A difficult-to-deform large-size nickel-based high-temperature alloy bar and its preparation method
By optimizing the chemical composition and process of nickel-based high-temperature alloys, the problems of insufficient performance and high manufacturing costs of high-temperature alloys in the existing technology have been solved, and high-performance, difficult-to-deform large-size nickel-based high-temperature alloy rods have been prepared to meet the requirements of naval gas turbines. High temperature strength requirements and reduced costs.
Patent Information
- Application Number
- CN202111298581.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-04
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-11-04
AI Technical Summary
It is difficult to develop a high-strength deformation superalloy with higher comprehensive properties than GH4169 and comparable to powder metallurgy superalloys with existing technology to meet the high-temperature strength and thermal strength requirements of high-power naval gas turbines, and the existing high-temperature deformation is difficult Alloy manufacturing costs are higher.
By optimizing the chemical composition of nickel-based high-temperature alloys, reducing the Co and Cr content, adding Al, Ti, and Nb elements, increasing the γ' phase volume fraction and thermal stability, vacuum induction melting, vacuum electric arc furnace remelting, forging and heat treatment are adopted process to prepare high-performance, difficult-to-deform large-size nickel-based high-temperature alloy rods.
It achieves the reduction of alloy cost on the basis of ensuring high strength, improves the upper limit temperature and structural stability of the alloy, meets the high performance requirements of large ship gas turbines, and lays the foundation for the future application of nickel-based high-temperature alloys.
Smart Images

Figure SMS_3 
Figure SMS_7 
Figure SMS_8
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of difficult-to-deform nickel-based alloys, and more specifically, to a difficult-to-deform large-size nickel-based high-temperature alloy bar and a preparation method thereof. Background Art
[0002] High-temperature alloys refer to a type of alloy that can withstand certain stresses at temperatures above 600°C and has oxidation resistance and corrosion resistance. According to the matrix, they can be divided into iron-based, nickel-based and cobalt-based. According to the forming process, they are generally divided into three categories: deformed high-temperature alloys, cast high-temperature alloys, and powder metallurgy high-temperature alloys. Among them, nickel-based deformed high-temperature alloys are widely used in aerospace engines, gas turbines, oil and gas fields, and the automotive industry due to their excellent oxidation resistance and corrosion resistance as well as high high-temperature strength.
[0003] With the rapid development of the navy, the requirements for ship gas turbines, the core components of ships, are getting higher and higher. The existing 30MW gas turbine is the only medium and large power ship gas turbine currently available in my country, but its power can no longer meet the development needs of the next generation of naval ships. The 40MW high-power ship gas turbine will be the main model used by naval ships in the next 10 to 15 years; as the power of ship gas turbines increases, the working environment of the turbine disc becomes more severe and the operating temperature is also higher, and the corresponding high-temperature mechanical performance indicators such as high-temperature strength and thermal strength are also getting higher and higher. Taking the common turbine disk material as an example, GH4169 alloy is currently the most widely used turbine disk material in my country's aero-engines, but its operating temperature is below 650°C. If it exceeds 650°C, the structure will be unstable and fail. Although powder metallurgy high-temperature alloys are a manufacturing solution for high-performance turbine disks in the future, the powder metallurgy process is complex and the process is long, while the manufacturing cost of deformed high-temperature alloys is relatively low. According to the research progress of high-temperature alloys for turbine disks in recent years, the use of short-process, low-cost casting + forging deformation technology to prepare high-performance high-temperature alloys is the key development direction and trend in the future.
[0004] In the prior art, publication number CN103498075 A provides a difficult-to-deform high-temperature alloy and a preparation method thereof, the composition of which is controlled as shown in Table 1. The technology uses vacuum induction + vacuum arc remelting for smelting and casting into steel ingots; however, the diameter of the remelted ingot is small, only It cannot be used to produce large-sized plates, but can be used to produce cakes. Publication No. CN108441705 A provides a high-strength nickel-based high-temperature alloy, the composition of which is shown in Table 1 below. The alloy designed by this technology has better room temperature and high temperature strength and durability compared with GH4169 and FGH4097. However, the Co content in this alloy is relatively high, which leads to a corresponding increase in the manufacturing cost of the alloy.
