Diamond cutting fluid for silicon carbide wafer and preparation method thereof
By using diamond cutting fluid in the silicon carbide wafer cutting process, the problems of poor adhesion and suspension stability of the cutting fluid are solved, cutting accuracy and efficiency are improved, production costs are reduced, and suspension stability is quickly evaluated through yield value detection. Achieving efficient and easy-to-clean cutting results.
Patent Information
- Application Number
- CN202211594625.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-13
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-12-13
AI Technical Summary
During the silicon carbide wafer cutting process, there are problems such as TTV and WARP values that do not meet the requirements, line mark defects, low cutting fluid viscosity, poor suspension stability, and poor abrasive adhesion, which affect processing accuracy and efficiency.
An efficient and easy-to-clean diamond cutting fluid composed of diamond powder, thixotrope solution, base oil, dispersant and surfactant is used to ensure uniform dispersion of diamond powder through ultrasonic dispersion and high-speed emulsification dispersing machine, combined with yield value detection Methods to assess suspension stability.
It improves the suspension stability and cleaning performance of cutting fluid, extends the cycle life of abrasives, reduces waste liquid emissions and processing costs, simplifies the production process and shortens formula development time.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicon carbide cutting auxiliary materials, in particular to a diamond cutting liquid for silicon carbide wafers and a preparation method thereof. Background Art
[0002] Silicon carbide single crystal material is a representative of the third generation of semiconductor materials. With its excellent properties, it has a wide range of applications and broad application prospects. According to the use of the device, the silicon carbide single crystal polishing sheet is required to have high surface quality: smooth surface, low surface roughness, no defects, no damage, and excellent surface parameters such as TTV and Warp. The quality and precision of silicon carbide material processing will directly affect the performance of its device. However, silicon carbide material has a high hardness, which is only about 0.5 lower than the hardness of diamond; it has high chemical stability and hardly reacts with any strong acid or strong base. Therefore, this material also faces the current situation of high processing difficulty.
[0003] For the processing technology of silicon carbide materials, crystal cutting is a very critical link and plays a decisive role in the quality of wafers. At present, the common wafer cutting methods in the market include diamond wire cutting and oil sand wire cutting, but the saw kerf loss of diamond wire cutting is larger than that of oil sand wire cutting and the cutting accuracy is lower than that of oil sand wire cutting. Considering the high cost of single silicon carbide wafers, the cutting of silicon carbide wafers in the market is still mainly done by oil sand wire cutting.
[0004] At present, the common problems of wafers cut by wire cutting fluid in the market mainly include: TTV and WARP values do not meet the requirements, wire marks and other defects. The system containing inorganic suspending agents such as organic modified bentonite in the wire cutting fluid is difficult to clean in the later stage, and it is easy to cause abrasives to accumulate in the pipeline after the machine stops, forming waste residue in the later stage, affecting the processing accuracy and cutting life; the cutting fluid system without inorganic suspending agents generally has low system viscosity, poor suspension stability, easy sedimentation and stratification, poor adhesion of abrasives on the steel wire, and difficult to clean, which affects the processing efficiency. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a diamond cutting fluid for silicon carbide wafers and a preparation method thereof. The diamond cutting fluid is efficient and easy to clean. The diamond cutting fluid is composed of finely processed and controlled diamond cutting powder and a uniform and stable carrier, wherein the cutting fluid carrier is composed of base oil, thixotropic solution, dispersant, surfactant, oil antioxidant, etc. After the above substances are mixed evenly by a certain method, they can be used for multi-wire cutting of silicon carbide wafers. In addition, it is found that the yield value detection method of the diamond cutting fluid can shorten the judgment time of the suspension stability in the process of formula development and accelerate the progress of formula development.
[0006] The present invention is achieved through the following technical solutions:
[0007] A diamond cutting fluid for silicon carbide wafers, comprising the following raw materials by weight percentage: 8-20% diamond powder
[0008] Dispersant 0.5-2.5%
[0009] Surfactant 2-6%
[0010] Thixotropic solution 10-40%
[0011] Base oil 31.5-79.5%;
[0012] Wherein, the thixotropic solution comprises the following raw materials:
[0013] Vegetable oil 85-97%
[0014] Aluminum stearate 2-10% Oil antioxidant T501 1-5%;
[0015] Among them, the aluminum stearate has an effective ingredient content of not less than 99%; the oil antioxidant T501 is the oil additive T501 (the main ingredient is 2,6-di-tert-butyl-p-methylphenol).
