Elastic yarn and preparation method thereof
Through the method of parallel twisting of bicomponent fiber filaments and spandex filaments, the existing elastic yarn preparation complex and low strength problems are solved, and yarn preparation with high strength, high elasticity and good mechanical properties is achieved, which avoids the It eliminates hairiness and entanglement phenomena, and improves the ductility and acid and alkali resistance of the yarn.
Patent Information
- Application Number
- CN202310067176.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-06
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-02-06
AI Technical Summary
The existing elastic yarn preparation methods are complex and prone to problems such as hairiness and entanglement during the interweaving process, resulting in low yarn strength and poor elasticity.
Parallel bicomponent fiber filaments and spandex filaments are twisted in parallel, and elastic yarns are prepared through polymer A and polymer A* with different melt indexes. The mechanical properties of the parallel bicomponent fiber filaments and the properties of spandex filaments are used. The elastic properties are stimulated by twisting and stretching to form high-strength, high-elastic yarns.
It achieves high strength, high elasticity, good mechanical properties and processability, avoids hairiness and entanglement, and the yarn has good ductility, acid and alkali resistance and soft feel.
Smart Images

Figure CN116043383B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of yarn filaments, in particular to an elastic yarn and a preparation method thereof. Background Art
[0002] Spandex is a type of elastic fiber filament, known for its excellent elasticity and recovery properties, making it a popular choice among consumers. Spandex is not typically used directly, but is often processed with other materials to create stretch yarns with excellent stretchability, elastic recovery, and bulk.
[0003] Knitted and woven fabrics made from elastic yarns offer comfort, aesthetics, and warmth. Traditional elastic yarns, primarily core-spun, covered, and wrapped yarns, have a promising market. However, existing elastic yarn production methods are complex. Furthermore, due to the inherent structural and elastic properties of elastic yarns, these yarns are prone to hairiness and entanglement during interweaving, further contributing to a loss of elasticity and strength, resulting in low strength and elasticity in the resulting elastic yarns. Summary of the Invention
[0004] The object of the present invention is to provide an elastic yarn and a preparation method thereof, wherein the obtained elastic yarn has high strength and good elasticity.
[0005] To this end, the present invention provides an elastic yarn, comprising at least one parallel bicomponent fiber filament and at least one spandex filament twisted in parallel, wherein the parallel bicomponent fiber filament comprises polymer A and polymer A*, wherein polymer A and polymer A* are of the same type of polyolefin material, the melt index of polymer A and polymer A* differs by more than 10, and the mass ratio of polymer A to polymer A* is 1:(0.1-5).
[0006] Preferably, the diameter of the parallel bicomponent fiber filaments is 12 μm-30 μm.
[0007] Preferably, the specifications of the spandex filaments are distributed in the range of 20-140D.
[0008] Preferably, the polyolefin material includes one of polypropylene (PP), polyethylene (PE), polyamide (PA), and polyester (PET).
[0009] Preferably, the melt index of the polymer A is 20-40, and the melt index of the polymer A* is 30-100.
[0010] The present invention also provides a method for preparing the elastic yarn, comprising:
[0011] (1) preparing the parallel bicomponent fiber filaments:
[0012] The polymer A and the polymer A* were respectively fed into the barrels on both sides of the spunbond machine, and the temperature of the front zone was set to 210°C, and the temperature of the back zone and the spinneret was set to 230°C;
[0013] The polymer A and the polymer A* are sequentially passed through a screw extruder, a metering pump, and a filament separator from a barrel, and then merged at a spinneret hole, and are drawn and wound onto a bobbin to obtain parallel bicomponent fiber filaments;
[0014] (2) preparing the elastic yarn:
[0015] Parallel bicomponent fiber filaments and spandex filaments with specifications of 20-140D are selected for doubling, and the doubling is placed in a doubling and twisting machine for parallel twisting to obtain stretch-activated elastic yarns.
[0016] Preferably, in step (1), the extrusion speed is 0.1-0.5 g / h / min, and the spinning speed is 50-100 m / min.