[0005] Table 1 Alloy composition of prior art (wt%)
[0006]
[0007] Therefore, it is necessary to develop a high-strength deformable high-temperature alloy with higher comprehensive performance than GH4169 and equivalent to powder metallurgy high-temperature alloy to meet the use requirements of high-power shipboard gas turbines. Summary of the invention
[0008] In view of the above-mentioned defects existing in the prior art, the purpose of the present invention is to provide a large-size nickel-based high-temperature alloy bar that is difficult to deform and a preparation method thereof. By optimizing the alloy composition, the Co and Cr contents in the alloy are reduced on the basis of ensuring the high strength of the alloy, and Al, Ti, and Nb elements are added in combination to increase the volume fraction and thermal stability of the γ' phase, thereby increasing the upper limit temperature of the alloy. Vacuum induction melting, vacuum arc furnace remelting, homogenization treatment, forging, and heat treatment are used to obtain a deformable high-temperature alloy with high performance and good organizational stability, thereby ensuring the feasibility of the engineering application of the alloy and meeting the application requirements of ship gas turbines.
[0009] To achieve the above object, the present invention adopts the following technical solution:
[0010] The first aspect of the present invention provides a large-size nickel-based high-temperature alloy bar that is difficult to deform, comprising the following chemical components by weight percentage: C: 0.01-0.10%, Cr: 10.0-20.0%, Co: 9.0-14.0%, Al: 1.0-3.0%, Ti: 1.0-3.0%, Nb: 1.0-3.0%, Mo: 2.0-7.0%, W≤0.20%, B≤0.010%, N≤0.020%, O≤0.008%, Fe: 0.1-2.0%, and the balance is nickel and unavoidable impurities.
[0011] Preferably, C: 0.020-0.080%, Cr: 13.0-15.0%, Co: 9.0-11.0%, Al: 2.0-3.0%, Ti: 2.0-3.0%, Nb: 2.0-3.0%, Mo: 4.5-5.5%, N≤0.010%, O≤0.0050%, Fe≤1.0%.
[0012] Preferably, at room temperature, the tensile strength σ of the hard-to-deform large-size nickel-based high-temperature alloy rod is b ≥1500MPa, yield strengthσ 0.2 ≥1150MPa, elongation δ5 ≥21.5%, section shrinkage ψ ≥31.5%;
[0013] Under the conditions of a temperature of 650° C. and a pressure of 873 MPa, the elongation δ5 of the difficult-to-deform large-size nickel-based high-temperature alloy rod is ≥3.5 and the surface shrinkage ψ is ≥8%.
[0014] The second aspect of the present invention provides a method for preparing a large-size nickel-based high-temperature alloy bar that is difficult to deform as described in the first aspect of the present invention, comprising the following steps:
[0015] S1, smelting in a vacuum induction furnace, adding the main ingredients Ni, Cr, Co, Mo, and C at the same time, evacuating to below 2.7Pa, increasing the power to perform chemical reaction, refining after chemical reaction, adding alloying elements Ti, Al, Nb and B for alloying smelting, and then analyzing the composition of the molten steel. After reaching the target composition requirement, Ar is charged, Ni-Mg alloy is added, and steel is tapped and electrodes are cast after smelting;
[0016] S2, vacuum consumable smelting, cleaning the surface of the electrode and then performing vacuum consumable smelting to obtain a consumable ingot;
[0017] S3, forging, homogenizing the consumable ingot, and then forging the consumable ingot by multiple upsetting and drawing processes to obtain a large-sized bar, and polishing the surface of the large-sized bar;
[0018] S4, heat treatment, subjecting the large-sized rod to solid solution treatment and aging heat treatment, and finally obtaining the difficult-to-deform large-sized nickel-based high-temperature alloy rod.
[0019] Preferably, the step S1:
[0020] During the chemical process, the power is 300-1000kw; and / or
[0021] During the refining process, the refining temperature is 1480-1530° C. and the refining time is 30-60 min; and / or
[0022] During the alloying smelting process, the power is 200-600kw and the temperature is 1490-1520°C; and / or
[0023] After the Ar is filled, the pressure is 20-25 KPa; the amount of the Ni-Mg alloy added to each ton of molten steel is 5-9 kg; and after the Ni-Mg alloy is added, smelting is continued for 5-10 minutes.
