Preparation method and application of aluminum-copper-carbon composite material for efficient reduction of nitrate to nitrogen
Through the ball milling process of aluminum-copper-carbon composite materials, copper catalysis and carbon are used to provide the Galvanic cathode effect, which solves the problem of zero-valent aluminum being difficult to continuously provide electrons under neutral conditions, and achieves efficient and selective reduction of nitrate to Nitrogen reduces treatment costs and avoids secondary pollution, and is suitable for a variety of water body restoration scenarios.
Patent Information
- Application Number
- CN202310099951.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-07
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-02-07
AI Technical Summary
When existing technologies treat nitrate pollution in water bodies, zero-valent aluminum metal is difficult to continuously provide electrons under near-neutral conditions, resulting in low nitrate reduction efficiency. Commonly used precious metal catalysts are costly, and electrochemical reduction methods consume a lot of energy. , there is a risk of secondary pollution.
The aluminum-copper-carbon composite material is formed through a ball milling process. The copper catalysis and carbon are used to provide the Galvanic cathode effect to achieve efficient and selective reduction of nitrate to nitrogen, avoiding the passivation of zero-valent aluminum and precious metals. of use.
It achieves efficient and selective reduction of nitrate under normal temperature and pressure, adapts to a wide pH range, reduces treatment costs, avoids secondary pollution, and is suitable for a variety of water body restoration scenarios.
Smart Images

Figure CN116062870B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water pollution treatment, and specifically relates to a preparation method of an aluminum-copper-carbon composite material for efficiently reducing nitrate to nitrogen, and also relates to an application of the aluminum-copper-carbon composite material in treating nitrate-containing wastewater. Background Art
[0002] The disorderly discharge of industrial wastewater and domestic sewage and the extensive use of agricultural nitrogen fertilizers have caused nitrates to become the main nitrogen-containing pollutants in groundwater, rivers and lakes. Excessive nitrate concentrations in the water environment can lead to eutrophication of water bodies and threaten human health. my country's "Sanitary Standards for Drinking Water" (GB 5749-2022) stipulates that the limit of nitrate in drinking water is 10 mg / L (in terms of N).
[0003] The ideal way to remove nitrates from water bodies is to convert them into harmless nitrogen. The existing methods for removing nitrates mainly include biological denitrification, physical methods and chemical reduction methods. Biological denitrification has high requirements for operating conditions, and there are also disadvantages such as secondary pollution caused by residual sludge and low resistance to shock loads. Physical technologies such as ion exchange, adsorption and membrane separation only enrich and transfer nitrates from water bodies, and further deep treatment is still required. Chemical reduction methods are divided into zero-valent metal reduction, hydrogen catalytic reduction and electrochemical reduction. The use of precious metal catalysts such as palladium and platinum in hydrogen catalytic reduction leads to extremely high water treatment costs. As an electron donor, hydrogen still has great hidden dangers in terms of cost, storage and transportation. The electrochemical reduction method has high energy consumption, and the active chlorine produced at the anode has the risk of secondary pollution. The zero-valent metal reduction method is low in cost, efficient and easy to operate, and has a wide range of adaptability. However, common metal materials (such as zero-valent iron) usually need to be active under acidic conditions, and the nitrate reduction products of metals such as zero-valent iron are mainly ammonia nitrogen, and the nitrogen selectivity is poor. Zero-valent aluminum metal has the advantages of active properties, strong reducing ability, and low price. However, zero-valent aluminum metal is easily passivated, and the oxide film formed on the surface makes it difficult for it to continuously provide electrons to promote the reduction reaction.
[0004] Therefore, it is of great practical significance to develop a new zero-valent metal material technology to achieve efficient and selective reduction of nitrate under near-neutral conditions. Summary of the invention
[0005] One of the purposes of the present invention is to provide a method for preparing an aluminum-copper-carbon composite material for highly efficient and selective chemical reduction of nitrate to nitrogen.
[0006] A second object of the present invention is to provide an aluminum-copper-carbon composite material for the efficient and selective chemical reduction of nitrates to nitrogen for use in the treatment of nitrate-containing wastewater.