[0017] Preferably, in step (2), the number of the parallel bicomponent fiber filaments is 2-10, and the number of the spandex filaments is 1-3.
[0018] Preferably, in step (2), the twist of the elastic yarn is 80-200 twists / 10cm.
[0019] Preferably, in step (2), the specifications of the spandex filaments are distributed in the range of 20-140D.
[0020] Compared with the prior art, the advantages and positive effects of the present invention are: the present invention provides an elastic yarn and a preparation method thereof, the elastic yarn comprising at least one parallel bicomponent fiber filament and at least one spandex filament twisted in parallel, the parallel bicomponent fiber filament comprising polymer A and polymer A*, the polymer A and the polymer A* being of the same type of polyolefin material, the melt index of the polymer A and the polymer A* differing by more than 10, and the mass ratio of the polymer A to the polymer A* being 1:(0.1-5). (1) Benefiting from the good mechanical properties of the parallel bicomponent fiber filaments themselves, the prepared elastic yarn also has good mechanical properties; the parallel bicomponent fiber filaments and the spandex filaments are not prone to hairiness, mutual entanglement, etc. during the interweaving process, and the obtained elastic fiber has high strength and good elasticity; (2) The twisted yarn obtained after the parallel bicomponent fiber filaments and the spandex filaments are twisted in parallel is similar to the ordinary twisted yarn in morphology, can be processed by ordinary weaving process, and has good processability; (3) In the stretch-induced elastic yarn, the spandex is in a twisted state, which can fix the silk loops formed by the stretched curled fibers, and the silk loops are firm and not easy to fall apart, and have high strength; (4) The stretch-induced elastic yarn has excellent properties such as good ductility, elasticity, acid and alkali resistance, sweat resistance, etc., and feels soft. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram of the structure of elastic yarn obtained by twisting parallel bicomponent fiber filaments and spandex;
[0022] Figure 2 Schematic diagram of the structure of a stretched and curled elastic yarn;
[0023] Reference numerals: 1 spandex filament; 2 parallel bicomponent fiber filament. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive and should not be used to limit the scope of protection of the present invention.
[0025] The elastic yarn of the present invention comprises at least one parallel bicomponent fiber filament and at least one spandex filament twisted in parallel, wherein the parallel bicomponent fiber filament comprises polymer A and polymer A*, polymer A and polymer A* are of the same type of polyolefin material, the melt index of polymer A and polymer A* differs by more than 10, and the mass ratio of polymer A to polymer A* is 1:(0.1-5).
[0026] The polymer A and polymer A* of the present invention are similar polyolefins and are highly similar. Therefore, they are not prone to fiber opening during subsequent processing. Since similar polyolefins have extremely low moisture regain, they do not need to be dried before use.
[0027] The parallel bicomponent fiber filaments of the present invention are prepared from two polyolefins with different melt indices. The melt indices of polymer A and polymer A* differ by more than 10. Polyolefins with different melt indices are distributed on both sides of each filament. Since the melt indices of the polyolefins on both sides of each filament are different, the shrinkage rates of the polyolefins with different melt indices are also different during the cooling and stretching process, resulting in obvious curling of the filaments. Therefore, the prepared parallel bicomponent fiber filaments have the characteristics of three-dimensional curling, high elasticity, high bulkiness, high filtration efficiency, high porosity, etc.
[0028] The polyolefin material includes one of polypropylene (PP), polyethylene (PE), polyamide (PA), and polyester (PET).
[0029] The diameter of the parallel two-component fiber filament is 12μm-30μm. After stretching, it has the characteristics of three-dimensional curling, high elasticity, high bulkiness, high filtration efficiency, and high porosity.
[0030] The fineness specifications of the spandex filaments are distributed in the range of 20-140D, which is conducive to making the prepared parallel bicomponent fiber filaments have the characteristics of three-dimensional curling, high elasticity, high bulkiness, etc.