[0024] Preferably, in the step S2, during the vacuum consumable smelting process, the melting rate is 3.5-5.5 kg / min.
[0025] Preferably, in step S3:
[0026] During the homogenization process, the consumable ingot is heated to 1130-1180° C. and kept at this temperature for more than 60 hours; and / or
[0027] During the forging process, the homogenized consumable ingot is heated to 1140-1160°C, upset to 1 / 2-2 / 3 of the original height of the consumable ingot, and then stretched by step-by-step cooling. The reheating temperature is gradually reduced from 1160°C to 1100°C, and the insulation time is ≥120min.
[0028] Preferably, in step S3, during the forging process, the start forging temperature is ≥1050°C, and the stop forging temperature is ≥1000°C.
[0029] Preferably, in step S4:
[0030] During the solution treatment process, the large-sized bars after polishing are heated to 1060-1100°C, kept at this temperature for 7-11 hours, and then taken out of the furnace and air-cooled;
[0031] During the aging treatment, the large-size bars after the solution treatment are heated to 750-790° C., kept at this temperature for 14-19 hours, and then taken out of the furnace and air-cooled.
[0032] The chemical composition design principle of the difficult-to-deform large-size nickel-based high-temperature alloy bar of the present invention is as follows:
[0033] C: C is an important grain boundary and interdendritic strengthening element in high temperature alloys, and is an essential element for the formation of carbides; when the C content in the alloy is less than 0.01wt%, the number of carbides in the alloy will be small, which is not conducive to grain refinement and performance improvement; when the C content is too high, excessive carbide formation and increased segregation tendency will result in uneven grains and deteriorate alloy plasticity. Therefore, the C content is controlled within the range of 0.01-0.10wt%, preferably within the range of 0.02-0.08wt%.
[0034] Cr: The addition of Cr can improve the high temperature oxidation resistance and corrosion resistance of the alloy, and promote the formation of single-phase austenite solid solution; when the Cr content in the alloy is not less than 10%, the antioxidant and corrosion resistance of Cr can be fully exerted, but too high Cr content in the alloy will lead to the formation of σ phase, thereby deteriorating the performance of the alloy. In order to ensure the comprehensive performance of the alloy and inhibit harmful phases, the range of Cr is controlled to be 10.0-20.0wt%, preferably 13.0-15.0wt%.
[0035] Co: Co can form substitutional solid solution with Ni, which can play a role in solid solution strengthening. Adding Co to the alloy can reduce the stacking fault energy of the matrix, thereby improving the alloy's endurance strength and creep resistance. However, adding too much Co will also have disadvantages. On the one hand, it will lead to the precipitation of harmful phases. On the other hand, Co is a strategic resource. Adding too much Co to the alloy will increase the cost. Therefore, the range of Co is controlled at 9.0 to 14.0 wt%, preferably at 9.0 to 11.0 wt%.
[0036] Al: Al is an essential element for forming γ′ phase in nickel-based alloys. The higher the Al content, the greater the precipitation amount, the better the precipitation strengthening effect, and the corresponding strength of the alloy. However, too high Al content will increase the difficulty of hot working and easily cause cracking. Therefore, the Al content is controlled within the range of 1.0 to 3.0 wt%, preferably within the range of 2.0 to 3.0 wt%.
[0037] Ti: Ti is also an essential element for the formation of γ′ phase. When it dissolves into γ′ phase, it can replace two-thirds of Al atoms. After Ti enters γ′, it slows down the precipitation of γ′ and effectively prevents the effect of over-aging. This effect enables the alloy to serve for a long time in a high temperature environment. However, if too much Ti is added, coarse and flake η-Ni3Ti phase will appear, making the alloy brittle and reducing strength and plasticity. Therefore, the range of Ti is controlled to be 1.0-3.0wt%, and the preferred range is 2.0-3.0wt%.
[0038] Nb: Nb has a strong affinity with C. The addition of Nb will promote the precipitation of carbides, thereby refining the grains and strengthening the grain boundaries. In addition to combining with C, most of the Nb element enters the γ′ phase, reducing the amount of Al and Ti dissolved in the matrix, promoting the precipitation of the γ′ phase, delaying the aggregation and growth of the γ′ phase, and increasing the strength and dissolution temperature of the γ′ phase. In general, the Nb element can increase the use temperature of the alloy. However, excessive addition of Nb elements will easily lead to segregation during the smelting process, such as metallurgical defects such as black spots. Therefore, the range of Nb is controlled to be 1.0 to 3.0wt%, and the range of 2.0 to 3.0wt% is preferred.