[0007] The technical solution adopted by the present invention to achieve one of the purposes is: to provide a preparation method of an aluminum-copper-carbon composite material for efficiently reducing nitrate to nitrogen, comprising the following steps: placing acid-treated activated carbon, aluminum powder, copper powder and ball milling beads in a ball milling jar, sealing and evacuating the jar, and then filling with inert gas; performing ball milling treatment under an inert atmosphere to obtain the aluminum-copper-carbon composite material.
[0008] The present invention provides a method for preparing an aluminum-copper-carbon composite material that can achieve efficient step-by-step selective reduction and removal of nitrate-nitrite-nitrogen by coupling active hydrogen reduction and direct electron transfer processes. In the preparation method, the synergistic effect of the three materials of copper, carbon and aluminum is utilized, and a ball milling process is adopted to achieve the depassivation of aluminum metal and continuous supply of electrons. Copper serves as a catalytic active center for converting nitrate into nitrous acid, and the carbon material provides a galvanic cathode effect to ensure the alkaline dissolution of aluminum, and provides a reduction site for highly selectively reducing nitrate to nitrogen.
[0009] Furthermore, the present invention uses acid-treated activated carbon as a raw material, and pre-treats the activated carbon with dilute acid, which can remove surface impurities and improve hydrophobicity. Preferably, the method for preparing the acid-treated activated carbon includes: firstly impregnating the activated carbon with dilute acid, then washing it with pure water, and then drying it. The dried carbon material, copper powder and aluminum powder are mechanically ball-milled under the action of ball milling beads in a certain mass ratio to obtain an aluminum-copper-carbon composite material. During the ball milling process, the aluminum powder, copper powder and ball milling beads abrade the metal surface during high-speed collisions to form dislocation defects, thereby destroying the passivation layer on the surface of the metal powder and exposing a fresh active metal surface.
[0010] Preferably, the concentration of the dilute acid is 20 to 50 mmol / L, the soaking time is 0.5 to 2 hours, and the pH of the effluent from the pure water cleaning is 5.5 to 6.2. Furthermore, the dilute acid is selected from dilute hydrochloric acid or dilute sulfuric acid.
[0011] Preferably, the activated carbon is selected from one or more combinations of coconut shell activated carbon, wood activated carbon, fruit shell activated carbon and coal activated carbon. Such activated carbon materials have a large specific surface area and rich functional groups.
[0012] Preferably, the inert gas is selected from one of nitrogen, argon or helium.
[0013] Preferably, the purity of the aluminum powder is 95-99%, and the particle size is 50-2000 mesh; the purity of the copper powder is 95-99%, and the particle size is 20-2000 mesh. There are risks in the storage and transportation process of metal powders with too small particle size, and metal powders with too large particle size have a small specific surface area and low reaction activity.
[0014] Preferably, the mass ratio of the activated carbon, aluminum powder and copper powder after the acid treatment is (1-10):1:(0.2-5). More preferably, the mass ratio of the activated carbon, aluminum powder and copper powder after the acid treatment is (3-6):1:1. Under this ratio condition, the obtained aluminum-copper-carbon composite material has a stronger selectivity for reducing nitrate to nitrogen when treating wastewater containing nitrate pollutants.
[0015] Preferably, the mass ratio of the ball milling beads to the material addition amount is (10-100):1; in some better embodiments, the ball milling beads are composed of ball milling beads with particle sizes of 6 mm, 10 mm and 15 mm in a quantitative ratio of 15:5:1.
[0016] Furthermore, the ball milling equipment is a planetary ball mill; the ball milling speed is 200-500 rpm, and the ball milling time is 1-20 hours. Preferably, the ball milling speed is 400 rpm, and the ball milling time is 3 hours.
[0017] Furthermore, the storage condition of the aluminum-copper-carbon composite material is: storage under nitrogen protection conditions.
