A method for improving the bonding strength between electric heating sheet and composite material

By using a polyimide film and a heating device during the bonding process between the electric heating plate and the composite material, the resin penetrates into the gap between the electric heating plate, which solves the problem of poor adhesion between the electric heating plate and the composite material in the existing technology and improves the Improved overall strength and anti-icing performance.

CN116061458BActive Publication Date: 2024-10-25JIANGXI JIUYOU AVIATION EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111459021.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-02
Publication Date
2024-10-25
Estimated Expiration
2041-12-02

AI Technical Summary

Technical Problem

In the existing technology, the adhesion between the electric heating plate and the composite material is poor, which leads to easy delamination after molding and a decrease in overall strength, affecting the anti-icing performance.

Method used

By laying the matrix prepreg on the molding mold, using a polyimide film electric heating sheet to bond to the matrix prepreg, and heating it through a heating device to allow the resin to penetrate into the gap between the electric heating sheets, and then lay the composite material and perform curing treatment. , ensure that the electric heating plate and the composite material are tightly bonded.

Benefits of technology

It improves the bonding strength between the electric heating plate and the composite material, prevents shifting, and significantly improves the strength of the composite material after molding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116061458B_ABST
    Figure CN116061458B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for improving the bonding strength between an electric heating sheet and a composite material, which is used to improve the bonding strength between the electric heating sheet and the composite material. First, a matrix prepreg is laid on a forming mold, and the side of the polyimide film electric heating sheet with the electric heating sheet faces the matrix prepreg, and then the polyimide film is torn off so that the electric heating sheet remains on the matrix prepreg, and the resin in the matrix prepreg is allowed to penetrate into the gap of the electric heating sheet through a heating device, and finally cured and formed. The method for bonding the electric heating sheet and the composite material has a high bonding strength, so that the electric heating sheet will not move after being laid on the composite material, and can also effectively improve the strength of the composite material after forming.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electric heating plate bonding technology, and in particular to a method for improving the bonding strength between an electric heating plate and a composite material. Background Art

[0002] Because the wings, rotors, air inlets and other parts of helicopters and fixed-wing aircraft will freeze during flight, thus affecting the aerodynamic shape and flight safety, anti-icing measures need to be taken in these parts to ensure flight quality. The electric heating anti-icing method requires integrating the electric heating plate into the skin of the parts prone to ice formation, so that the electric heating plate can be powered on during flight to increase the temperature of the skin of the parts prone to ice formation, thereby melting the ice on the skin surface.

[0003] Among them, fiber-reinforced resin-based composite materials have the characteristics of light weight, high strength, high modulus, fatigue resistance, corrosion resistance, good designability and processability, and are ideal aviation structural materials.

[0004] Patent No. CN201710173592.0 discloses a multilayer structure of an anti-icing / de-icing composite material, the defects of which are that the electric heating plate has poor adhesion to the composite material and is easily delaminated after molding, resulting in a decrease in the overall strength of the composite. Summary of the invention

[0005] In order to solve the defects of the prior art mentioned above, the present invention proposes a method for improving the bonding strength between an electric heating plate and a composite material.

[0006] The technical solution of the present invention is achieved in this way:

[0007] A method for improving the bonding strength between an electric heating sheet and a composite material, characterized by comprising the following steps:

[0008] The first step is to prepare a molding mold and lay the matrix prepreg on the molding mold;

[0009] The second step is to bond the polyimide film to the electric heating sheet to make a polyimide film electric heating sheet;

[0010] The third step is to place the polyimide film electric heating sheet with the electric heating sheet facing the base prepreg, and then evenly attach the polyimide film electric heating sheet to the base prepreg;

[0011] Step 4: tear off the polyimide film, leaving the electric heating sheet on the base prepreg;

[0012] The fifth step is to uniformly heat the electric heating sheet by a heating device so that the resin in the matrix prepreg can penetrate into the gap of the electric heating sheet;

[0013] Step 6: Continue to lay the composite material on the electric heating sheet, and after laying, perform a curing treatment on the electric heating sheet and the composite material;

[0014] Step 7: The electric heating plate is tightly bonded to the composite material.