[0039] Mo: Mo element is mainly dissolved into the matrix g phase. The atomic radius of Mo is much larger than that of Ni, which plays a solid solution strengthening effect and improves the corrosion resistance and high temperature stability of the alloy. However, too much Mo will cause the TCP phase to precipitate and deteriorate the mechanical properties of the alloy. Considering comprehensively, the Mo content is controlled within 2.0-7.0wt%, preferably within the range of 4.5-5.5wt%.
[0040] B: B is a grain boundary strengthening element, mainly distributed in the form of borides at grain boundaries and between columnar crystals and plays a strengthening role; the addition of B element can significantly improve the high temperature endurance and creep life of the alloy, but too much B will significantly deteriorate the hot working properties of the alloy and also make the welding process performance of the alloy worse. Taking comprehensive considerations, the B content is controlled within 0.010wt%.
[0041] N, O: The control of N and O in the alloy is a highlight of the composition design of the present invention. By controlling the interstitial elements, especially N and O, the fatigue performance of the alloy is improved significantly. Therefore, the present invention selects to control according to N≤0.020wt%, O≤0.0080wt%, preferably controlling the range of N≤0.010wt%, and preferably controlling O≤0.0050wt%.
[0042] Fe: The addition of Fe is mainly for the utilization of Fe-containing high-temperature alloy return materials and to reduce the cost of vacuum induction smelting; however, adding too much return materials will cause the Fe content in the alloy to exceed the standard. Therefore, the Fe content is ≤1.0wt% after comprehensive consideration, and the Fe content is preferentially controlled within 0.1-2.0wt%.
[0043] The present invention has the following beneficial effects:
[0044] 1. The large-size nickel-based high-temperature alloy bar with difficulty in deformation and the preparation method thereof of the present invention optimizes the alloy composition, reduces the content of Co and Cr in the alloy on the basis of ensuring the high strength of the alloy, and adds Al, Ti and Nb elements in combination to increase the volume fraction and thermal stability of the γ' phase, thereby increasing the upper limit temperature of the alloy;
[0045] 2. The method for preparing large-size nickel-based high-temperature alloy bars that are difficult to deform of the present invention adopts the preparation processes of vacuum induction melting, vacuum arc furnace remelting, consumable ingot homogenization treatment, forging, and heat treatment to obtain large-size nickel-based high-temperature alloy bars that are difficult to deform with high performance and good organizational stability. It can not only meet the use requirements of large-scale ship gas turbines for high-performance nickel-based high-temperature alloys, but also lay a solid foundation for the future application research of difficult-to-deform nickel-based high-temperature alloys in my country. DETAILED DESCRIPTION
[0046] In order to better understand the above technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with embodiments.
[0047] The invention discloses a large-size nickel-based high-temperature alloy bar that is difficult to deform and a preparation method thereof, comprising the following chemical components by weight percentage: C: 0.01-0.10%, Cr: 10.0-20.0%, Co: 9.0-14.0%, Al: 1.0-3.0%, Ti: 1.0-3.0%, Nb: 1.0-3.0%, Mo: 2.0-7.0%, W≤0.20%, B≤0.010%, N≤0.020%, O≤0.008%, Fe: 0.1-2.0%, and the balance is nickel and inevitable impurities. In a preferred embodiment, C: 0.020-0.080%, Cr: 13.0-15.0%, Co: 9.0-11.0%, Al: 2.0-3.0%, Ti: 2.0-3.0%, Nb: 2.0-3.0%, Mo: 4.5-5.5%, N≤0.010%, O≤0.0050%, Fe: 0.1-1.0%.
[0048] The above-mentioned large-size nickel-based high-temperature alloy bar that is difficult to deform has a tensile strength of σ b ≥1500MPa, yield strengthσ 0.2 ≥1150MPa, elongation δ5≥21.5%, and cross-sectional shrinkage ψ≥31.5%; under the conditions of temperature of 650℃ and pressure of 873MPa, the elongation δ5≥3.5 and cross-sectional shrinkage ψ≥8% of the difficult-to-deform large-size nickel-based high-temperature alloy rod.
