Rabbit skin gelatin nanofiber membrane and preparation method thereof

By covalently cross-linking rabbit skin gelatin and tannic acid, the problem of water intolerance of gelatin fiber membrane in aqueous solution is solved, its water resistance and antibacterial properties are improved, and its application potential in the fields of medical and tissue textiles is significantly enhanced.

CN116043412BActive Publication Date: 2024-10-01TIANJIN POLYTECHNIC UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211629173.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2024-10-01
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

The existing gelatin fiber membrane is not water-resistant in aqueous solutions, which limits its application. The non-covalent cross-linking method is not ideal and cannot effectively improve the water resistance.

Method used

By covalently cross-linking rabbit skin gelatin with oxidized tannic acid, electrospinning technology was used to prepare nanofiber membranes, which promoted the nucleophilic addition reaction of gelatin and oxidized tannic acid to form covalent bonds and passed through multiple Secondary cross-linking improves the water resistance and antibacterial properties of the fiber.

Benefits of technology

The water resistance and antibacterial properties of the gelatin fiber membrane have been improved, significantly improving its application potential in fields such as medical dressings and tissue textiles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116043412B_ABST
    Figure CN116043412B_ABST
Patent Text Reader

Abstract

The present invention provides a rabbit skin gelatin nanofiber membrane and a preparation method thereof, which belongs to the field of polymer fibers or the field of textile science and technology. The preparation method of the rabbit skin gelatin nanofiber membrane comprises: dissolving rabbit skin gelatin in a first solvent to obtain a spinning solution; oxidizing tannic acid and dissolving it in a second solvent to obtain a cross-linking agent solution containing oxidized tannic acid with a quinone structure; mixing the spinning solution and the cross-linking agent solution for electrostatic spinning to obtain a first nanofiber membrane; placing the first nanofiber membrane in an ethanol aqueous solution to allow the first nanofiber membrane containing rabbit skin gelatin to undergo a nucleophilic addition reaction with the oxidized tannic acid with a quinone structure to obtain a preliminarily cross-linked second nanofiber membrane containing a tannic acid structure; taking out the second nanofiber membrane, oxidizing it, placing it in an ethanol aqueous solution for static cross-linking, and obtaining a rabbit skin gelatin nanofiber membrane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of polymer fiber technology or textile science and technology, and in particular relates to a collagen nanofiber membrane, and more specifically to a rabbit skin gelatin nanofiber membrane and a preparation method thereof. Background Art

[0002] Rabbit skin is rich in collagen and is one of the excellent raw materials for gelatin extraction. Studies have shown that the functional quality of rabbit skin collagen is better than that of aquatic gelatin. In recent years, due to the frequent occurrence of chicken fever, swine fever and mad cow disease, rabbit skin has become a high-quality source of gelatin extraction.

[0003] Gelatin fiber has good hydrophilicity, so it cannot maintain its fibrous state in aqueous solution, which limits the practical application of gelatin fiber. Tannic acid is a biodegradable substance, which has a natural polyphenol structure and has good activity, such as antibacterial, antiviral, antioxidant, anticancer, antifouling, antigen, antitumor and homeostatic agent. In addition, tannic acid is also a very ideal cross-linking agent as a polyphenol substance. At present, there have been related studies that use tannic acid as a cross-linking agent to cross-link with gelatin molecules through non-covalent interaction to obtain gelatin nanofiber membranes to solve the problem of poor water resistance of gelatin nanofiber membranes, but this cross-linking effect through non-covalent interaction is not ideal, so that the problem of gelatin fiber not being water-resistant still exists. Summary of the invention

[0004] In view of the above technical problems, the present invention provides a rabbit skin gelatin nanofiber membrane and a preparation method thereof, in order to solve the problem that the gelatin fiber is not water-resistant through the covalent cross-linking effect of gelatin and tannic acid.

[0005] In order to solve the above technical problems, the technical solutions provided by the present disclosure are as follows:

[0006] As a first aspect of the present disclosure, a method for preparing a gelatin nanofiber membrane is provided, comprising:

[0007] Step 1: dissolving rabbit skin gelatin in a first solvent to obtain a spinning solution;

[0008] Step 2: oxidizing tannic acid and dissolving it in a second solvent to obtain a cross-linking agent solution containing oxidized tannic acid having a quinone structure;

[0009] Step 3: electrospinning the solutions obtained in step 1 and step 2 to obtain a first nanofiber membrane;

[0010] Step 4: placing the first nanofiber membrane into an ethanol aqueous solution, allowing the first nanofiber membrane containing rabbit skin gelatin to undergo a nucleophilic addition reaction with the oxidized tannic acid having a quinone structure, thereby obtaining a preliminarily cross-linked second nanofiber membrane containing a tannic acid structure;

[0011] Step 5: Take out the second nanofiber membrane, put it into an ethanol aqueous solution for static cross-linking after oxidation, and obtain a rabbit skin gelatin nanofiber membrane.

