zirconium oxide slurry under supergravity conditions; 3) Drying the solid phase material to obtain a preformed zirconia ceramic block; 4) performing shape processing on the zirconia ceramic block blank to obtain the zirconia ceramic block; In step 1), the volume percentage of the yttrium-stabilized zirconia powder in the zirconia slurry is 10-55%; The yttrium-stabilized zirconia powder uses a certain amount of yttrium oxide as a stabilizer; the molar percentage of the yttrium oxide in the yttrium-stabilized zirconia powder is 2.5-5.5%; In step 1), the additive is at least one of ethylene glycol, polyethylene glycol, glycerol, glucose, polydextrose, sucrose, ethylene oxide, citric acid, and polyvinyl alcohol; In step 2), the hypergravity condition is: the range of the hypergravity coefficient is 1000~10000 g, where g is the gravitational acceleration; In step 3), the drying conditions are: humidity range is 40-90%, temperature range is 15-80°C; In step 3), the magnification factor of the zirconia ceramic block ranges from 1.195 to 1.
255.
2. A dental gradient machinable zirconia ceramic block as claimed in claim 1 for use in making dental restorations.
3. A method for preparing a dental gradient machinable zirconia ceramic block according to claim 1, characterized in that: The zirconium oxide slurry is formed by a supergravity method, which specifically includes the following steps: 1) Yttrium-stabilized zirconium oxide powder with yttrium oxide as a stabilizer is used as the main raw material, mixed with additives and deionized water to prepare zirconium oxide slurry; 2) separating the solid phase material in the zirconium oxide slurry under supergravity conditions; 3) Drying the solid phase material to obtain a preformed zirconia ceramic block; 4) Performing shape processing on the zirconia ceramic block blank to obtain the gradient machinable zirconia ceramic block for dental use.
4. The method for preparing a dental gradient machinable zirconia ceramic block according to claim 3, characterized in that: In step 1), the volume percentage of the additive in the zirconium oxide slurry is 0.05-10%.