[0016] Preferably, the diamond powder includes one or more of single crystal diamond, polycrystalline diamond, and aggregate diamond, with an average particle size of 0.5-40 um.
[0017] Preferably, the dispersant is DISPERBYK-2157, DISPER BYK-180, DISPER BYK-110,
[0018] One or more of DISPERBYK-P104S.
[0019] Preferably, the surfactant is one or more of tallow amine polyoxyethylene (5) ether, oleyl alcohol polyoxyethylene ether, dodecanol polyoxyethylene (3) ether, oleylamine polyoxyethylene (2) ether, and oleic acid triglyceride.
[0020] Preferably, the base oil is one or more of C10-C30 straight-chain alkanes, C10-C30 branched-chain alkanes, and C10-C30 cycloalkanes.
[0021] Preferably, the vegetable oil is one or more of peanut blended oil, rapeseed blended oil, and soybean oil.
[0022] Wherein, the preparation method of the thixotropic solution comprises the following steps:
[0023] (1) Weigh the required raw materials according to weight percentage: aluminum stearate, vegetable oil, and oil antioxidant T501;
[0024] (2) Mix aluminum stearate, vegetable oil, and oil antioxidant T501, stir and disperse by ultrasonic for 5-10 minutes to ensure that aluminum stearate is evenly dispersed in the vegetable oil without obvious large agglomerated particles;
[0025] (3) placing the solution obtained in step (2) in a high-speed emulsifying and dispersing machine for high-speed emulsification and dispersion for 5-10 minutes to ensure that the aluminum stearate is evenly dispersed;
[0026] (4) placing the solution obtained in (3) above in a heating device for heating and stirring at a temperature of 160-180° C. for a heating time of 2-8 hours to ensure that the aluminum stearate is evenly dispersed and completely dissolved in the vegetable oil;
[0027] (5) Allow to cool naturally to room temperature to obtain a thixotropic adhesive solution, which should be set aside for later use.
[0028] A method for preparing a diamond cutting fluid for a silicon carbide wafer comprises the following steps:
[0029] (1) The diamond powder is fine powder that has been finely classified and sieved to remove large particles;
[0030] (2) Weigh the required amount of dispersant, surfactant, thixotropic solution and base oil in proportion, and stir and mix them evenly by ultrasonic stirring;
[0031] (3) The solution obtained in (2) is dispersed in a high-speed shear emulsifier for 15-30 minutes;
[0032] (4) The solution obtained in (3) is stirred and placed in an ultrasonic wave for ultrasonic treatment.
[0033] The diamond powder in (1) is added into the system in proportion and then stirred and ultrasonically dispersed for 15-30 minutes to ensure that the diamond powder is evenly dispersed in the system without agglomerated particles.
[0034] A method for evaluating the suspension stability of a diamond cutting fluid for a silicon carbide wafer comprises the following steps:
[0035] (1) Prepare diamond cutting fluid for the silicon carbide wafer to be tested;
[0036] (2) Detect the viscosity of diamond cutting fluid for silicon carbide wafers, with rotation speeds of at least 0.3, 0.6, 1.5, 3, and 6;
[0037] (3) Calculate the yield value. The yield value calculation formula is: (V0.3-V1.5) / 100, where V0.3 is the viscosity of the diamond cutting fluid for silicon carbide wafer measured at a rotation speed of 0.3 r / min, and V1.5 is the viscosity of the diamond cutting fluid for silicon carbide wafer measured at a rotation speed of 1.5 r / min;
[0038] (4) If the yield value is higher than 40, the suspension stability of the diamond cutting fluid for silicon carbide wafers is excellent; the higher the yield value of the diamond cutting fluid for silicon carbide wafers, the better its suspension stability.