[0012] In one embodiment, the concentration of the spinning solution is 3%-5%wt.

[0013] In one embodiment, the concentration of the cross-linking agent solution is 10 mg / mL-30 mg / mL.

[0014] In one embodiment, the first solvent includes hexafluoroisopropanol.

[0015] In one embodiment, the second solvent includes an ethanol aqueous solution; the ethanol aqueous solution contains 90% ethanol.

[0016] In one embodiment, the oxidation in step 2 comprises: introducing oxygen-containing gas into tannic acid to obtain oxidized tannic acid, wherein the oxygen-passing time is 30 min-2 h;

[0017] The oxidation in step five includes: introducing an oxygen-containing gas into the second nanofiber membrane to oxidize the polyphenol structure in the tannic acid structure into a quinone structure;

[0018] The oxygen-containing gas includes: any one of pure oxygen and air gas.

[0019] In one embodiment, the oxidation treatment in step five further comprises:

[0020] During the second nanofiber membrane oxidation process, heating is performed, wherein the heating temperature is 35-80° C. and the heating treatment time is 6-10 hours.

[0021] As a second aspect of the present disclosure, a rabbit skin gelatin nanofiber membrane is provided, which is prepared by the above-mentioned method for preparing the rabbit skin gelatin nanofiber membrane.

[0022] In one embodiment, the nanofiber membrane comprises tannic acid covalently cross-linked to gelatin.

[0023] In one embodiment, the nanofiber membrane is water resistant and antibacterial.

[0024] Based on the above technical solution, the present disclosure provides a rabbit skin gelatin nanofiber membrane and a preparation method thereof, which includes at least one of the following beneficial effects:

[0025] (1) According to the embodiments of the present invention, the tannic acid with a quinone structure obtained after oxidation of tannic acid is subjected to a nucleophilic addition reaction with a first nanofiber membrane containing rabbit skin gelatin, so that the first nanofiber membrane containing rabbit skin gelatin and the tannic acid with a quinone structure are cross-linked and form a covalent bond. At the same time, during the cross-linking process, the quinone structure in the oxidized tannic acid is restored to a polyphenol structure to obtain a second nanofiber membrane. After oxidation, the oxidized tannic acid with a quinone structure in the second nanofiber membrane continues to undergo a nucleophilic addition reaction with other first nanofiber membranes containing rabbit skin gelatin, so that the first nanofiber membrane and the tannic acid with a quinone structure in the second nanofiber membrane form a covalent bond and achieve cross-linking again. After multiple cross-linking, a rabbit skin gelatin fiber membrane is obtained. The obtained nanofiber membrane contains a tannic acid structure covalently cross-linked with gelatin, so that the gelatin fiber membrane has good water resistance and antibacterial properties.

[0026] (2) According to the embodiments of the present disclosure, the nanofiber membrane prepared by electrospinning technology has a high specific surface area, a high porosity and maintains the polyphenol structure naturally present in tannic acid, thereby making the rabbit skin gelatin nanofiber membrane have a significant application trend in the fields of medical dressings, tissue textiles, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is a diagram of the mechanism of preparing rabbit skin gelatin nanofiber membrane in the embodiment of the present disclosure;

[0028] Figure 2 This is a scanning electron microscope image of the pure rabbit skin gelatin nanofiber membrane in the embodiment of the present disclosure;

[0029] Figure 3 This is a scanning electron microscope image of the nanofiber membrane of tannic acid and gelatin non-covalent cross-linking in Comparative Example 1 after being immersed in water for 48 hours;

[0030] Figure 4 is a scanning electron microscope image of the nanofiber membrane covalently cross-linked with tannic acid and gelatin in Example 1;

[0031] Figure 5 This is a scanning electron microscope image of the nanofiber membrane covalently cross-linked with tannic acid and gelatin in Example 1 after being immersed in water for 48 hours;

[0032] Figure 6 is the instantaneous contact angle diagram of the nanofiber membrane of non-covalent cross-linking of tannic acid and gelatin in Comparative Example 1;

[0033] Figure 7 This is the contact angle diagram of the nanofiber membrane of tannic acid and gelatin non-covalent cross-linking in Comparative Example 1 after contacting water for 1 second;

[0034] Figure 8 is the instantaneous contact angle diagram of the nanofiber membrane covalently cross-linked by tannic acid and gelatin in Example 1;

[0035] Fig. 9 This is the contact angle diagram of the nanofiber membrane covalently cross-linked with tannic acid and gelatin in Example 1 after contacting water for 1 second. DETAILED DESCRIPTION

[0036] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.