[0049] The method for preparing the above-mentioned large-size nickel-based high-temperature alloy bar that is difficult to deform comprises the following steps:
[0050] S1, smelting in a vacuum induction furnace, adding the main ingredients Ni, Cr, Co, Mo, and C at the same time, evacuating to below 2.7Pa, increasing the power to perform chemical reaction, refining after chemical reaction, adding alloying elements Ti, Al, Nb and B for alloying smelting, and then analyzing the composition of the molten steel. After reaching the target composition requirement, Ar is charged, Ni-Mg alloy is added, and steel is tapped and electrodes are cast after smelting;
[0051] The specific process is as follows: according to the chemical composition of the large-size nickel-based high-temperature alloy bar that is difficult to deform, the proportion is made, and then the main material elements Ni, Cr, Co, and Mo are added, and C is added at the same time, and high vacuum and high-power smelting is carried out to ensure that the vacuum degree in the vacuum induction furnace is lower than 2.7Pa during the smelting process, and the power is increased to 300-1000kw to ensure that the O and N contents in the molten steel are reduced to the control requirements, and the C content is added according to the middle limit and the lower limit; after the material is quenched, the temperature is increased to 1480-1530℃ for refining, and the refining time is about 30-60min; then the power is reduced to 200-600kw, the temperature of the molten steel is reduced to 1490-1520℃, and the slag on the surface of the molten steel is paid attention to, and the alloying elements Ti, Al, Nb and B are added for alloying smelting; then samples are taken to analyze the composition of the molten steel. When Ni, Co, After the contents of Cr, Mo, Al, Ti, Nb, B and trace elements reach the target composition requirements, Ar is charged at a pressure of 20-25KPa, and Ni-Mg alloy is added, wherein the amount of Ni-Mg alloy added to each ton of molten steel is 5-9kg. After smelting for 5-10 minutes, steel is tapped and electrodes are cast;
[0052] S2, vacuum consumable smelting, cleaning the surface of the electrode and then performing vacuum consumable smelting to obtain a consumable ingot;
[0053] The specific process is: the surface of the electrode cast in step S1 is cleaned and ground to remove stains, scale, water stains, etc., and then vacuum consumable smelting is performed with the shrinkage hole of the electrode head facing upward, and the melting rate is set to 3.5-5.5 kg / min to finally obtain a consumable ingot; wherein the electrode can be annealed before the electrode surface is cleaned.
[0054] S3, forging, homogenizing the consumable ingot, and then forging the consumable ingot by multiple upsetting and drawing processes to obtain a large-sized bar, and polishing the surface of the large-sized bar;
[0055] The specific process is: heat the consumable ingot in the heating furnace for 22 to 28 hours, slowly increase the heating temperature from 480 to 530°C to 1130 to 1160°C, and keep it for more than 60 hours for homogenization and diffusion treatment, and peel and finish the consumable ingot after it is taken out of the furnace. Then heat the finished consumable ingot to 1140 to 1160°C and keep it for 7 to 11 hours before forging. Use multiple upsetting and drawing processes for forging, first upsetting to 1 / 2 to 2 / 3 of the original height of the consumable ingot, then use step-by-step cooling and drawing, return to the furnace and reheat the temperature gradually from 1160°C to 1100°C, keep it for ≥120 minutes, and finally forge large-sized bars, and polish the surface of the large-sized bars; during the forging process, the start forging temperature is ≥1050°C, and the stop forging temperature is ≥1000°C.
[0056] S4, heat treatment, subjecting the large-sized rod to solid solution treatment and aging heat treatment, and finally obtaining the difficult-to-deform large-sized nickel-based high-temperature alloy rod.
[0057] The specific process is: large-sized bars are subjected to solution treatment and aging heat treatment to finally obtain large-sized nickel-based high-temperature alloy bars that are difficult to deform. During the solution treatment process, the large-sized bars after polishing are heated to 1060-1100°C, kept warm for 7-11 hours, and then taken out of the furnace for air cooling; during the aging treatment process, the large-sized bars after solution treatment are heated to 750-790°C, kept warm for 14-19 hours, and then taken out of the furnace for air cooling. After that, the prepared large-sized nickel-based high-temperature alloy bars that are difficult to deform are subjected to flaw detection and physical and chemical property tests, and are stored in the warehouse after meeting the standards.
