A high-density polyester fabric dyeing and moisture absorption and perspiration finishing process

Through the dyeing and moisture-wicking finishing process of high-density polyester fabrics, combined with the grafting reaction of lactic acid and wool keratin and the coating of chitosan, the problems of oil removal and insufficient waterproof and moisture-permeable performance in the fabric are solved, achieving high performance Waterproof and breathable effect.

CN116043577BActive Publication Date: 2024-10-18WUJIANG DEYI FASHIONS CLOTHS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310108339.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-14
Publication Date
2024-10-18
Estimated Expiration
2043-02-14

AI Technical Summary

Technical Problem

The oil added to high-density polyester fabrics during the weaving process is difficult to remove, causing color staining problems. At the same time, existing waterproof and moisture-permeable functional membranes have problems with poor waterproofness or moisture permeability, making it difficult to meet high-performance needs.

Method used

The dyeing and moisture-absorbing finishing process of high-density polyester fabrics is adopted, including fabric pre-treatment, dyeing, moisture-permeable finishing and waterproof finishing steps, through thermal insulation cold stacking, water washing, adding wool keratin to lactic acid solution, vacuum dehydration and chitosan coating. Covering to enhance the moisture absorption, moisture permeability and waterproof properties of the fabric.

Benefits of technology

It effectively removes the oil on the surface of the fabric, improves the moisture permeability of high-density polyester fabrics, and enhances the waterproof effect of the fabric through the combination of wool keratin and chitosan, solving the problem of insufficient waterproof and moisture permeability in traditional processes. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a one-bath processing technology for dyeing and moisture absorption and perspiration wicking finishing of high-density polyester fabric, comprising the following steps: S1. cold-bundling and washing the high-density polyester fabric to remove the oil on the surface of the fabric to obtain a white high-density polyester grey cloth; S2. putting the high-density polyester grey cloth prepared in step S1 into a dyeing vat, first adding a leveling agent and a degreasing agent during the heat preservation process, then adding a disperse dye, and finally adding acetic acid, dyeing after the heat preservation is completed, cooling and reducing cleaning, and finally washing twice to obtain a dyed fabric; S3. moisture permeability finishing of the fabric: adding the fabric prepared in step S2 to a lactic acid solution, and adding a wool keratin solution after the lactic acid small molecules fully penetrate into the fabric, dehydrating and grafting under vacuum conditions to obtain a polyester fabric grafted with keratin; S4. waterproof finishing of the fabric: coating a surface of one side of the polyester fabric grafted with keratin prepared in step S3 with a chitosan finishing solution, heating, and then coating glycerol on the outer side of the chitosan, and continuing the reaction to obtain a functional high-density polyester fabric.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of functional fabrics, and in particular to a high-density polyester fabric dyeing and moisture absorption and perspiration wicking finishing process. Background Art

[0002] In recent years, with the improvement of living standards, people have higher and higher requirements for clothing performance. In addition to the basic needs of covering shame and avoiding cold, the demand for safety, protection, comfort, functionality and environmental protection of clothing fabrics is increasing. On the basis of satisfying material life, people are pursuing more spiritual satisfaction, especially the hot rise of outdoor sports such as leisure tourism, which has also set off a climax of outdoor clothing with waterproof and breathable functional fabrics as the core. High-density fabrics have good breathability due to the large pores between the yarns in the fabric, but poor waterproofness. Coated fabrics have good waterproofness due to the general use of non-porous membrane coating structure, but poor breathability. Laminated fabrics, as mainstream products, have relatively excellent comprehensive performance compared with the first two. This is because the core functional layer of the fabric plays a major role - the waterproof and breathable membrane. The waterproof and breathable functional membranes currently on the market mainly include polytetrafluoroethylene hydrophobic microporous membranes and thermoplastic polyurethane hydrophilic non-porous membranes. Although PTFE microporous membrane has excellent waterproof and breathable properties, it still has problems such as high price, foreign technology monopoly and unstable product quality. At the same time, the slippery and non-sticky nature of PTFE polymer makes its subsequent composite process difficult, which limits its application areas.