[0015] In the method of improving the bonding strength between the electric heating plate and the composite material of the present invention, before the first step, the surface of the molding mold is evenly coated with three layers of thermal insulation coating, and the thermal insulation coating is specifically any one of composite magnesium aluminum silicate thermal insulation coating, rare earth thermal insulation coating, and coated composite silicate thermal insulation coating.

[0016] In the method for improving the bonding strength between the electric heating sheet and the composite material of the present invention, the heating device is a hair dryer, and the heating temperature of the hair dryer is 50°C-80°C.

[0017] In the method of improving the bonding strength between the electric heating plate and the composite material of the present invention, the composite material is the skin material for the wings, rotors, air inlets and other parts, and is made of at least one of high-strength aluminum, magnesium alloy, titanium alloy and the like.

[0018] In the method for improving the bonding strength between the electric heating plate and the composite material of the present invention, the matrix prepreg is formed by impregnating a high-strength carbon fiber cloth reinforcement into a resin glue solution.

[0019] In the method for improving the bonding strength between the electric heating plate and the composite material of the present invention, the resin adhesive is bismaleimide adhesive and epoxy resin adhesive.

[0020] In the method for improving the bonding strength between the electric heating plate and the composite material of the present invention, the mass of the resin glue in the matrix prepreg accounts for 36%-42% of the total mass of the matrix prepreg.

[0021] The method of improving the bonding strength between an electric heating sheet and a composite material according to the present invention has the following beneficial effects: the method of improving the bonding strength between an electric heating sheet and a composite material improves the adhesion between the electric heating sheet and the matrix prepreg during lamination, so that the electric heating sheet will not shift after being laid on the composite material, and can also effectively improve the strength of the composite material after molding. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a process flow chart of laying the electric heating sheet of the present invention;

[0023] Figure 2 It is a schematic diagram of the electric heating plate and the polyimide film;

[0024] Figure 3 It is a schematic diagram of a polyimide film electric heating sheet;

[0025] Figure 4It is a schematic diagram of the matrix prepreg and the molding mold;

[0026] Figure 5 This is a schematic diagram of laying a polyimide film electric heating sheet;

[0027] Figure 6 Schematic diagram of polyimide film electric heating sheet being applied to base prepreg;

[0028] Figure 7 Schematic diagram of tearing off the polyimide film. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the accompanying drawings in the embodiments of the present invention.

[0030] like Figures 1 to 7 As shown, the method of improving the bonding strength between the electric heating sheet and the composite material of the present invention is used to improve the bonding strength between the electric heating sheet and the composite material. It includes the following steps:

[0031] The first step is to prepare a molding die 5 and lay a matrix prepreg 4 on the molding die 5 .

[0032] The matrix prepreg 4 is formed by impregnating a high-strength carbon fiber cloth reinforcement into an epoxy resin adhesive or a bismaleimide resin adhesive, wherein the mass of the resin adhesive in the matrix prepreg 4 accounts for 36%-42% of the total mass of the matrix prepreg 4.

[0033] When the resin glue is epoxy resin glue, the mass of epoxy resin glue in the matrix prepreg 4 accounts for 38%±2% of the total mass of the matrix prepreg 4, and the thickness of the prepared matrix prepreg 4 is 0.2mm, and the surface density is 210g / m2; when the resin glue is bismaleimide resin glue, the mass of bismaleimide resin glue in the matrix prepreg 4 accounts for 40%±2% of the mass of the matrix prepreg 4, and the thickness of the prepared matrix prepreg 4 is 0.2mm, and the surface density is 210g / m2. By controlling the content of resin glue in the prepreg, the performance requirements of the final product can be effectively guaranteed.

[0034] The number of layers of the matrix prepreg 4 is 1 to 5. When the layer thickness is such, the bonding quality between the matrix prepreg 4 and the electric heating plate 2 can be ensured, local debonding can be further avoided, and the surface accuracy of the final product can be ensured.

[0035] In the second step, a polyimide film 1 and an electric heating plate 2 are prepared, and the polyimide film 1 and the electric heating plate 2 are bonded together to form a polyimide film electric heating plate 3.

[0036] Since the polyimide film 1 has a relatively high tensile strength of more than 115 MPa, it can fully support the electric heating plate 2, so that the electric heating plate 2 is not easily deformed, thereby improving the molding quality of the final product.