[0058] The difficult-to-deform large-size nickel-based high-temperature alloy rod and its preparation method of the present invention are further introduced below with reference to specific examples.
[0059] Example
[0060] According to the preparation method of the difficult-to-deform large-size nickel-based high-temperature alloy rod of the present invention, three furnaces of alloy are produced. In the specific preparation process, a 12-ton vacuum induction furnace and a 10-ton vacuum consumable furnace are used for smelting, and then the consumable ingot is homogenized, forged, and subjected to "solid solution + aging" heat treatment to obtain the difficult-to-deform large-size nickel-based high-temperature alloy rod. The specific process is as follows:
[0061] 1) 12 tons vacuum induction furnace smelting
[0062] Select high-purity metal Ni, Cr, Co and W raw materials, remove rust and clean the surface of raw material blocks without oil stains. The main elements Ni, Cr, Co, and W are added according to the target composition, and special attention is paid to the substitution of Si, Mn, and Cu, and C is added according to the middle and lower limits; vacuum is evacuated to below 2.6Pa, and the power is increased to control the power at 300-1000kw. Raise the temperature to 1480-1530℃ for refining, and the refining time is about 30-60min. Then reduce the power value to 200-600kw, reduce the temperature of molten steel to 1490-1520℃, and pay attention to the slag on the surface of molten steel; add Ti, Al, Nb and B elements for alloying smelting. Take samples for component analysis. When the alloy element content in the cup sample meets the requirements of the technical agreement, fill it with 20-25kPa Ar, where the amount of Ni-Mg alloy added to each ton of molten steel is 5-9kg. Smelt at a power of 400-1000kw for 5-10min to cast the electrode.
[0063] 2) 10 tons vacuum consumable remelting
[0064] The electrode surface is ground clean, and no stains, oxide scale, water stains, etc. are allowed. The electrode head shrinkage hole is facing upwards for smelting to obtain a consumable ingot. For the consumable crystallizer, the melting rate is set at 3.5~5.5Kg / min.
[0065] 3) Forging
[0066] The consumable ingot is heated and kept at 1130-1180℃ for more than 60h for homogenization and diffusion, and then peeled and finished. After that, the consumable ingot is heated to 1140-1160℃ and kept for 7-11h before forging. The consumable ingot is upset and drawn several times, upset to 1 / 2-2 / 3 of the original height of the consumable ingot, and the ingot diameter is about 650-750mm. The forging ratio is increased to break the internal structure of the ingot as much as possible; the temperature is gradually reduced and drawn, and the reheating temperature is gradually reduced from 1160℃ to 1100℃, and the holding time is ≥120min. The final forging is Large size bars, polished to The start forging temperature is ≥1050℃, and the stop forging temperature is ≥1000℃.
[0067] 4) Heat treatment
[0068] The forged large-size bars are heat treated according to the following process:
[0069] Solution treatment: in the range of 1060℃~1100℃, the sample is kept warm for 7~11h, and then air-cooled after being taken out of the furnace;
[0070] Aging treatment: 750-790℃, keep warm for 14-19h, air-cool out of the furnace; finally, large-size nickel-based high-temperature alloy bars that are difficult to deform are obtained.
[0071] The specific chemical compositions of the three furnaces of alloys produced according to the above-mentioned method for preparing the difficult-to-deform large-size nickel-based high-temperature alloy rod are shown in Table 2. Then, the three furnaces of alloys were sampled and subjected to high-temperature endurance performance tests at room temperature and at a temperature of 650°C and a pressure of 873MPa. The specific results are shown in Tables 3 and 4.