[0003] TPU hydrophilic membrane has high water pressure resistance due to its non-porous structure, but its moisture permeability is poor and it is easily wetted by water, causing discomfort, so it is limited to the low-end market. Therefore, it is necessary to develop high-performance waterproof and breathable materials to replace the PTFE waterproof and breathable functional membrane monopolized by foreign technology. Summary of the invention

[0004] Technical problem to be solved: The purpose of the present invention is to provide a high-density polyester fabric dyeing and moisture absorption and perspiration finishing process, to solve the problem that during the weaving process of polyester high-density fabric, the weaving factory will add a higher proportion of oil, the oil is not removed cleanly before dyeing, and color spots are formed. At the same time, the problem of high-density polyester fabric being both waterproof and breathable is solved.

[0005] Technical solution: A high-density polyester fabric dyeing and moisture absorption and perspiration finishing process, comprising the following steps:

[0006] S1. Fabric pretreatment: The high-density polyester fabric is subjected to heat preservation cold stacking and water washing to remove the oil agent on the surface of the fabric to obtain a white high-density polyester grey fabric;

[0007] S2. Fabric dyeing: The high-density polyester grey fabric prepared in step S1 is put into a dyeing vat, heated to 40-45°C, and kept warm for 10 minutes. During the heat preservation process, a leveling agent and a degreasing agent are first added, and then disperse dyes are added, and finally acetic acid is added. After the heat preservation is completed, the temperature is raised to 90°C at 1.5-2°C / min, and the temperature is kept for 10 minutes. Then, the temperature is raised to 130-135°C at 1.5°C / min, and dyeing is performed for 45-55 minutes. Then, the temperature is reduced and washed, and the washing temperature is 80°C for 10-15 minutes. Finally, the second washing is performed at a washing temperature of 60°C for 10-15 minutes to obtain a dyed fabric;

[0008] S3 fabric moisture permeability finishing: the fabric prepared in step S2 is added to the lactic acid solution, the temperature is raised to 90 ° C, after the lactic acid small molecules fully penetrate the fabric, a concentration of 8.5-12wt% wool keratin solution is added, and the grafting is dehydrated under vacuum conditions to obtain a polyester fabric grafted with keratin;

[0009] S4. Fabric waterproof finishing: Coat one side of the keratin grafted polyester fabric prepared in step S3 with chitosan finishing solution, raise the ambient temperature to 50-60°C, then coat glycerol on the outside of the chitosan, and continue the reaction for 90-180 minutes to obtain a functional high-density polyester fabric.

[0010] Preferably, the treatment liquid of the cold stack in step S1 contains 80-100 g / L of liquid alkali, 4-6 g / L of degreasing agent, and 3-7 g / L of refining agent. The stacking time of the cold stack is 20-30 h, and the temperature is 35-40°C. The water washing is open-width water washing, and the washing tank temperatures are 60°C, 70°C, 90°C, 95°C, 85°C, 60°C and 50°C respectively.

[0011] Preferably, the cleaning solution for reduction cleaning in step S2 contains 2 g / L of acetic acid and 1 g / L of acidic reducing cleaning agent.

[0012] Preferably, the wool keratin in step S3 is wool keratin that has been subjected to flash blast treatment, the flash blast treatment parameters are 1.5-1.8 MPa, and the treatment time is 120-160 s.

[0013] Preferably, the temperature of the dehydration reaction in step S3 is 80-90°C.

[0014] Preferably, the chitosan finishing liquid in step S4 is chitosan acetic acid solution, the chitosan is low deacetylation chitosan, the acetylation degree is 55-60%, the molecular weight of low deacetylation chitosan is 5000-15000, and the concentration of the chitosan finishing liquid is 3-5wt%.

[0015] Preferably, the warp density of the high-density polyester fabric is 560-620 strands / 10cm, and the weft density is 350-400 strands / 10cm, and the polyester fibers in the high-density polyester fabric are triangular special-shaped interface fibers.