[0018] The technical solution adopted by the present invention to achieve the second purpose is: to provide an aluminum-copper-carbon composite material prepared by the preparation method described in one of the purposes of the present invention for use in treating wastewater containing nitrates.
[0019] Furthermore, the concentration of nitrate in the wastewater is 10 to 2000 mg / L (in terms of N), and the pH of the wastewater is 3 to 11. Preferably, the reaction temperature for treating the wastewater containing nitrate is 10 to 30°C.
[0020] Furthermore, the dosage of the aluminum-copper-carbon composite material in the wastewater containing nitrate is 1 to 30 g / L.
[0021] In the present invention, as shown in formula 1-4, the aluminum-copper-carbon composite material is used to reduce nitrate in water, and mainly undergoes a two-stage reaction process: (1) the aluminum powder with an active surface exposed after ball milling reacts rapidly with water to produce hydrogen, and the hydrogen produces active hydrogen (H*) under the catalytic action of copper. Since copper has a good nitrate adsorption capacity and a weak nitrite adsorption capacity, the active hydrogen will reduce the nitrate adsorbed on the copper surface to nitrite; aluminum and activated carbon will form a microscopic corrosion galvanic cell, aluminum will gradually dissolve as an anode and release electrons, and the carbon surface as a cathode will undergo a hydrolysis reaction, and the generated OH -This will cause the pH on the carbon surface to rise, forming a local alkaline environment, and this phenomenon is named the "Galvanic cathode effect"; (2) The local alkaline environment on the surface of activated carbon will maintain the activity of aluminum and continue to release electrons. At the same time, the generation rate of H* under alkaline conditions is inhibited. Activated carbon with a large specific surface area acts as a cathode and efficiently and selectively reduces nitrite to nitrogen through a direct electron transfer process.
[0022] Anode reaction: Al-3e - =Al 3+ E 0 (Al 3+ / Al)=-1.66V (Formula 1)
[0023] Cathode reaction (on carbon material): 2H2O+2e - =H2+2OH - (Formula 2)
[0024] Nitrate step reduction reaction:
[0025] NO3 - +2H ads =NO2 - +H20 (Formula 3)
[0026] NO2 - +H2O+e - =N2+OH - (Formula 4)
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) The present invention provides a method for preparing an aluminum-copper-carbon composite material, wherein the aluminum-copper-carbon composite material is obtained by ball milling acid-treated activated carbon, aluminum powder, and copper powder. The preparation method is carried out at room temperature and pressure, the synthesis process is simple, the reaction conditions are mild, and it is suitable for industrial preparation and production. In addition, the carbon material, aluminum powder, and copper powder used can be industrial-grade raw materials, the material price is low and easy to obtain, and can be used on a large scale, effectively controlling the cost of treating wastewater.
[0029] (2) The aluminum-copper-carbon composite material provided by the present invention is suitable for treating nitrates in wastewater. It can utilize the galvanic cathode effect to form a local alkaline environment to promote aluminum activation. Zero-valent aluminum can be continuously dissolved without passivation, effectively solving the practical problem of zero-valent aluminum materials in the field of environmental remediation. In addition, the composite material generates hydrogen in situ by means of the synergistic effect of aluminum, copper, and carbon, and couples the active hydrogen reduction and direct electron transfer processes to achieve step-by-step, efficient, and selective reduction of nitrates. At the same time, copper does not dissolve, avoiding secondary pollution.