[0072] Table 2 Chemical composition of large-size nickel-based high-temperature alloy bars that are difficult to deform (wt%)
[0073]
[0074]
[0075] Table 3 Mechanical properties of alloys at room temperature
[0076] Serial number <![CDATA[σ b / MPa]]> <![CDATA[σ 0.2 / MPa]]> <![CDATA[δ5 / %]]> ψ / % Example 1 1580 1240 21.5 32 Example 2 1580 1230 21.5 31.5 Example 3 1500 1160 23.5 32.5 GH4169 1400 1240 13 22 GH738 1310 980 25 32
[0077] Table 4 High temperature endurance performance at 650℃ and 873Mpa
[0078]
[0079] As shown in Tables 3 and 4, the comprehensive performance of the large-size nickel-based high-temperature alloy rods that are difficult to deform prepared in the embodiment is better than that of GH4169 and GH738 alloys, and has excellent high-temperature mechanical properties above 650°C. It is expected to become an alternative high-temperature alloy material for turbine discs of the next generation of ship gas turbines, and also lay a solid foundation for the future application research of difficult-to-deform nickel-based high-temperature alloys in my country.
[0080] In summary, the large-size nickel-based high-temperature alloy rod difficult to deform and the preparation method thereof of the present invention, by optimizing the alloy composition, reduce the Co and Cr contents in the alloy on the basis of ensuring the high strength of the alloy, compositely add Al, Ti, and Nb elements, increase the volume fraction of the γ' phase and thermal stability, and increase the upper limit temperature of the alloy; the preparation method of the large-size nickel-based high-temperature alloy rod difficult to deform of the present invention adopts vacuum induction melting, vacuum arc furnace remelting, consumable ingot homogenization treatment, forging, and heat treatment preparation processes to obtain large-size nickel-based high-temperature alloy rods difficult to deform with high performance and good organizational stability, which can not only meet the use requirements of large-scale ship gas turbines for high-performance nickel-based high-temperature alloys, but also lay a solid foundation for the future application research of difficult-to-deform nickel-based high-temperature alloys in my country.
[0081] This embodiment. Those skilled in the art should recognize that the above embodiments are only used to illustrate the present invention, and are not intended to limit the present invention. As long as they are within the spirit of the present invention, any changes or modifications to the above embodiments will fall within the scope of the claims of the present invention.
Claims
1. A large-size nickel-based high-temperature alloy bar that is difficult to deform, characterized in that: The chemical composition by weight percentage is as follows: C: 0.020-0.080%, Cr: 13.0-15.0%, Co: 9.0-11.0%, Al: 2.0-3.0%, Ti: 2.0-3.0%, Nb: 2.0-3.0%, Mo: 4.5-5.5%, W: ≤0.20%, B: ≤0.010%, N≤0.010%, O≤0.0050%, Fe: 0.1-1.0%, the balance is nickel and unavoidable impurities, The hard-to-deform large-size nickel-based high-temperature alloy bar is prepared by the following preparation method, comprising the steps of: S1, smelting in a vacuum induction furnace, adding the main ingredients Ni, Cr, Co, Mo, and C at the same time, evacuating to below 2.7Pa, increasing the power to perform chemical reaction, refining after chemical reaction, adding alloying elements Ti, Al, Nb and B for alloying smelting, and then analyzing the composition of the molten steel. After reaching the target composition requirements, Ar is charged, Ni-Mg alloy is added, and steel is tapped and electrodes are cast after smelting; During the material processing, the power is 300-1000 kw; During the refining process, the refining temperature is 1480-1530°C and the refining time is 30-60 minutes; During the alloying smelting process, the power is 200-600kw and the temperature is 1490-1520°C; After the Ar is filled, the pressure is 20-25 KPa; the amount of the Ni-Mg alloy added to each ton of molten steel is 5-9 kg; after adding the Ni-Mg alloy, the smelting is continued for 5-10 minutes; S2, vacuum consumable smelting, cleaning the surface of the electrode and then performing vacuum consumable smelting to obtain a consumable ingot; During the vacuum consumable smelting process, the melting rate is 3.5-5.5 kg / min; S3, forging, homogenizing the consumable ingot, and then forging the consumable ingot by multiple upsetting and drawing processes to obtain a large-sized bar, and polishing the surface of the large-sized bar. The diameter of the large-sized bar obtained by forging is 425 mm; During the homogenization process, the consumable ingot is heated to 1130-1180° C. and kept warm for more than 60 hours; During the forging process, the homogenized consumable ingot is heated to 1140-1160°C, upset to 1 / 2-2 / 3 of the original height of the consumable ingot, and then stretched by step-by-step cooling. The reheating temperature is gradually reduced from 1160°C to 1100°C, and the holding time is ≥120min. During the forging process, the start forging temperature is ≥1050°C and the stop forging temperature is ≥1000°C; S4, heat treatment, subjecting the large-sized rod to solid solution treatment and aging heat treatment, and finally obtaining the difficult-to-deform large-sized nickel-based high-temperature alloy rod; During the solution treatment process, the large-sized bars after polishing are heated to 1060-1100°C, kept at this temperature for 7-11 hours, and then taken out of the furnace and air-cooled; During the aging treatment, the large-size bars after the solution treatment are heated to 750-790°C, kept at this temperature for 14-19 hours, and then taken out of the furnace and air-cooled. At room temperature, the tensile strength σ of the large-size nickel-based high-temperature alloy bar that is difficult to deform b ≥1500MPa, yield strengthσ 0.2 ≥1150 MPa, elongation δ5 ≥21.5%, section shrinkage ψ ≥31.5%; Under the conditions of a temperature of 650° C. and a pressure of 873 MPa, the elongation δ of the difficult-to-deform large-size nickel-based high-temperature alloy rod is 3.5-5.0%, and the cross-sectional shrinkage ψ is 8%.