[0016] Beneficial effects: The process of the present invention has the following advantages:

[0017] 1. The present invention uses high concentration liquid alkali for heat preservation, cold stacking and flat width, which can dissolve the oil agent to the greatest extent;

[0018] 2. The high-density polyester fabric in the present invention has better moisture permeability than fabrics of other specifications. However, if a waterproof film is applied like a conventional process, the moisture permeability will be affected. In the present invention, lactic acid molecules are inserted into the gaps between the yarns of the fabric, and then dehydrated and condensed to form polylactic acid. During the polymerization, a wool keratin solution with a concentration of 8.5-12wt% is added. The wool keratin treated with flash explosion exposes reactive hydroxyl groups. The condensation polymerization and grafting reaction are carried out simultaneously. The wool keratin is grafted onto the polylactic acid. The wool keratin is generated on the surface of the fabric, which will enhance the moisture absorption and moisture permeability.

[0019] 3. In the last step, the present invention coats one side with low deacetylation degree. The chitosan with low deacetylation degree has less amino content, that is, less active group content, but contains some active groups. These active groups can react with the hydroxyl and carboxyl groups of wool keratin exposed on the outer surface of the fabric through dehydration condensation, greatly reducing the hydrophilic groups and improving the waterproof effect of the surface. At the same time, chitosan also has antibacterial effect. DETAILED DESCRIPTION

[0020] The present invention will be further described below in conjunction with embodiments, which are explanations of the present invention and are not limited to the following embodiments:

[0021] Example 1

[0022] A high-density polyester fabric dyeing and moisture absorption and perspiration finishing process, comprising the following steps:

[0023] S1. Fabric pretreatment: The high-density polyester fabric is subjected to heat preservation cold stacking and water washing, the cold stacking treatment liquid contains 80g / L of liquid alkali, 4g / L of degreasing agent, and 7g / L of refining agent, the cold stacking time is 20h, and the time is 40°C; the water washing is open-width water washing, and the washing tank temperatures are 60°C, 70°C, 90°C, 95°C, 85°C, 60°C and 50°C, respectively, to remove the oil on the surface of the fabric to obtain a white high-density polyester grey cloth;

[0024] S2. Fabric dyeing: The high-density polyester grey fabric prepared in step S1 is put into a dyeing vat, heated to 40°C, and kept warm for 10 minutes. During the heat preservation process, a leveling agent and a degreasing agent are first added, and then disperse dyes are added, and finally acetic acid is added. After the heat preservation is completed, the temperature is raised to 90°C at 2°C / min, and the temperature is kept for 10 minutes. Then, the temperature is raised to 135°C at 1.5°C / min, and dyeing is performed for 45 minutes. Then, the temperature is lowered and reduced for cleaning. The cleaning solution for reduction cleaning contains 2g / L of acetic acid and 1g / L of acidic reducing cleaning agent. The washing temperature is 80°C for 10 minutes. Finally, the second washing is performed at a temperature of 60°C for 10-15 minutes to obtain a dyed fabric.

[0025] S3. Fabric moisture permeability finishing: the fabric prepared in step S2 is added to the lactic acid solution, the temperature is raised to 90°C, and after the lactic acid small molecules are fully infiltrated into the fabric, a wool keratin solution with a concentration of 8.5wt% is added, the wool keratin is the wool keratin after flash explosion treatment, the flash explosion treatment parameter is 1.8MPa, the treatment time is 120s, and the grafting is dehydrated under vacuum conditions, the dehydration reaction temperature is 80°C, and a polyester fabric grafted with keratin is obtained;

[0026] S4. Fabric waterproof finishing: Coat one side of the keratin grafted polyester fabric prepared in step S3 with a low deacetylation chitosan acetic acid solution, wherein the deacetylation degree is 55%, the molecular weight of the low deacetylation chitosan is 15,000, and the concentration of the chitosan finishing solution is 5wt%. Raise the ambient temperature to 60°C, and then coat glycerol on the outside of the chitosan. Continue the reaction for 90 minutes to obtain a functional high-density polyester fabric.