[0037] In view of the problem that gelatin and tannic acid are cross-linked by non-covalent action in the related art, the prepared gelatin fiber has a low degree of cross-linking and cannot effectively improve the water resistance of gelatin, wherein the non-covalent action includes: hydrogen bonds and van der Waals forces between gelatin molecules and tannic acid. The present disclosure provides a method for preparing a rabbit skin gelatin nanofiber membrane, wherein gelatin molecules and oxidized tannic acid are subjected to nucleophilic addition to form covalent cross-linking, so that the prepared gelatin nanofiber membrane has good water resistance, and the nanofiber membrane has a tannic acid structure covalently cross-linked with gelatin, so that the nanofiber membrane also has antibacterial properties.

[0038] As a first aspect of the present disclosure, a method for preparing a rabbit skin gelatin nanofiber membrane is first provided, comprising:

[0039] Step 1: dissolving rabbit skin gelatin in a first solvent to obtain a spinning solution;

[0040] Step 2: oxidizing tannic acid and dissolving it in a second solvent to obtain a cross-linking agent solution containing oxidized tannic acid having a quinone structure;

[0041] Step 3: electrospinning the solutions obtained in step 1 and step 2 to obtain a first nanofiber membrane;

[0042] Step 4: placing the first nanofiber membrane into an ethanol aqueous solution, allowing the first nanofiber membrane containing rabbit skin gelatin to undergo a nucleophilic addition reaction with the oxidized tannic acid having a quinone structure, thereby obtaining a preliminarily cross-linked second nanofiber membrane containing a tannic acid structure;

[0043] Step 5: Take out the second nanofiber membrane, and then put it into an ethanol aqueous solution for static cross-linking after oxidation to obtain a nanofiber membrane.

[0044] Figure 1 It is a mechanism diagram for preparing rabbit skin gelatin nanofiber membrane in the embodiment of the present disclosure.

[0045] like Figure 1As shown, since tannic acid is a polyphenol structure (a), tannic acid is oxidized to form oxidized tannic acid with a quinone structure (b). Then, the spinning solution of step one is mixed with the cross-linking agent in step two for electrostatic spinning to obtain a first nanofiber membrane containing gelatin. At this time, the degree of cross-linking between gelatin and oxidized tannic acid in the first nanofiber membrane is low. The first nanofiber membrane is placed in an ethanol aqueous solution, which can promote the nucleophilic addition reaction between the first nanofiber membrane containing rabbit skin gelatin and the oxidized tannic acid with a quinone structure, so that the rabbit skin gelatin and the tannic acid with a quinone structure form a covalent bond to achieve cross-linking. At the same time, during the nucleophilic addition reaction, the oxidized tannic acid with a quinone structure is restored to tannic acid containing a polyphenol structure to obtain a second nanofiber membrane (c). Then, the tannic acid containing the polyphenol structure in the second nanofiber membrane is oxidized again, and the polyphenol structure is oxidized into a quinone structure (d), which can continue to undergo a nucleophilic addition reaction with the other first nanofiber membrane containing rabbit skin gelatin, so that the first nanofiber membrane and the tannic acid with a quinone structure in the second nanofiber membrane form a covalent bond to achieve cross-linking again. Such repeated oxidation and cross-linking eventually form a nanofiber membrane containing tannic acid covalently cross-linked with gelatin (e). In the embodiment of the present disclosure, the irreversible covalent interaction mechanism between tannic acid and gelatin molecules is utilized to achieve the purpose of maintaining the morphology and water resistance of gelatin nanofibers.

[0046] According to an embodiment of the present disclosure, the preparation method of rabbit skin gelatin includes: cleaning the rabbit skin and then scraping the fat and depilating the hair, and then soaking it in sodium chloride and hydrochloric acid, bathing it in water, cleaning it, and other operations to obtain the rabbit skin gelatin.