2. A method for preparing a large-size nickel-based high-temperature alloy bar that is difficult to deform as claimed in claim 1, characterized in that: The following steps are involved: S1, smelting in a vacuum induction furnace, adding the main ingredients Ni, Cr, Co, Mo, and C at the same time, evacuating to below 2.7Pa, increasing the power to perform chemical reaction, refining after chemical reaction, adding alloying elements Ti, Al, Nb and B for alloying smelting, and then analyzing the composition of the molten steel. After reaching the target composition requirements, Ar is charged, Ni-Mg alloy is added, and steel is tapped and electrodes are cast after smelting; During the material processing, the power is 300-1000 kw; During the refining process, the refining temperature is 1480-1530°C and the refining time is 30-60 minutes; During the alloying smelting process, the power is 200-600kw and the temperature is 1490-1520°C; After the Ar is filled, the pressure is 20-25 KPa; the amount of the Ni-Mg alloy added to each ton of molten steel is 5-9 kg; after adding the Ni-Mg alloy, the smelting is continued for 5-10 minutes; S2, vacuum consumable smelting, cleaning the surface of the electrode and then performing vacuum consumable smelting to obtain a consumable ingot; During the vacuum consumable smelting process, the melting rate is 3.5-5.5 kg / min; S3, forging, homogenizing the consumable ingot, and then forging the consumable ingot by multiple upsetting and drawing processes to obtain a large-sized bar, and polishing the surface of the large-sized bar. The diameter of the large-sized bar obtained by forging is 425 mm; During the homogenization process, the consumable ingot is heated to 1130-1180° C. and kept warm for more than 60 hours; During the forging process, the homogenized consumable ingot is heated to 1140-1160°C, upset to 1 / 2-2 / 3 of the original height of the consumable ingot, and then stretched by step-by-step cooling. The reheating temperature is gradually reduced from 1160°C to 1100°C, and the holding time is ≥120min. During the forging process, the start forging temperature is ≥1050°C and the stop forging temperature is ≥1000°C; S4, heat treatment, subjecting the large-sized rod to solid solution treatment and aging heat treatment, and finally obtaining the difficult-to-deform large-sized nickel-based high-temperature alloy rod; During the solution treatment process, the large-sized bars after polishing are heated to 1060-1100°C, kept at this temperature for 7-11 hours, and then taken out of the furnace and air-cooled; During the aging treatment, the large-size bars after the solution treatment are heated to 750-790°C, kept at this temperature for 14-19 hours, and then taken out of the furnace and air-cooled. At room temperature, the tensile strength σ of the large-size nickel-based high-temperature alloy bar that is difficult to deform b ≥1500MPa, yield strengthσ 0.2 ≥1150 MPa, elongation δ5 ≥21.5%, section shrinkage ψ ≥31.5%; Under the conditions of a temperature of 650° C. and a pressure of 873 MPa, the elongation δ of the difficult-to-deform large-size nickel-based high-temperature alloy rod is 3.5-5.0%, and the cross-sectional shrinkage ψ is 8%.