[0027] Example 2

[0028] A high-density polyester fabric dyeing and moisture absorption and perspiration finishing process, comprising the following steps:

[0029] S1. Fabric pretreatment: The high-density polyester fabric is subjected to heat preservation cold stacking and water washing, the cold stacking treatment liquid contains 100g / L of liquid alkali, 6g / L of degreasing agent, and 3g / L of refining agent, the cold stacking time is 30h, and the time is 35°C; the water washing is open-width water washing, and the washing tank temperatures are 60°C, 70°C, 90°C, 95°C, 85°C, 60°C and 50°C, respectively, to remove the oil on the surface of the fabric to obtain a white high-density polyester grey cloth;

[0030] S2. Fabric dyeing: The high-density polyester grey fabric prepared in step S1 is put into a dyeing vat, heated to 45°C, and kept warm for 10 minutes. During the heat preservation process, a leveling agent and a degreasing agent are first added, and then disperse dyes are added, and finally acetic acid is added. After the heat preservation is completed, the temperature is raised to 90°C at 2°C / min, and the temperature is kept for 10 minutes. Then, the temperature is raised to 130°C at 1.5°C / min, and dyeing is performed for 55 minutes. Then, the temperature is lowered and reduced for cleaning. The cleaning solution for reduction cleaning contains 2g / L of acetic acid and 1g / L of acidic reducing cleaning agent. The washing temperature is 80°C for 15 minutes. Finally, the second washing is performed at a temperature of 60°C for 10-15 minutes to obtain a dyed fabric.

[0031] S3. Fabric moisture permeability finishing: the fabric prepared in step S2 is added to the lactic acid solution, the temperature is raised to 90°C, and after the lactic acid small molecules are fully infiltrated into the fabric, a 12wt% wool keratin solution is added, the wool keratin is the wool keratin after flash explosion treatment, the flash explosion treatment parameter is 1.5MPa, the treatment time is 160s, and the grafting is dehydrated under vacuum conditions, the dehydration reaction temperature is 90°C, and a polyester fabric grafted with keratin is obtained;

[0032] S4. Fabric waterproof finishing: Coat one side of the surface of the keratin grafted polyester fabric prepared in step S3 with a low deacetylation chitosan acetic acid solution, the deacetylation degree is 60%, the molecular weight of the low deacetylation chitosan is 5000, the concentration of the chitosan finishing solution is 3wt%, the ambient temperature is raised to 50°C, glycerol is coated on the outside of the chitosan, and the reaction is continued for 180 minutes to obtain a functional high-density polyester fabric.

[0033] Example 3

[0034] A high-density polyester fabric dyeing and moisture absorption and perspiration finishing process, comprising the following steps:

[0035] S1. Fabric pretreatment: The high-density polyester fabric is subjected to heat preservation cold stacking and water washing, the cold stacking treatment liquid contains 85g / L of liquid alkali, 5g / L of degreasing agent, and 6g / L of refining agent, the cold stacking time is 22h, and the time is 35°C; the water washing is open-width water washing, and the washing tank temperatures are 60°C, 70°C, 90°C, 95°C, 85°C, 60°C and 50°C, respectively, to remove the oil on the surface of the fabric to obtain a white high-density polyester grey cloth;

[0036] S2. Fabric dyeing: The high-density polyester grey fabric prepared in step S1 is put into a dyeing vat, heated to 40°C, and kept warm for 10 minutes. During the heat preservation process, a leveling agent and a degreasing agent are first added, and then disperse dyes are added, and finally acetic acid is added. After the heat preservation is completed, the temperature is raised to 90°C at 2°C / min, and the temperature is kept for 10 minutes. Then, the temperature is raised to 135°C at 1.5°C / min, and dyeing is performed for 50 minutes. Then, the temperature is lowered and reduced for cleaning. The cleaning solution for reduction cleaning contains 2g / L of acetic acid and 1g / L of acidic reducing cleaning agent. The washing temperature is 80°C for 10 minutes. Finally, the second washing is performed at a temperature of 60°C for 10 minutes to obtain a dyed fabric.

[0037] S3. Fabric moisture permeability finishing: the fabric prepared in step S2 is added to the lactic acid solution, the temperature is raised to 90°C, and after the lactic acid small molecules are fully infiltrated into the fabric, a wool keratin solution with a concentration of 9.5wt% is added, the wool keratin is the wool keratin after flash explosion treatment, the flash explosion treatment parameter is 1.6MPa, the treatment time is 150s, and the grafting is dehydrated under vacuum conditions, the dehydration reaction temperature is 80°C, and a polyester fabric grafted with keratin is obtained;

[0038] S4. Fabric waterproof finishing: Coat one side of the keratin grafted polyester fabric prepared in step S3 with a low deacetylation chitosan acetic acid solution, wherein the deacetylation degree is 58%, the molecular weight of the low deacetylation chitosan is 7000, and the concentration of the chitosan finishing solution is 4wt%. Raise the ambient temperature to 55°C, and then coat glycerol on the outside of the chitosan. Continue the reaction for 120 minutes to obtain a functional high-density polyester fabric.