[0047] According to the embodiments of the present disclosure, electrospinning is an important technology for making nanofibers. The surface tension of the polymer solution is destroyed by high voltage to form a jet. During the solution spraying process, as the solvent evaporates, a fiber membrane with a diameter of nanometer level can be formed. In the embodiments of the present disclosure, the rotation speed of the electrospinning receiver is set to 250-350rpm, the voltage is 20KV, the distance from the nozzle to the receiver is 14-16cm, the flow rate of the gelatin spinning solution is 0.4-0.6ml / h; the flow rate of the cross-linking agent solution of oxidized tannic acid is 1-2ml / h, so as to realize the preparation of rabbit skin gelatin nanofiber membrane.

[0048] According to an embodiment of the present disclosure, the first solvent includes: hexafluoroisopropanol. Hexafluoroisopropanol is selected as the solvent. It has the advantages of strong volatility and large polarity, and can dissolve gelatin well. It is an ideal solvent for gelatin electrospinning. Moreover, after the nanofiber membrane spun with hexafluoroisopropanol as solvent is dried, there is no hexafluoroisopropanol residue on the nanofiber membrane, which is beneficial to the subsequent application of the nanofiber membrane in medical dressings, drug delivery and other fields.

[0049] According to the embodiments of the present disclosure, tannic acid is soluble in ethanol, while oxidized tannic acid is insoluble in ethanol. If only water is used as a solvent, the solvent evaporates slowly, which easily dissolves gelatin molecules in water and affects the cross-linking effect, and makes the prepared nanofiber membrane difficult to dry. Therefore, the oxidized tannic acid needs to be dissolved in a second solvent, and a small amount of water is used to dissolve the oxidized tannic acid, wherein the second solvent includes: an ethanol aqueous solution, wherein the ethanol aqueous solution contains 90% ethanol and the rest is water.

[0050] According to an embodiment of the present disclosure, the concentration of the spinning solution is 3%-5%wt, and the concentration of the cross-linking agent solution is 10mg / mL-30mg / mL.

[0051] According to an embodiment of the present disclosure, the oxidation treatment in step two and step five includes: introducing an oxygen-containing gas into the reaction system to oxidize the polyphenol structure into a quinone structure to retain the polyphenol structure in the tannic acid, wherein the oxygen-containing gas includes any one of pure oxygen and air gas.

[0052] According to an embodiment of the present disclosure, the oxidation in step 2 includes: introducing oxygen-containing gas into tannic acid to obtain oxidized tannic acid, wherein the oxygenation time is 30min-2h. In this step, the polyphenol structure in the tannic acid is first oxidized into a quinone structure, so that when the oxidized tannic acid is subsequently cross-linked with the gelatin in the first nanofiber membrane, the gelatin and the tannic acid with the quinone structure can undergo a nucleophilic addition reaction to form a covalent bond to complete the cross-linking, rather than cross-linking by non-covalent bonds such as hydrogen bonds and van der Waals forces, so that the nanofiber membrane provided by the present disclosure has a stable structure and good water resistance.

[0053] According to an embodiment of the present disclosure, in step four, the first nanofiber membrane containing rabbit skin gelatin is cross-linked with oxidized tannic acid to obtain a second nanofiber membrane containing a tannic acid structure, and the tannic acid and gelatin in the second nanofiber membrane are in a semi-cross-linked state, and the cross-linking is not complete; then the second nanofiber membrane is taken out, and the second nanofiber membrane is further oxidized to form a second nanofiber membrane with a quinone structure, which is further cross-linked with the first nanofiber membrane containing gelatin, thereby obtaining a rabbit skin gelatin nanofiber membrane with better water resistance.

[0054] According to an embodiment of the present disclosure, the oxidation treatment in step five further includes: heating during the oxidation process of the second nanofiber membrane, wherein the heating temperature is 35-80°C and the heating treatment time is 6-10 hours, for example, the heating temperature can be 40°C and the heating treatment time can be 8 hours. By heating the second nanofiber membrane, the degree of covalent cross-linking reaction between the second nanofiber membrane containing rabbit skin gelatin and the oxidized tannic acid containing a quinone structure can be effectively promoted.

[0055] As a second aspect of the present disclosure, a rabbit skin gelatin nanofiber membrane is also provided, wherein the nanofiber membrane comprises tannic acid covalently cross-linked with gelatin.

[0056] According to the embodiments of the present disclosure, since gelatin and tannic acid produce covalent bonds through nucleophilic addition reaction, the rabbit skin gelatin nanofiber membrane has good water resistance. At the same time, since the gelatin nanofiber membrane also retains the polyphenol structure of tannic acid, the nanofiber membrane also has certain antibacterial properties, making it feasible for use in fields such as medical dressings.