[0037] In the third step, the polyimide film electric heating sheet 3 with the electric heating sheet 2 faces the base prepreg 4, and then the polyimide film electric heating sheet 3 is evenly attached to the base prepreg 4.

[0038] It should be noted that the length of the electric heating plate 2 is consistent with the direction of the base prepreg 4, the length of the electric heating plate 2 is smaller than the length of the base prepreg 4, and the width of the electric heating plate 2 is smaller than the width of the base prepreg 4, so that the electric heating plate 2 is completely attached to the base prepreg 4, thereby improving the adhesion between the electric heating plate 2 and the base prepreg 4.

[0039] The fourth step is to tear off the polyimide film 1 so that the electric heating plate 2 remains on the base prepreg 4.

[0040] The fifth step is to uniformly heat the electric heating sheet 2 by a heating device so that the resin in the matrix prepreg 4 can penetrate into the gap of the electric heating sheet 2. The heating device is a hair dryer, and the heating temperature of the hair dryer is 50°C-80°C. Due to the high adhesion of the resin in the matrix prepreg, the electric heating sheet 2 and the matrix prepreg 4 can be basically bonded before curing by heating with a hair dryer.

[0041] In the sixth step, the composite material is continued to be laid on the electric heating sheet 2. After laying, the electric heating sheet 2 and the composite material are cured. The composite material is a skin material for the wings, rotors, air inlets and other parts, and is made of at least one of high-strength aluminum, magnesium alloy, titanium alloy and the like. The curing treatment is a heat treatment method, including any one of resistance heating, induction heating, arc heating, electron beam heating, infrared heating and the like.

[0042] Step 7: The electric heating plate 2 is tightly bonded to the composite material.

[0043] The cured electric heating sheet 2 has a high bonding strength with the composite material, so that the electric heating sheet 2 will not move after being laid on the composite material, and can also effectively improve the strength of the composite material after molding.

[0044] Before the first step, three layers of thermal insulation coating are evenly coated on the mold surface. The thermal insulation coating is any one of composite magnesium aluminum silicate thermal insulation coating, rare earth thermal insulation coating, and coating composite silicate thermal insulation coating. The thermal insulation coating makes the molding mold 5 not easily affected by the curing temperature.

[0045] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for improving the bonding strength between an electric heating sheet and a composite material, characterized in that: The steps include: The first step is to prepare a molding mold and lay the matrix prepreg on the molding mold; The second step is to bond the polyimide film to the electric heating sheet to make a polyimide film electric heating sheet; The third step is to place the polyimide film electric heating sheet with the electric heating sheet facing the base prepreg, and then evenly attach the polyimide film electric heating sheet to the base prepreg; Step 4: tear off the polyimide film, leaving the electric heating sheet on the base prepreg; The fifth step is to uniformly heat the electric heating sheet by a heating device so that the resin in the matrix prepreg can penetrate into the gap of the electric heating sheet; Step 6: Continue to lay the composite material on the electric heating sheet, and after laying, perform a curing treatment on the electric heating sheet and the composite material; Step 7: The electric heating sheet is tightly bonded to the composite material; Before the first step, the surface of the molding mold is evenly coated with three layers of thermal insulation coating, and the thermal insulation coating is specifically any one of composite magnesium aluminum silicate thermal insulation coating, rare earth thermal insulation coating, and coated composite silicate thermal insulation coating; The matrix prepreg is formed by impregnating a high-strength carbon fiber cloth reinforcement into a resin adhesive, wherein the resin adhesive is a bismaleimide resin adhesive or an epoxy resin adhesive. The composite material is a skin material for making wings, rotors, and air inlet parts, and is made of at least one of high-strength aluminum, magnesium alloy, and titanium alloy.

2. The method for improving the bonding strength between an electric heating sheet and a composite material according to claim 1, characterized in that: The heating device is a hair dryer, and the heating temperature of the hair dryer is 50°C-80°C.

3. The method for improving the bonding strength between an electric heating sheet and a composite material according to claim 1, characterized in that: The mass of the resin glue in the matrix prepreg accounts for 36%-42% of the total mass of the matrix prepreg.