[0039] Example 4

[0040] A high-density polyester fabric dyeing and moisture absorption and perspiration finishing process, comprising the following steps:

[0041] S1. Fabric pretreatment: The high-density polyester fabric is subjected to heat preservation cold stacking and water washing, the cold stacking treatment liquid contains 95g / L of liquid alkali, 6g / L of degreasing agent, and 4g / L of refining agent, the cold stacking time is 28h, and the time is 40°C; the water washing is open-width water washing, and the washing tank temperatures are 60°C, 70°C, 90°C, 95°C, 85°C, 60°C and 50°C, respectively, to remove the oil on the surface of the fabric to obtain a white high-density polyester grey cloth;

[0042] S2. Fabric dyeing: The high-density polyester grey fabric prepared in step S1 is put into a dyeing vat, heated to 45°C, and kept warm for 10 minutes. During the heat preservation process, a leveling agent and a degreasing agent are first added, and then disperse dyes are added, and finally acetic acid is added. After the heat preservation is completed, the temperature is raised to 90°C at 1.5°C / min, and the temperature is kept for 10 minutes. Then, the temperature is raised to 35°C at 1.5°C / min, dyeing is performed for 55 minutes, and then the temperature is lowered for reduction cleaning. The cleaning solution for reduction cleaning contains 2g / L acetic acid and 1g / L acidic reducing cleaning agent. The washing temperature is 80°C for 15 minutes. Finally, the second washing is performed at a temperature of 60°C for 15 minutes to obtain a dyed fabric.

[0043] S3. Fabric moisture permeability finishing: the fabric prepared in step S2 is added to the lactic acid solution, the temperature is raised to 90°C, and after the lactic acid small molecules are fully infiltrated into the fabric, a wool keratin solution with a concentration of 11wt% is added, the wool keratin is the wool keratin after flash explosion treatment, the flash explosion treatment parameter is 1.8MPa, the treatment time is 140s, and the grafting is dehydrated under vacuum conditions, the dehydration reaction temperature is 90°C, and a polyester fabric grafted with keratin is obtained;

[0044] S4. Fabric waterproof finishing: Coat one side of the keratin grafted polyester fabric prepared in step S3 with a low deacetylation chitosan acetic acid solution, wherein the deacetylation degree is 55%, the molecular weight of the low deacetylation chitosan is 12000, and the concentration of the chitosan finishing solution is 5wt%. Raise the ambient temperature to 53°C, and then coat glycerol on the outside of the chitosan. Continue the reaction for 150 minutes to obtain a functional high-density polyester fabric.

[0045] Example 5

[0046] A high-density polyester fabric dyeing and moisture absorption and perspiration finishing process, comprising the following steps:

[0047] S1. Fabric pretreatment: The high-density polyester fabric is subjected to heat preservation cold stacking and water washing, the cold stacking treatment liquid contains 90g / L of liquid alkali, 5.5g / L of degreasing agent, and 5g / L of refining agent, the cold stacking time is 25h, and the time is 35°C; the water washing is open-width water washing, and the washing tank temperatures are 60°C, 70°C, 90°C, 95°C, 85°C, 60°C and 50°C, respectively, to remove the oil on the surface of the fabric to obtain a white high-density polyester grey cloth;

[0048] S2. Fabric dyeing: The high-density polyester grey fabric prepared in step S1 is put into a dyeing vat, heated to 45°C, and kept warm for 10 minutes. During the heat preservation process, a leveling agent and a degreasing agent are first added, and then disperse dyes are added, and finally acetic acid is added. After the heat preservation is completed, the temperature is raised to 90°C at 2°C / min, and the temperature is kept for 10 minutes. Then, the temperature is raised to 130-135°C at 1.5°C / min, and dyeing is performed for 55 minutes. Then, the temperature is lowered and reduced for cleaning. The cleaning solution for reduction cleaning contains 2g / L of acetic acid and 1g / L of acidic reducing cleaning agent. The washing temperature is 80°C for 15 minutes. Finally, the second washing is performed at a temperature of 60°C for 12 minutes to obtain a dyed fabric.