[0057] The technical solution of the present disclosure is further described below through specific examples and in conjunction with the accompanying drawings. The chemicals and raw materials used in the following examples are all commercially available or homemade through public preparation methods.

[0058] Comparative Example 1

[0059] Nanofibrous membranes of non-covalent cross-linking of tannic acid and gelatin

[0060] Step 1: dissolving rabbit skin gelatin in hexafluoroisopropanol, and using a magnetic stirrer to stir at a speed of 600 rpm for 6 hours to fully dissolve the gelatin in the hexafluoroisopropanol solution to obtain a spinning solution with a mass fraction of 5 wt%;

[0061] Step 2: Dissolve 100 mg of tannic acid in 10 ml of 90% by volume ethanol aqueous solution, and stir with a magnetic stirrer at 300 rpm for 3 h to fully dissolve the tannic acid in the ethanol solution.

[0062] Step 3: Place the gelatin spinning solution in step 1 and the tannic acid crosslinking agent solution in step 2 in two syringes for mixed electrospinning to obtain a nanofiber membrane with non-covalent crosslinking of tannic acid and gelatin. In the electrospinning process, the speed of the receiver is 300 rpm, the voltage is 20 KV, the distance from the nozzle to the receiver is 13 cm, the flow rate of the gelatin spinning solution is 0.5 ml / h; the flow rate of the oxidized tannic acid crosslinking agent solution is 1 ml / h.

[0063] The preparation method of rabbit skin gelatin comprises the following steps:

[0064] Step 1: Wash the rabbit skin with water, scrape the fat and remove the hair to obtain a clean rabbit skin;

[0065] Step 2: Cut the rabbit skin into pieces (1 cm*1 cm), soak the pieces in 1% sodium chloride solution for 6 h, wash and set aside;

[0066] Step 3: After washing, soak the rabbit skin in hydrochloric acid solution;

[0067] Step 4: Place the rabbit skin block into the same volume of deionized water, shake in a water bath at a constant temperature for 6 hours, filter and centrifuge the solution, and dry it in an oven at 60°C to obtain rabbit skin gelatin.

[0068] Step 5: Then, the rabbit skin gelatin is spun into nanofiber membrane.

[0069] Example 1

[0070] Nanofibrous membrane covalently cross-linked with tannic acid and gelatin

[0071] Step 1: dissolving rabbit skin gelatin in hexafluoroisopropanol, and using a magnetic stirrer to stir at a speed of 600 rpm for 6 hours to fully dissolve the gelatin in the hexafluoroisopropanol solution, to obtain a spinning solution containing gelatin with a mass fraction of 5 wt%;

[0072] Step 2: After oxygenating tannic acid for 1 hour, oxidized tannic acid is obtained. Then, 100 mg of oxidized tannic acid is dissolved in 10 ml of 90% by volume ethanol aqueous solution, and a magnetic stirrer is used to stir at a speed of 300 rpm for 3 hours to fully dissolve the oxidized tannic acid in the ethanol aqueous solution to obtain a cross-linker solution of oxidized tannic acid containing a quinone structure.

[0073] Step 3: The spinning solution of step 1 and the crosslinking agent solution of step 2 are placed in two syringes for mixing and electrospinning to obtain the first nanofiber membrane. In the electrospinning process, the speed of the electrospinning receiver is set to 300 rpm, the voltage is 20 KV, the distance from the nozzle to the receiver is 13 cm, the flow rate of the gelatin spinning solution is 0.5 ml / h, and the flow rate of the oxidized tannic acid crosslinking agent solution is 1 ml / h.

[0074] Step 4: Place the prepared first nanofiber membrane into a 90% ethanol aqueous solution and allow to stand at 40° C. under aerobic conditions for 8 hours to obtain a rabbit skin gelatin nanofiber membrane.

[0075] Figure 2 This is a scanning electron microscope image of the pure rabbit skin gelatin nanofiber membrane in the embodiment of the present disclosure; Figure 3 This is a scanning electron microscope image of the nanofiber membrane of tannic acid and gelatin non-covalent cross-linking in Comparative Example 1 after being immersed in water for 48 hours; Figure 4 is a scanning electron microscope image of the nanofiber membrane covalently cross-linked with tannic acid and gelatin in Example 1; Figure 5 This is a scanning electron microscope image of the nanofiber membrane covalently cross-linked with tannic acid and gelatin in Example 1 after being immersed in water for 48 hours.