[0031] The melt index of polymer A is 20-40, and the melt index of polymer A* is 30-100. During the cooling and stretching process, the shrinkage rates of polyolefins with different melt indexes are also different, resulting in obvious curling of the filaments. Therefore, the prepared parallel bicomponent fiber filaments have the characteristics of three-dimensional curling, high elasticity, and high fluffiness.
[0032] The preparation method of the elastic yarn of the present invention comprises:
[0033] (1) Preparation of parallel bicomponent fiber filaments:
[0034] Polymer A and polymer A* were respectively fed into the two barrels of the spunbond machine. The front zone temperature was set to 210°C, the rear zone and spinneret temperature was set to 230°C, the extrusion speed was 0.1-0.5 g / h / min, and the spinning speed was 50-100 m / min.
[0035] Polymer A and polymer A* are fed from the barrel through a screw extruder, a metering pump, and a filament separator in sequence, and then merged at the spinneret. After being drawn and wound onto a bobbin, parallel bicomponent fiber filaments are obtained.
[0036] (2) preparing the elastic yarn:
[0037] 2-10 parallel bicomponent fiber filaments and 1-3 spandex filaments with a specification of 20-50D are selected for parallel yarn drawing, and the parallel yarns are placed in a parallel twisting machine for parallel twisting to obtain stretch-activated elastic yarn, and the twist of the obtained elastic yarn is 80-200 twists / 10cm.
[0038] The advantages and positive effects of the present invention include:
[0039] (1) Benefiting from the good mechanical properties of the parallel bicomponent fiber filaments themselves, the prepared elastic yarn also has good mechanical properties; the parallel bicomponent fiber filaments and spandex filaments are not prone to hairiness or entanglement during the interweaving process, and the obtained elastic fiber has high strength and good elasticity;
[0040] (2) The twisted yarn obtained by parallel twisting of the bicomponent fiber filaments and the spandex filaments is similar in morphology to the ordinary twisted yarn, can be subjected to ordinary weaving process, and has good processability;
[0041] (3) In the stretch-induced elastic yarn, the spandex is in a twisted state, which can fix the loops formed by the stretched curled fibers. The loops are firm and not easy to fall apart, and have high strength.
[0042] (4) The stretch-induced elastic yarn has excellent properties such as good ductility, elasticity, acid and alkali resistance, sweat resistance, etc., and feels soft.
[0043] Example 1
[0044] (1) Preparation of parallel bicomponent fiber filaments:
[0045] Polymer A and polymer A* were respectively fed into the two barrels of the spunbond machine. The front zone temperature was set to 210°C, the rear zone and spinneret temperature was set to 230°C, the extrusion speed was 0.1-0.5 g / h / min, and the spinning speed was 50-100 m / min.
[0046] Polymer A and polymer A* pass through a screw extruder, a metering pump, and a filament separator in sequence from a barrel, and then merge at a spinneret hole. After being drawn and wound onto a bobbin, parallel bicomponent fiber filaments are obtained.
[0047] (2) Preparation of elastic yarn:
[0048] 2-10 parallel bicomponent fiber filaments and 1-3 spandex filaments with a specification of 20-50D are selected for doubling; the doubling filaments are placed in a doubling and twisting machine for doubling and twisting to obtain a doubly twisted elastic yarn; and both ends of the doubly twisted elastic yarn are stretched to increase the yarn length by 2-5 times to obtain a stretched and curled elastic yarn, wherein the twist of the stretched and curled elastic yarn is 80-150 twists / 10 cm.
[0049] Figure 1 Schematic diagram of the structure of elastic yarn obtained by twisting bicomponent fiber filaments and spandex in parallel. At this time, the elastic yarn does not yet have elasticity;
[0050] Figure 2 This is a schematic diagram of the structure of a stretched and curled elastic yarn. The parallel bicomponent fibers in the yarn are elongated and curled, achieving elastic properties. It also gives the stretched yarn good ductility and elasticity, and a soft feel.