[0049] S3. Fabric moisture permeability finishing: the fabric prepared in step S2 is added to the lactic acid solution, the temperature is raised to 90°C, and after the lactic acid small molecules are fully infiltrated into the fabric, a wool keratin solution with a concentration of 10.5wt% is added, the wool keratin is the wool keratin after flash explosion treatment, the flash explosion treatment parameter is 1.7MPa, the treatment time is 150s, and the grafting is dehydrated under vacuum conditions, the dehydration reaction temperature is 85°C, and a polyester fabric grafted with keratin is obtained;

[0050] S4. Fabric waterproof finishing: Coat one side of the keratin grafted polyester fabric prepared in step S3 with a low deacetylation chitosan acetic acid solution, wherein the deacetylation degree is 56%, the molecular weight of the low deacetylation chitosan is 8000, and the concentration of the chitosan finishing solution is 4.5wt%. Raise the ambient temperature to 55°C, and then coat glycerol on the outside of the chitosan. Continue the reaction for 140 minutes to obtain a functional high-density polyester fabric.

[0051] Comparative Example 1

[0052] A high-density polyester fabric dyeing and moisture absorption and perspiration finishing process, comprising the following steps:

[0053] S1. Fabric pretreatment: The high-density polyester fabric is subjected to heat preservation cold stacking and water washing, the cold stacking treatment liquid contains 90g / L of liquid alkali, 5.5g / L of degreasing agent, and 5g / L of refining agent, the cold stacking time is 25h, and the time is 35°C; the water washing is open-width water washing, and the washing tank temperatures are 60°C, 70°C, 90°C, 95°C, 85°C, 60°C and 50°C, respectively, to remove the oil on the surface of the fabric to obtain a white high-density polyester grey cloth;

[0054] S2. Fabric dyeing: The high-density polyester grey fabric prepared in step S1 is put into a dyeing vat, heated to 45°C, and kept warm for 10 minutes. During the heat preservation process, a leveling agent and a degreasing agent are first added, and then disperse dyes are added, and finally acetic acid is added. After the heat preservation is completed, the temperature is raised to 90°C at 2°C / min, and the temperature is kept for 10 minutes. Then, the temperature is raised to 130-135°C at 1.5°C / min, and dyeing is performed for 55 minutes. Then, the temperature is lowered and reduced for cleaning. The cleaning solution for reduction cleaning contains 2g / L of acetic acid and 1g / L of acidic reducing cleaning agent. The washing temperature is 80°C for 15 minutes. Finally, the second washing is performed at a temperature of 60°C for 12 minutes to obtain a dyed fabric.

[0055] S3. Fabric moisture permeability finishing: The fabric prepared in step S2 is added to a lactic acid solution, heated to 90°C, and after the lactic acid small molecules fully penetrate into the fabric, a 11wt% wool keratin solution is added, and the grafting is dehydrated under vacuum conditions. The dehydration reaction temperature is 85°C to obtain a polyester fabric grafted with keratin;

[0056] S4. Fabric waterproof finishing: Coat one side of the keratin grafted polyester fabric prepared in step S3 with a low deacetylation chitosan acetic acid solution, wherein the deacetylation degree is 56%, the molecular weight of the low deacetylation chitosan is 8000, and the concentration of the chitosan finishing solution is 4.5wt%. Raise the ambient temperature to 55°C, and then coat glycerol on the outside of the chitosan. Continue the reaction for 140 minutes to obtain a functional high-density polyester fabric.