[0076] The nanofiber membrane of tannic acid and gelatin non-covalent cross-linking prepared in Comparative Example 1 has the same morphology as the nanofiber membrane in Example 1, and will not be described in detail here. Figure 2-Figure 5It can be seen from the scanning electron microscope image that the nanofiber membrane using tannic acid and gelatin non-covalent cross-linking (Comparative Example 1) cannot maintain the fiber state after being immersed in water, while the nanofiber membrane using tannic acid and gelatin covalent cross-linking (Example 1) can still maintain the fiber state well after being immersed in water, indicating that the nanofiber membrane prepared by the method provided in the present invention has good water resistance.

[0077] Figure 6 is the instantaneous contact angle diagram of the nanofiber membrane of non-covalent cross-linking of tannic acid and gelatin in Comparative Example 1; Figure 7 This is the contact angle diagram of the nanofiber membrane of tannic acid and gelatin non-covalent cross-linking in Comparative Example 1 after contacting water for 1 second.

[0078] Depend on Figure 6-Figure 7 By comparison, it can be seen that the water on the surface of the nanofiber membrane in Comparative Example 1 disappears after contacting water for 1 second, indicating that the water resistance of the nanofiber membrane in Comparative Example 1 is poor.

[0079] Figure 8 is the instantaneous contact angle diagram of the nanofiber membrane covalently cross-linked by tannic acid and gelatin in Example 1; Fig. 9 This is the contact angle diagram of the nanofiber membrane covalently cross-linked with tannic acid and gelatin in Example 1 after contacting water for 1 second.

[0080] Depend on Figure 8-Figure 9 By comparison, it can be seen that the nanofiber membrane in Example 1 still maintains a certain water resistance after contacting water.

[0081] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.

Claims

1. A method for preparing a rabbit skin gelatin nanofiber membrane, comprising: Step 1: dissolving rabbit skin gelatin in a first solvent to obtain a spinning solution; Step 2: oxidizing tannic acid and dissolving it in a second solvent to obtain a cross-linking agent solution containing oxidized tannic acid having a quinone structure; Step 3: electrospinning the solutions obtained in step 1 and step 2 to obtain a first nanofiber membrane; Step 4: placing the first nanofiber membrane into an ethanol aqueous solution, so that the first nanofiber membrane containing rabbit skin gelatin and the oxidized tannic acid with a quinone structure undergo a nucleophilic addition reaction, wherein the rabbit skin gelatin and the tannic acid with a quinone structure form a covalent bond to achieve cross-linking, and simultaneously during the nucleophilic addition reaction, the oxidized tannic acid with a quinone structure is restored to a tannic acid containing a polyphenol structure, thereby obtaining a preliminarily cross-linked second nanofiber membrane containing a tannic acid structure; Step 5: Take out the second nanofiber membrane, oxidize the tannic acid containing polyphenol structure in the second nanofiber membrane into quinone structure, and then put it into ethanol aqueous solution for static cross-linking to obtain rabbit skin gelatin nanofiber membrane.

2. The method according to claim 1, wherein: The concentration of the spinning solution is 3%-5%wt.

3. The method according to claim 1, wherein: The concentration of the cross-linking agent solution is 10 mg / mL-30 mg / mL.

4. The method according to claim 1, wherein: The first solvent includes hexafluoroisopropanol.

5. The method according to claim 1, wherein: The second solvent includes an ethanol aqueous solution; The ethanol aqueous solution contains 90% ethanol.

6. The method according to claim 1, wherein: The oxidation in step 2 comprises: introducing oxygen-containing gas into tannic acid to obtain oxidized tannic acid, wherein the oxygen-passing time is 30 min-2 h; The oxidation in step five comprises: introducing an oxygen-containing gas into the second nanofiber membrane to oxidize the polyphenol structure in the tannic acid structure into a quinone structure; The oxygen-containing gas includes any one of pure oxygen and air gas.

7. The method according to claim 6, wherein: The oxidation treatment in step 5 further comprises: The second nanofiber membrane is heated during the oxidation process, wherein the heating temperature is 35-80° C. and the heating treatment time is 6-10 hours.

8. A rabbit skin gelatin nanofiber membrane, comprising: The method according to any one of claims 1 to 7 is adopted.

9. The nanofiber membrane according to claim 8, wherein: The nanofiber membrane comprises tannic acid covalently cross-linked with gelatin.

10. The nanofiber membrane according to claim 9, wherein: The nanofiber membrane has water resistance and antibacterial properties.