[0039] Due to the adoption of the above technical solution, the present invention has the following advantages compared with the prior art:
[0040] .This diamond cutting fluid for silicon carbide wafer solves the problems of poor adhesion and poor abrasive suspension of the currently common easy-to-clean suspension fluid, and solves the problems of increased viscosity of waste fluid, reduced number of cycles, and poor cleaning performance of cutting fluids with good suspension properties in the later stage;
[0041] . The diamond cutting fluid for silicon carbide wafers increases the number of cycle cutting and grinding while reducing the discharge of waste liquid and the processing cost;
[0042] 3. The production method of the diamond cutting fluid for silicon carbide wafers is simple and easy to mass produce;
[0043] 4. The method for determining the suspension stability of the diamond cutting fluid for silicon carbide wafers is simple to operate and can greatly shorten the research and development time of the formula. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0045] Example 1
[0046] A diamond cutting fluid for multi-wire cutting of silicon carbide wafers is prepared from the following raw materials in parts by weight:
[0047] The thixotropic adhesive solution is prepared from the following raw materials in parts by weight:
[0048] ① Thixotropic glue solution: Weigh the required raw materials according to the above proportions, mix and stir the Golden Dragon Fish Peanut Blended Oil with aluminum stearate and oil antioxidant T501 evenly, place it in a high-speed emulsifying disperser for emulsification and dispersion for 5 minutes, place the above solution in a 165℃ heating device for heating and stirring for 4 hours to ensure that the aluminum stearate in the container is completely dissolved and dispersed in the Golden Dragon Fish Peanut Blended Oil, and cool it to room temperature for use.
[0049] ② Diamond cutting fluid for multi-wire cutting of silicon carbide wafers: weigh the required raw materials except diamond powder according to the above proportions, mix and stir the raw materials evenly, place them in a high-speed emulsifying disperser for high-speed shear dispersion for 30 minutes, ensure that the system is mixed evenly without heterogeneous phases, then place them in an ultrasonic mixer for ultrasonic stirring, then weigh the required mass of diamond powder, add it to the above solution and continue stirring and ultrasonic dispersion for 20 minutes to ensure that the diamond powder is completely dispersed in the system.
[0050] Example 2
[0051] A diamond cutting fluid for multi-wire cutting of silicon carbide wafers is prepared from the following raw materials in parts by weight:
[0052] C14-C19 isoalkanes 67%;
[0053] The thixotropic solution is prepared from the following raw materials by weight: soybean oil 91%
[0054] Aluminum Stearate 8%
[0055] Oil antioxidant T501 1%.
[0056] The production steps are as follows:
[0057] ① Thixotropic glue solution: weigh the required raw materials according to the above proportions, mix and stir soybean oil with aluminum stearate and oil antioxidant T501, place in a high-speed emulsifier for emulsification and dispersion for 5 minutes, place the above solution in a 180℃ heating device for heating and stirring for 6 hours, ensure that the aluminum stearate in the container is completely dissolved and dispersed in the soybean oil, and cool to room temperature for use. ② Diamond cutting fluid for multi-wire cutting of silicon carbide wafers: weigh the required raw materials according to the above proportions except diamond powder, mix and stir the raw materials, place in a high-speed emulsifier for high-speed shear dispersion for 30 minutes, ensure that the system is evenly mixed and has no heterogeneous phases, and then place in an ultrasonic mixer for ultrasonic stirring, then weigh the required mass of diamond powder, add it to the above solution and continue to stir and ultrasonically disperse for 20 minutes to ensure that the diamond powder is completely dispersed in the system.
[0058] Comparative Example 1
[0059] A diamond cutting fluid for multi-wire cutting of silicon carbide wafers is prepared from the following raw materials in parts by weight:
[0060] ① Weigh the required raw materials as described above, mix and stir oleyl alcohol polyoxyethylene (3) ether, DISPERBYK-180, and C11-C17 straight-chain alkane;
[0061] ② Add diamond powder to the mixed solution obtained in ① above, and place the solution apparatus in ① above in ultrasonic wave, and perform ultrasonic and stirring dispersion for 20 minutes.