[0051] Example 2
[0052] (1) Preparation of parallel bicomponent fiber filaments:
[0053] Polymer A and polymer A* were respectively fed into the two side barrels of the spunbond machine. The front zone temperature was set to 210°C, the rear zone and spinneret temperature was set to 230°C, the extrusion speed was 0.5-1g / h / min, and the spinning speed was 100-150m / min.
[0054] Polymer A and polymer A* are sequentially passed through a screw extruder, a metering pump, a filament separator, and a spinneret hole from a barrel, and are drawn and wound onto a bobbin to obtain parallel bicomponent fiber filaments.
[0055] (2) Preparation of elastic yarn:
[0056] 2-10 parallel bicomponent fiber filaments and 1-2 spandex filaments with a specification of 50-70D are selected for doubling; the doubling filaments are placed in a doubling and twisting machine for doubling and twisting to obtain a doubly twisted elastic yarn; and both ends of the doubly twisted elastic yarn are stretched to increase the yarn length by 2-5 times to obtain a stretched and curled elastic yarn, wherein the twist of the stretched and curled elastic yarn is 100-180 twists / 10 cm.
[0057] Example 3
[0058] (1) Preparation of parallel bicomponent fiber filaments:
[0059] Polymer A and polymer A* were respectively put into the barrels on both sides of the spunbond machine, and the temperature of the front zone was set to 210°C, the temperature of the rear zone and the spinneret was set to 230°C, the extrusion speed was 1-1.5 g / h / min, and the spinning speed was 150-200 m / min.
[0060] Polymer A and polymer A* are sequentially passed through a screw extruder, a metering pump, a filament separator, and a spinneret hole from a barrel, and are drawn and wound onto a bobbin to obtain parallel bicomponent fiber filaments.
[0061] (2) Preparation of elastic yarn:
[0062] 2-10 parallel bicomponent fiber filaments and 1-2 spandex filaments with a specification of 70-100D are selected for doubling; the doubling filaments are placed in a doubling and twisting machine for doubling and twisting to obtain a doubly twisted elastic yarn; and both ends of the doubly twisted elastic yarn are stretched to increase the yarn length by 2-5 times to obtain a stretched and curled elastic yarn, wherein the twist of the stretched and curled elastic yarn is 120-160 twists / 10 cm.
[0063] Example 4
[0064] (1) Preparation of parallel bicomponent fiber filaments:
[0065] Polymer A and polymer A* were respectively put into the barrels on both sides of the spunbond machine, and the temperature of the front zone was set to 210°C, the temperature of the rear zone and the spinneret was set to 230°C, the extrusion speed was 1.5-2g / h / min, and the spinning speed was 200-300m / min.
[0066] Polymer A and polymer A* are sequentially passed through a screw extruder, a metering pump, a filament separator, and a spinneret hole from a barrel, and are drawn and wound onto a bobbin to obtain parallel bicomponent fiber filaments.
[0067] (2) Preparation of elastic yarn:
[0068] 2-10 parallel bicomponent fiber filaments and 1-2 spandex filaments with a specification of 100-140D are selected for doubling; the doubling filaments are placed in a doubling and twisting machine for doubling and twisting to obtain a doubly twisted elastic yarn; and both ends of the doubly twisted elastic yarn are stretched to increase the yarn length by 2-5 times to obtain a stretched and curled elastic yarn, wherein the twist of the stretched and curled elastic yarn is 120-150 twists / 10 cm.
[0069] Example 5
[0070] (1) Preparation of parallel bicomponent fiber filaments:
[0071] Polymer A and polymer A* were respectively put into the barrels on both sides of the spunbond machine, and the temperature of the front zone was set to 190°C, the temperature of the rear zone and the spinneret was set to 210°C, the extrusion speed was 0.2-1g / h / min, and the spinning speed was 100-200m / min.
[0072] Polymer A and polymer A* are sequentially passed through a screw extruder, a metering pump, a filament separator, and a spinneret hole from a barrel, and are drawn and wound onto a bobbin to obtain parallel bicomponent fiber filaments.