[0057] Comparative Example 2

[0058] A high-density polyester fabric dyeing and moisture absorption and perspiration finishing process, comprising the following steps:

[0059] S1. Fabric pretreatment: The high-density polyester fabric is subjected to heat preservation cold stacking and water washing, the cold stacking treatment liquid contains 85g / L of liquid alkali, 5g / L of degreasing agent, and 6g / L of refining agent, the cold stacking time is 22h, and the time is 35°C; the water washing is open-width water washing, and the washing tank temperatures are 60°C, 70°C, 90°C, 95°C, 85°C, 60°C and 50°C, respectively, to remove the oil on the surface of the fabric to obtain a white high-density polyester grey cloth;

[0060] S2. Fabric dyeing: The high-density polyester grey fabric prepared in step S1 is put into a dyeing vat, heated to 40°C, and kept warm for 10 minutes. During the heat preservation process, a leveling agent and a degreasing agent are first added, and then disperse dyes are added, and finally acetic acid is added. After the heat preservation is completed, the temperature is raised to 90°C at 2°C / min, and the temperature is kept for 10 minutes. Then, the temperature is raised to 135°C at 1.5°C / min, and dyeing is performed for 50 minutes. Then, the temperature is lowered and reduced for cleaning. The cleaning solution for reduction cleaning contains 2g / L of acetic acid and 1g / L of acidic reducing cleaning agent. The washing temperature is 80°C for 10 minutes. Finally, the second washing is performed at a temperature of 60°C for 10 minutes to obtain a dyed fabric.

[0061] S3. Fabric moisture permeability finishing: the fabric prepared in step S2 is added to the lactic acid solution, the temperature is raised to 90°C, and after the lactic acid small molecules are fully infiltrated into the fabric, a wool keratin solution with a concentration of 8.5wt% is added, the wool keratin is the wool keratin after flash explosion treatment, the flash explosion treatment parameter is 1.6MPa, the treatment time is 150s, and the grafting is dehydrated under vacuum conditions, and the dehydration reaction temperature is 80°C to obtain a polyester fabric grafted with keratin;

[0062] S4. Fabric waterproof finishing: Coat one side of the keratin grafted polyester fabric prepared in step S3 with a low deacetylation chitosan acetic acid solution, wherein the deacetylation degree is 90%, the molecular weight of the low deacetylation chitosan is 7000, and the concentration of the chitosan finishing solution is 4wt%. Raise the ambient temperature to 55°C, and then coat glycerol on the outside of the chitosan. Continue the reaction for 120 minutes to obtain a functional high-density polyester fabric.

[0063] Comparative Example 3

[0064] A high-density polyester fabric dyeing and moisture absorption and perspiration finishing process, comprising the following steps:

[0065] S1. Fabric pretreatment: The high-density polyester fabric is subjected to heat preservation cold stacking and water washing, the cold stacking treatment liquid contains 95g / L of liquid alkali, 6g / L of degreasing agent, and 4g / L of refining agent, the cold stacking time is 28h, and the time is 40°C; the water washing is open-width water washing, and the washing tank temperatures are 60°C, 70°C, 90°C, 95°C, 85°C, 60°C and 50°C, respectively, to remove the oil on the surface of the fabric to obtain a white high-density polyester grey cloth;

[0066] S2. Fabric dyeing: The high-density polyester grey fabric prepared in step S1 is put into a dyeing vat, heated to 45°C, and kept warm for 10 minutes. During the heat preservation process, a leveling agent and a degreasing agent are first added, and then disperse dyes are added, and finally acetic acid is added. After the heat preservation is completed, the temperature is raised to 90°C at 1.5°C / min, and the temperature is kept for 10 minutes. Then, the temperature is raised to 35°C at 1.5°C / min, dyeing is performed for 55 minutes, and then the temperature is lowered for reduction cleaning. The cleaning solution for reduction cleaning contains 2g / L acetic acid and 1g / L acidic reducing cleaning agent. The washing temperature is 80°C for 15 minutes. Finally, the second washing is performed at a temperature of 60°C for 15 minutes to obtain a dyed fabric.

[0067] S3. Fabric moisture permeability finishing: The fabric prepared in step S2 is added to a lactic acid solution, heated to 90°C, and after the lactic acid small molecules fully penetrate into the fabric, dehydrated and grafted under vacuum conditions, the dehydration reaction temperature is 90°C, and a polyester fabric grafted with keratin is obtained;

[0068] S4. Fabric waterproof finishing: Coat one side of the polyester fabric prepared in step S3 with a low deacetylation chitosan acetic acid solution, the deacetylation degree is 55%, the molecular weight of the low deacetylation chitosan is 12000, the concentration of the chitosan finishing solution is 5wt%, raise the ambient temperature to 53°C, and then coat glycerol on the outside of the chitosan. Continue the reaction for 150 minutes to obtain a functional high-density polyester fabric.