[0030] (3) The aluminum-copper-carbon composite material provided by the present invention can adapt to a wider pH range (3 to 11), and can still maintain good activity properties and pollutant removal capabilities in the presence of dissolved oxygen and interference from multiple ions. It can efficiently and selectively chemically reduce nitrate to nitrogen gas and can be applied to a variety of water body remediation scenarios. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 A schematic diagram of the principle of highly efficient and selective chemical reduction of nitrates into nitrogen by the aluminum-copper-carbon composite material provided by the present invention;
[0032] Figure 2 The microscopic morphology and energy spectrum analysis of the aluminum-copper-carbon composite material prepared in Example 1 of the present invention; wherein (a) is an EDs element map; (b) is a SEM map, and (c)-(f) are single element distribution maps;
[0033] Figure 3 The photos are of the aluminum-copper-carbon composite material prepared in Example 1 of the present invention and the aluminum-carbon material, copper-carbon material and aluminum-copper material prepared in Comparative Examples 2-4;
[0034] Figure 4 This is a comparison chart of the effects of the aluminum-copper-carbon composite material prepared in Example 1 of the present invention and the carbon material, aluminum-carbon material, copper-carbon material and aluminum-copper material prepared in Comparative Examples 1-4 for treating nitrate-containing wastewater;
[0035] Among them, (a) is a comparison chart of nitrate removal rate; (b) is a comparison chart of nitrite concentration change; (c) is a comparison chart of nitrogen selectivity and total nitrogen removal rate; (d) is an ESR chart of active hydrogen. DETAILED DESCRIPTION
[0036] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0038] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited thereto.
[0039] The main raw materials and parameters involved in Examples 1-8 and Comparative Examples 1-4 of the present invention are shown in Table 1 below:
[0040] Table 1
[0041]
[0042]
[0043] Among the raw materials in the above table, the particle size of aluminum powder is 80-150μm, and the purity is 99%; the particle size of copper powder is 10-20μm, and the purity is 99%; the activated carbon is soaked in dilute sulfuric acid or dilute hydrochloric acid with a concentration of 20-50mmol / L for 0.5-2h, and then washed with pure water until the pH value of the outlet water is 5.5-6.2.
[0044] Example 1
[0045] In a stainless steel ball mill with a volume of 100 mL, ball mill beads (agate beads) with diameters of 15 mm, 10 mm, and 6 mm were added in a ratio of 1:5:15; 2.5 g coconut shell activated carbon, 0.5 g aluminum powder, and 0.5 g copper powder were weighed into the ball mill respectively, that is, the mass ratio between aluminum, copper, and carbon was 1:1:5, and the mass ratio of the added material to the ball mill beads was 1:20. After the closed ball mill was evacuated, argon gas was introduced as a protective gas, and the ball mill was placed in a planetary ball mill with a speed of 400 rpm and a continuous ball milling time of 3 h. After ball milling, the obtained aluminum-copper-carbon composite material was taken out and placed under nitrogen protection.
[0046] The microstructure and energy spectrum analysis of the aluminum-copper-carbon composite material prepared in Example 1 are as follows: Figure 2 As shown in the figure, aluminum and copper metal components are well dispersed inside the activated carbon. The particle sizes of copper and aluminum after ball milling are between 10-30μm.
[0047] Example 2
[0048] On the basis of Example 1, an aluminum-copper-carbon composite material (AC:Al:Cu=3:1:1) was prepared according to the raw material ratios and parameters shown in Table 1, while other conditions remained unchanged, and the product was stored in nitrogen.
[0049] Example 3
[0050] On the basis of Example 1, an aluminum-copper-carbon composite material (AC:Al:Cu=4:1:1) was prepared according to the raw material ratios and parameters shown in Table 1, while other conditions remained unchanged, and the product was stored in nitrogen.
[0051] Example 4
[0052] On the basis of Example 1, an aluminum-copper-carbon composite material (AC:Al:Cu=6:1:1) was prepared according to the raw material ratios and parameters shown in Table 1, while other conditions remained unchanged, and the product was stored in nitrogen.
[0053] Example 5
[0054] On the basis of Example 1, an aluminum-copper-carbon composite material (AC:Al:Cu=5:3:1) was prepared according to the raw material ratios and parameters shown in Table 1, while other conditions remained unchanged, and the product was stored in nitrogen.
[0055] Example 6
[0056] On the basis of Example 1, an aluminum-copper-carbon composite material (AC:Al:Cu=5:1:3) was prepared according to the raw material ratios and parameters shown in Table 1, while other conditions remained unchanged, and the product was stored in nitrogen.