[0073] (2) Preparation of elastic yarn:
[0074] 5-20 parallel bicomponent fiber filaments and 1-2 spandex filaments with a specification of 20-100D are selected for doubling; the doubling filaments are placed in a doubling and twisting machine for doubling and twisting to obtain a doubly twisted elastic yarn; and both ends of the doubly twisted elastic yarn are stretched to increase the yarn length by 2-5 times to obtain a stretched and curled elastic yarn, wherein the twist of the stretched and curled elastic yarn is 80-120 twists / 10 cm.
[0075] The elastic yarns of Examples 1, 2, 3, 4, and 5 were tested with a clamping distance of 50 mm, according to ASTM D2731-2001, "Standard Test Method for Elasticity of Elastomeric Yarns (CRE Tensile Tester). The test results are shown in Table 1. As shown in Table 1, the yarns of the present invention exhibit excellent elasticity and ductility, which are significantly affected by yarn twist and spandex fineness.
[0076] Table 1
[0077] Example 1 Example 2 Example 3 Example 4 Example 5 Elongation / mm 190.5±9 186.5±15.5 175±12.5 189.5±14.5 199.5±11 Elongation / % 3.81±0.18 3.73±0.31 3.5±0.25 3.79±0.29 3.99±0.22
[0078] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for a person skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to replace some of the technical features therein with equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions claimed to be protected by the present invention.
Claims
1. An elastic yarn, characterized in that: include At least one parallel bicomponent fiber filament and at least one spandex filament are twisted in parallel, The parallel bicomponent fiber filaments include polymer A and polymer A*, the polymer A and the polymer A* are similar polyolefin materials, the melt index of the polymer A and the polymer A* differ by more than 10, and the mass ratio of the polymer A to the polymer A* is 1:0.1-1:5; The preparation method of the elastic yarn comprises: (1) Preparing the parallel bicomponent fiber filaments: The polymer A and the polymer A* were respectively put into the barrels on both sides of the spunbond machine, and the temperature of the front zone was set to 210°C, and the temperature of the rear zone and the spinneret was set to 230°C; The polymer A and the polymer A* are sequentially passed through a screw extruder, a metering pump, and a filament separator from a barrel, and then merged at a spinneret hole, and are drawn and wound onto a bobbin to obtain parallel bicomponent fiber filaments; (2) Preparing the elastic yarn: Select parallel bicomponent fiber filaments and spandex filaments with specifications of 20-140D for doubling, and place the doubling filaments in a doubling and twisting machine for parallel twisting. The two ends of the twisted elastic yarn are stretched so that the yarn length increases by 2-5 times, and then the yarn is stretched to obtain a stretched and curled elastic yarn.
2. The elastic yarn according to claim 1, characterized in that The diameter of the parallel bicomponent fiber filaments is 12 μm-30 μm.
3. The elastic yarn according to claim 1, characterized in that The specifications of the spandex filaments are distributed in the range of 20-140D.
4. The elastic yarn according to claim 1, characterized in that The polyolefin material includes one of polypropylene (PP), polyethylene (PE), polyamide (PA), and polyester (PET).
5. The elastic yarn according to claim 1, characterized in that The melt index of the polymer A is 20-40, and the melt index of the polymer A* is 30-100.
6. The method for preparing elastic yarn according to claim 1, characterized in that: In the step (1), the extrusion speed is 0.1-0.5 g / h / min, and the spinning speed is 50-100 m / min.
7. The method for preparing elastic yarn according to claim 1, characterized in that: In the step (2), the number of the parallel bicomponent fiber filaments is 2-10, and the number of the spandex filaments is 1-3.
8. The method for preparing elastic yarn according to claim 1, characterized in that: In the step (2), the twist of the elastic yarn is 80-200 twists / 10cm.
9. The method for preparing elastic yarn according to claim 1, characterized in that: In the step (2), the specifications of the spandex filaments are distributed in the range of 20-140D.