[0062] Comparative Example 2
[0063] A diamond cutting fluid for multi-wire cutting of silicon carbide wafers is prepared from the following raw materials in parts by weight:
[0064] ② Place the C14-C19 isoparaffin weighed in ① above in a heating device and heat it at 50°C.
[0065] ③ Add the weighed organic modified bentonite into the above solution ② and stir evenly until no large particles remain;
[0066] ④ Place the solution in ③ above in a high-speed emulsifying and dispersing machine for high-speed emulsification and dispersion for 20 minutes;
[0067] ⑤ Cool the above solution ④ naturally to room temperature;
[0068] ⑥ Add the weighed diamond powder into the above solution ⑤, turn on the stirring and ultrasonic device at the same time, stir and ultrasonic for 30 minutes until the abrasive is completely dispersed in the system.
[0069] Example 3
[0070] A method for evaluating the suspension stability of a diamond cutting fluid for a silicon carbide wafer comprises the following steps:
[0071] (1) Prepare diamond cutting fluid for the silicon carbide wafer to be tested;
[0072] (2) Use NDJ-8S (Shanghai Fangrui Instrument Co., Ltd.) to test the viscosity of diamond cutting fluid for silicon carbide wafers, with the rotation speeds at least including 0.3, 0.6, 1.5, 3, and 6;
[0073] (3) Calculate the yield value. The yield value calculation formula is: (V0.3-V1.5) / 100, where V0.3 is the viscosity of the diamond cutting fluid for silicon carbide wafers measured at a rotation speed of 0.3 r / min, which can be regarded as the viscosity of the solution that is closest to the static state that can be accurately detected at a rotation speed of 0 r / min or above. V1.5 is the viscosity of the diamond cutting fluid for silicon carbide wafers measured at a rotation speed of 1.5 r / min, which can be regarded as the viscosity of the solution at the beginning of its flow. The yield value reflects the force required for the fluid to just start flowing;
[0074] (4) If the yield value is higher than 40, the suspension stability of the diamond cutting fluid for silicon carbide wafers is excellent; the higher the yield value of the diamond cutting fluid for silicon carbide wafers, the better its suspension stability.
[0075] When the suspension stability evaluation method of diamond cutting fluid for silicon carbide wafer is used to test the suspension stability of multiple diamond cutting fluids to be tested, the yield value of each sample to be tested is calculated and compared. The sample with a high yield value has better suspension stability for abrasives.
[0076] Compared with the traditional method (judging the suspension stability of diamond cutting fluid by standing it for a long time), this evaluation method greatly saves time.
[0077] Test example
[0078] The silicon carbide wafer diamond cutting fluids described in Examples 1 and 2 and Comparative Examples 1 and 2 were subjected to the following tests respectively;
[0079] (1) The viscosity V6 was tested by NDJ-8S (Shanghai Fangrui Instrument Co., Ltd.), where V6 is the viscosity of the diamond cutting fluid for silicon carbide wafers measured at a rotation speed of 6 r / min;
[0080] (2) Determine the yield value according to the method described in Example 3;
[0081] (3) Leave it to stand for two weeks and observe and record its suspension stability during the period;
[0082] (4) Use a multi-wire cutting machine to perform multi-wire cutting on silicon carbide and collect application feedback results.
[0083] The above data are plotted into a table, as shown in Table 1;
[0084]
[0085] The results show that ① Example 1 and Example 2 have the best suspension stability for abrasives, and the corresponding yield values are higher; Comparative Example 2 is second, and Comparative Example 1 is the worst, with the smallest yield value, that is, the size of the yield value can verify the suspension stability of the cutting fluid formula for the abrasive; ② By comparing Example 1 with Comparative Example 1, it can be seen that the cutting fluid with excellent abrasive suspension stability has higher cutting efficiency and better wafer quality; ③ By comparing Example 2 with Comparative Example 2, it is found that when the suspension stability of the cutting fluid is slightly different, the cutting fluid of the present invention has more processing grinding times, that is, the same amount of cutting fluid has more cutting times, which can greatly reduce the amount of cutting fluid used and the amount of waste liquid discharged in the later stage, reduce production costs, and reduce environmental pollution; the cutting fluid of the present invention does not have the disadvantage of fast heating during the cutting process, and is easier to clean in the later stage.