[0057] Example 7
[0058] On the basis of Example 1, an aluminum-copper-carbon composite material (AC:Al:Cu=5:5:1) was prepared according to the raw material ratios and parameters shown in Table 1, while other conditions remained unchanged, and the product was stored in nitrogen.
[0059] Example 8
[0060] On the basis of Example 1, an aluminum-copper-carbon composite material (AC:Al:Cu=5:1:5) was prepared according to the raw material ratios and parameters shown in Table 1, and other conditions remained unchanged, and the product was stored in nitrogen.
[0061] Comparative Example 1
[0062] In a stainless steel ball mill with a volume of 100 mL, add ball milling beads (agate beads) with diameters of 15 mm, 10 mm, and 6 mm in a ratio of 1:5:15; weigh 2.5 g of coconut shell activated carbon into the ball mill, and the mass ratio of the added material to the ball milling beads is 1:20. After the sealed ball mill is evacuated, argon gas is introduced as a protective gas, and the ball mill is placed in a planetary ball mill with a speed of 400 rpm and a continuous ball milling time of 3 hours. After ball milling, take out the obtained carbon material and place it under nitrogen protection.
[0063] Comparative Example 2
[0064] In a stainless steel ball mill with a volume of 100 mL, add ball mill beads (agate beads) with diameters of 15 mm, 10 mm, and 6 mm in a ratio of 1:5:15; weigh 2.5 g coconut shell activated carbon and 0.5 g aluminum powder into the ball mill respectively, that is, the mass ratio between aluminum and carbon is 1:5, and the mass ratio of the added material to the ball mill beads is 1:20. After the closed ball mill is evacuated, argon gas is introduced as a protective gas, and the ball mill is placed in a planetary ball mill with a speed of 400 rpm and a continuous ball milling time of 3 hours. After ball milling, take out the obtained aluminum-carbon material and place it under nitrogen protection.
[0065] Comparative Example 3
[0066] In a stainless steel ball mill with a volume of 100 mL, ball mill beads (agate beads) with diameters of 15 mm, 10 mm, and 6 mm were added in a ratio of 1:5:15; 2.5 g coconut shell activated carbon and 0.5 g copper powder were weighed into the ball mill respectively, that is, the mass ratio between copper and carbon was 1:5, and the mass ratio between the added material and the ball mill beads was 1:20. After the closed ball mill was evacuated, argon gas was introduced as a protective gas, and the ball mill was placed in a planetary ball mill with a speed of 400 rpm and a continuous ball milling time of 3 hours. After ball milling, the copper-carbon material obtained was taken out and placed under nitrogen protection.
[0067] Comparative Example 4
[0068] In a stainless steel ball mill with a volume of 100 mL, ball mill beads (agate beads) with diameters of 15 mm, 10 mm, and 6 mm were added in a ratio of 1:5:15; 0.5 g of aluminum powder and 0.5 g of copper powder were weighed into the ball mill respectively, that is, the mass ratio between aluminum and copper was 1:1, and the mass ratio of the added material to the ball mill beads was 1:20. After the closed ball mill was evacuated, argon gas was introduced as a protective gas, and the ball mill was placed in a planetary ball mill with a speed of 400 rpm and a continuous ball milling time of 3 hours. After ball milling, the copper-aluminum material obtained was taken out and placed under nitrogen protection.
[0069] The physical pictures of the products obtained in Example 1 and Comparative Examples 2-4 are as follows Figure 3 Due to the cold welding effect of zero-valent aluminum, the copper-aluminum sample of comparative example 4 is in the form of metal flakes after ball milling, while the carbon-containing materials of embodiment 1, comparative examples 2 and 3 have better dispersibility.