[0069]

[0070] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A high-density polyester fabric dyeing and moisture absorption and perspiration finishing process, characterized in that: The following steps are involved: S1. Fabric pretreatment: cold-batch and wash the high-density polyester fabric to remove the oil on the surface of the fabric to obtain a white high-density polyester grey fabric; S2. Fabric dyeing: The high-density polyester grey fabric prepared in step S1 is put into a dyeing vat, heated to 40-45°C, and kept warm for 10 minutes. During the heat preservation process, a leveling agent and a degreasing agent are first added, and then disperse dyes are added, and finally acetic acid is added. After the heat preservation is completed, the temperature is raised to 90°C at 1.5-2°C / min, and the temperature is kept for 10 minutes. Then, the temperature is raised to 130-135°C at 1.5°C / min, and dyeing is performed for 45-55 minutes. Then, the temperature is reduced and washed, and the washing temperature is 80°C for 10-15 minutes. Finally, the second washing is performed at a washing temperature of 60°C for 10-15 minutes to obtain a dyed fabric; S3 fabric moisture permeability finishing: the fabric prepared in step S2 is added to the lactic acid solution, the temperature is raised to 90 ° C, after the lactic acid small molecules fully penetrate the fabric, a concentration of 8.5-12wt% wool keratin solution is added, and the grafting is dehydrated under vacuum conditions to obtain a polyester fabric grafted with keratin; S4. Fabric waterproof finishing: Coat one side of the keratin grafted polyester fabric prepared in step S3 with chitosan finishing solution, wherein the chitosan is low deacetylated chitosan with an acetylation degree of 55-60%, raise the ambient temperature to 50-60°C, and then coat glycerol on the outside of the chitosan, and continue the reaction for 90-180 minutes to obtain a functional high-density polyester fabric.

2. The high-density polyester fabric dyeing and moisture absorption and perspiration finishing process according to claim 1, characterized in that: The cold stacking treatment liquid in step S1 contains 80-100 g / L of liquid caustic soda, 4-6 g / L of degreasing agent, and 3-7 g / L of refining agent, and the stacking time of the cold stacking is 20-30 h; the water washing is open-width water washing, and the water tank temperatures are 60°C, 70°C, 90°C, 95°C, 85°C, 60°C and 50°C respectively.

3. The high-density polyester fabric dyeing and moisture absorption and perspiration finishing process according to claim 1, characterized in that: The cleaning solution for reduction cleaning in step S2 contains 2 g / L of acetic acid and 1 g / L of acidic reducing cleaning agent.

4. The high-density polyester fabric dyeing and moisture absorption and perspiration finishing process according to claim 1, characterized in that: The wool keratin in step S3 is wool keratin that has been subjected to flash blast treatment, the flash blast treatment parameters are 1.5-1.8 MPa, and the treatment time is 120-160 s.

5. The high-density polyester fabric dyeing and moisture absorption and perspiration finishing process according to claim 1, characterized in that: The temperature of the dehydration reaction in step S3 is 80-90°C.

6. The high-density polyester fabric dyeing and moisture absorption and perspiration finishing process according to claim 1, characterized in that: In step S4, the chitosan finishing solution is a chitosan acetic acid solution, the molecular weight of low deacetylated chitosan is 5000-15000, and the concentration of the chitosan finishing solution is 3-5wt%.

7. The high-density polyester fabric dyeing and moisture absorption and perspiration finishing process according to claim 1, characterized in that: The warp density of the high-density polyester fabric is 560-620 strands / 10cm, and the weft density is 350-400 strands / 10cm. The polyester fibers in the high-density polyester fabric are triangular special-shaped cross-section fibers.

Citation Information

Patent Citations

  • A waterproof moisture-permeable membrane and uses thereof

    CN104513472A

  • Production process of single-faced hydrophilic wool-polyester fabric

    CN105926285A