[0086] The above is a further detailed description of the present invention in combination with a specific implementation method, and it cannot be determined that the specific implementation of the present invention is limited to this; for technical personnel in the technical field to which the present invention belongs and related technical fields, based on the technical solution of the present invention, the expansion and replacement of operating methods and data should all fall within the protection scope of the present invention.
Claims
1. A diamond cutting fluid for silicon carbide wafers, characterized in that: In terms of weight percentage, the following raw materials are included: Diamond powder 8-20% Dispersant 0.5-2.5% Surfactant 2-6% Thixotropic solution 10-40% Base oil 31.5-79.5%; Wherein, the thixotropic solution comprises the following raw materials: Vegetable oil 85-97% Aluminum stearate 2-10% Oil antioxidant T501 1-5%; The surfactant is one or more of tallow amine polyoxyethylene (5) ether, oleyl alcohol polyoxyethylene ether, dodecanol polyoxyethylene (3) ether, oleylamine polyoxyethylene (2) ether, and oleic acid triglyceride; The preparation method of the thixotropic solution comprises the following steps: (1) Weigh the required raw materials according to weight percentage: aluminum stearate, vegetable oil, and oil antioxidant T501; (2) Mix aluminum stearate, vegetable oil, and oil antioxidant T501, stir and disperse by ultrasonic for 5-10 minutes to ensure that aluminum stearate is evenly dispersed in the vegetable oil without obvious large agglomerated particles; (3) placing the solution obtained in step (2) in a high-speed emulsifying and dispersing machine for high-speed emulsification and dispersion for 5-10 minutes to ensure that the aluminum stearate is evenly dispersed; (4) placing the solution obtained in (3) above in a heating device for heating and stirring at a temperature of 160-180° C. for a heating time of 2-8 hours to ensure that the aluminum stearate is evenly dispersed and completely dissolved in the vegetable oil; (5) Allow to cool naturally to room temperature to obtain a thixotropic adhesive solution, which should be set aside for later use.
2. The diamond cutting fluid for silicon carbide wafer according to claim 1, characterized in that: The diamond powder includes one or more of single crystal diamond, polycrystalline diamond and aggregate diamond, and has an average particle size of 0.5-40 um.
3. The diamond cutting fluid for silicon carbide wafer according to claim 1, characterized in that: The dispersant is one or more of DISPERBYK-2157, DISPERBYK-180, DISPERBYK-110, and DISPERBYK-P104S.
4. The diamond cutting fluid for silicon carbide wafer according to claim 1, characterized in that: The base oil is one or more of C10-C30 straight-chain alkanes, C10-C30 branched-chain alkanes, and C10-C30 cycloalkanes.
5. The diamond cutting fluid for silicon carbide wafer according to claim 1, characterized in that: The vegetable oil is one or more of peanut blended oil, rapeseed blended oil and soybean oil.
6. A method for preparing a diamond cutting fluid for silicon carbide wafer according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) The diamond powder is fine powder that has been finely classified and sieved to remove large particles; (2) Weigh the required amount of dispersant, surfactant, thixotropic solution and base oil in proportion, and stir and mix them evenly by ultrasonic stirring; (3) The solution obtained in (2) is placed in a high-speed shear emulsifier and dispersed for 15-30 minutes; (4) The solution obtained in the above (3) is stirred and placed in an ultrasonic chamber for ultrasonic treatment. In this state, the diamond powder in the above (1) is added to the system in proportion and stirred and ultrasonically dispersed for 15-30 minutes to ensure that the diamond powder is evenly dispersed in the system without agglomerated particles.
Citation Information
Patent Citations
Emery line cutting liquid and preparation method thereof
CN103525532A
Cooling liquid for cutting polycrystalline silicon chip employing diamond wire
CN104342273A
Photovoltaic solar silicon wafer cutting liquid
CN105112133A
Wire-electrode cutting oil and preparation method thereof
CN105176647A
Water-soluble and oil-soluble diamond grinding liquid and preparation method thereof
CN105647475A