[0070] Performance Testing
[0071] (I) Test of treatment capacity of wastewater containing nitrates
[0072] Prepare 100mL of 30mg / L NO3 - -N simulated wastewater was prepared in multiple portions without adjusting the initial pH of the solution (approximately 6.7). 20 g / L of the aluminum-copper-carbon composite material prepared in Examples 1-8, and the carbon, aluminum-carbon, copper-carbon and aluminum-copper materials prepared in Comparative Examples 1-4 were added to the serum bottles respectively (the amount added was consistent with the mass of each component contained in the aluminum-copper-carbon composite material of Example 1). The serum bottle was sealed and placed in a constant temperature water bath oscillator. The temperature was set to 25°C, the speed was set to 200 rpm, and the reaction time was 8 hours. 1.5 mL of sample was taken at regular intervals and filtered with a 0.22 micron polyethersulfone filter head. The concentrations of nitrate and nitrite were detected by ion chromatography, and the concentration of ammonia nitrogen was detected by ultraviolet spectrophotometer. The results are shown in Table 2 and Figure 4 shown.
[0073] Table 2
[0074]
[0075] As can be seen from the above table,
[0076] When the aluminum-copper-carbon composite material prepared in Examples 1-8 is used to treat wastewater containing nitrate, the nitrite removal rate is 100%, the total nitrogen removal rate is 60.1-87.7%, and the nitrogen selectivity is 60.1-87.7% after 8 hours of treatment at a dosage of 20 g / L.
[0077] Examples 2-4 adjusted the ratio of carbon and aluminum based on Example 1, and Examples 5-8 adjusted the ratio of aluminum and copper based on Example 1. By comparison, when the masses of carbon, aluminum and copper were controlled to be (3-6):1:1, the selectivity of the obtained aluminum-copper-carbon composite material for chemical reduction of nitrate to nitrogen was relatively higher (75.1-87.7%), and Example 1 (AC:Al:Cu=5:1:1) had the highest selectivity.
[0078] Furthermore, Figure 4 A comparison chart showing the effects of the aluminum-copper-carbon composite material prepared in Example 1 of the present invention and the carbon material, aluminum-carbon material, copper-carbon material and aluminum-copper material prepared in Comparative Examples 1-4 for treating nitrate-containing wastewater is shown.
[0079] like Figure 4 As shown in a-4c, the aluminum-copper-carbon composite material prepared in Example 1 can completely remove 30 mg / L of NO3 within 8 hours. - -N, the nitrite concentration gradually increased with the increase of reaction time in the first 6 hours, and was quickly reduced and removed by activated aluminum in 7-8 hours, while the removal effect of other comparative materials was poor. Further, the change of nitrite concentration in the solution verified the step-by-step reduction process of nitrate by the aluminum-copper-carbon material prepared by the present invention, and the ammonia nitrogen production (in terms of N) was 3.7 mg / L, the total nitrogen removal rate was 87.7%, and the nitrogen selectivity was as high as 87.7%.
[0080] like Figure 4 As shown in Figure d, during the reduction of nitrate by the aluminum-copper-carbon composite material, there was an obvious active hydrogen response peak in the first 4 hours, and the DMPO-H* response peak weakened rapidly at the 7th hour. This indicates that with the formation of a local alkaline environment, active hydrogen contributes less to nitrate reduction.
[0081] (II) Treatment capacity test of wastewater containing different concentrations of nitrate
[0082] Prepare 100mL of NO with concentrations of 50, 100, 300, and 500mg / L respectively. 3--N simulated wastewater samples 1-4, without adjusting the initial pH of the solution (about 6.7), add 20g / L of the aluminum-copper-carbon composite material prepared in Example 1 to the serum bottle. The serum bottle was sealed and placed in a constant temperature water bath oscillator, the temperature was set to 25°C, the speed was set to 200rpm, and the reaction time was 10h. 1.5mL was sampled regularly and filtered with a 0.22 micron polyethersulfone filter head, the nitrate and nitrite concentrations were detected by ion chromatography, and the ammonia nitrogen concentration was detected by ultraviolet spectrophotometer. The test results are shown in Table 3.
[0083] Table 3
[0084]
[0085]
[0086] As can be seen from the above table,
[0087] When the nitrate concentration is increased to 50 mg / L, the nitrate removal rate can still be maintained at 100%, and the nitrogen selectivity exceeds 80%. When the nitrate concentration is further increased, due to insufficient active metals and a shorter reaction time, the nitrate removal rate and nitrogen selectivity both decrease accordingly. Therefore, for high-concentration nitrate wastewater, the dosage of aluminum-copper-carbon materials can be increased accordingly and the reaction time can be extended to obtain better nitrate removal effects and nitrogen selectivity.
[0088] (III) Reducibility test under different pH conditions
[0089] Prepare 100mL of 30mg / L NO3 - -N simulated wastewater was placed in a serum bottle, and the pH values were adjusted to 3, 5, 9 and 11 respectively using sodium hydroxide and sulfate. According to the dosage of 20g / L, the aluminum-copper-carbon composite material prepared in Example 1 (the mass ratio of carbon-copper-aluminum was 5:1:1) was added to the serum bottle respectively. The serum bottle was sealed and placed in a constant temperature water bath oscillator, the temperature was set to 25°C, the speed was set to 200rpm, and the reaction time was 8h. 1.5mL was sampled regularly and filtered with a 0.22 micron polyethersulfone filter head. The concentrations of nitrate and nitrite were detected by ion chromatography, and the concentration of ammonia nitrogen was detected by ultraviolet spectrophotometer. The results are shown in Table 2 below.
[0090] Table 4
[0091]
[0092] As can be seen from the above table,
[0093] The aluminum-copper-carbon composite material prepared by the present invention has good reducing performance in a wide pH range, and has a good reduction performance for NO3 in the range of pH = 5 to 11. -The removal rate of TN is relatively higher. In particular, for wastewater solutions with a pH of 3 to 11, the N2 selectivity is 64.2 to 85.2%, which fully demonstrates that the aluminum-copper-carbon composite material prepared by the present invention has the advantage of highly efficient and selective chemical reduction of nitrates to nitrogen in a wide pH range.
[0094] The above are only preferred embodiments of the present invention, and are not intended to limit the implementation methods and protection scope of the present invention. Those skilled in the art should be aware that all solutions obtained by equivalent substitutions and obvious changes made using the contents of the specification of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an aluminum-copper-carbon composite material for efficiently reducing nitrate to nitrogen, comprising the following steps: The acid-treated activated carbon, aluminum powder, and copper powder are placed in a ball mill jar at a mass ratio of (3-6):1:1 together with ball mill beads. After being sealed and evacuated, an inert gas is introduced. Ball milling is performed under an inert atmosphere to obtain an aluminum-copper-carbon composite material.
2. The preparation method according to claim 1, characterized in that: The method for preparing the acid-treated activated carbon comprises: firstly soaking the activated carbon with dilute acid, then washing it with pure water, and then drying it.
3. The preparation method according to claim 2, characterized in that: The concentration of the dilute acid is 20-50 mmol / L, the soaking time is 0.5-2 h, and the pH of the effluent from the pure water cleaning is 5.5-6.
2.
4. The preparation method according to claim 3, characterized in that: The activated carbon is selected from one or more combinations of coconut shell activated carbon, wood activated carbon, fruit shell activated carbon and coal activated carbon.
5. The preparation method according to claim 1, characterized in that: The purity of the aluminum powder is 95-99%, and the particle size is 50-2000 meshes.
6. The preparation method according to claim 1, characterized in that: The copper powder has a purity of 95-99% and a particle size of 20-2000 meshes.
7. The preparation method according to claim 1, characterized in that: The mass ratio of the ball milling beads to the material addition amount is (10-100):1; the ball milling beads are composed of ball milling beads with particle sizes of 6 mm, 10 mm and 15 mm in a quantity ratio of 15:5:
1.
8. The preparation method according to claim 1, characterized in that: The equipment for ball milling is a planetary ball mill; the rotation speed of the ball milling is 200-500 rpm, and the time of the ball milling is 1-20 hours.
9. An application of an aluminum-copper-carbon composite material prepared by the preparation method according to any one of claims 1 to 8 in treating wastewater containing nitrates, characterized in that: The dosage of the aluminum-copper-carbon composite material in wastewater containing nitrate is 1-30 g / L.