Electrolytic capacitor and method for manufacturing the same
By using a double-layer solid electrolyte layer structure in an electrolytic capacitor, the self-doped conductive polymer is used to fill the gaps in the first layer, the problem of deterioration of conductivity of the electrolytic capacitor at high temperature is solved, and its heat resistance is significantly improved. stability.
Patent Information
- Application Number
- CN202310282970.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-01-17
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2040-01-17
AI Technical Summary
Existing electrolytic capacitors are prone to deterioration of conductive polymers in high temperature environments, resulting in the problems of rising equivalent series resistance and reducing electrostatic capacitance.
Using a bilayer solid electrolyte layer structure including a first conductive polymer and a self-doped second conductive polymer, the contact between air and oxygen is reduced by filling the gap of the first layer with the second conductive polymer. This improves heat resistance.
It effectively suppresses the rise of the equivalent series resistance and the decrease of the electrolytic capacitor, and improves the heat resistance of the electrolytic capacitor.
Smart Images

Figure CN116072432B_ABST
Abstract
Description
[0001] This application is a divisional application. The application number of the parent application is: 202080009867.7 (PCT / JP2020 / 001435), the application date is: 2020.1.17, the invention name is: Electrolytic capacitor and its manufacturing method Technical Field
[0002] The present invention relates to an electrolytic capacitor having a solid electrolyte layer and a method for manufacturing the same. Background Art
[0003] An electrolytic capacitor includes a capacitor element including a solid electrolyte layer, an electrode terminal electrically connected to the capacitor element, and an outer casing sealing the capacitor element. For example, the capacitor element includes an anode body, a dielectric layer formed on the anode body, and a solid electrolyte layer formed on the dielectric layer.
[0004] The solid electrolyte layer contains a conductive polymer. Patent Document 1 proposes a solid electrolytic capacitor comprising: a dielectric oxide film and a conductive polymer layer, wherein the dielectric oxide film is formed on the surface of an anode body having pores, and the conductive polymer layer is formed inside the pores and contains amines and a water-soluble self-doped conductive polymer having a sulfonic acid group.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application No. 2013-081099 Summary of the invention
[0008] In an electrolytic capacitor, the dielectric layer is usually formed in a manner that covers the surface of the porous portion formed on the anode body. The anode body is connected to the electrode terminal, and sometimes the outside air intrudes into the interior of the capacitor element through the porous portion of the anode body. If the oxygen in the intruding air contacts the solid electrolyte layer, the conductive polymer contained in the solid electrolyte layer deteriorates, and the ESR (equivalent series resistance) of the electrolytic capacitor increases, or the electrostatic capacitance decreases.
[0009] One aspect of the present invention relates to an electrolytic capacitor including an anode body, a dielectric layer formed on the anode body, and a solid electrolyte layer formed on the dielectric layer.
[0010] The solid electrolyte layer includes a first layer including a first conductive polymer and a second layer formed on the first layer and including a self-doping second conductive polymer.
[0011] Another aspect of the present invention relates to a method for manufacturing an electrolytic capacitor, comprising:
[0012] A step of preparing an anode body having a dielectric layer formed thereon; and
[0013] forming a solid electrolyte layer on the dielectric layer;
[0014] The above-mentioned step of forming a solid electrolyte layer includes:
[0015] a step of polymerizing a precursor of a first conductive polymer on the dielectric layer to form a first layer including the first conductive polymer; and
[0016] A step of forming a second layer including the second conductive polymer on the first layer by allowing a liquid composition including a self-doping type second conductive polymer to adhere to the first layer.
[0017] According to the present invention, even after exposure to high temperature, an increase in ESR of an electrolytic capacitor including a solid electrolyte layer can be suppressed, and a decrease in electrostatic capacitance can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a cross-sectional view schematically showing an electrolytic capacitor according to one embodiment of the present invention.
[0019] Figure 2 Yes Figure 1 A schematic cross-sectional view after enlarging region II. DETAILED DESCRIPTION
[0020] The electrolytic capacitor comprises an anode body, a dielectric layer formed on the anode body, and a solid electrolyte layer formed on the dielectric layer. For the anode body, in order to increase the surface area of the surface where the dielectric layer and the solid electrolyte layer are formed, a porous portion is usually provided on the surface layer. The porous portion contains a large number of voids. One end of the anode body is connected to the electrode terminal, and air penetrates into the capacitor element from the electrode terminal side through the voids in the porous portion, sometimes degrading the conductive polymer contained in the solid electrolyte layer. Such degradation of conductive polymers is particularly significant in high temperature environments.
[0021] According to an electrolytic capacitor of one aspect of the present invention, a solid electrolyte layer including a first layer and a second layer is formed, wherein the first layer includes a first conductive polymer, and the second layer is formed on the first layer and includes a second conductive polymer of a self-doping type. By using a conductive polymer of a self-doping type as the second conductive polymer, the second conductive polymer can be easily introduced into the first layer. This is because, compared with the case of a non-self-doping conductive polymer, the conductive polymer of the self-doping type is stably maintained in a state with a small particle size in a liquid composition. Even if there is a gap in the first layer, since the second conductive polymer is filled into the gap of the first layer, even if air invades the capacitor element, it is not easy to penetrate the solid electrolyte layer. Since the contact between the solid electrolyte layer and the oxygen contained in the air can be reduced, the degradation of the conductive polymer is suppressed. Thus, the heat resistance of the solid electrolyte layer is improved, and the heat resistance of the electrolytic capacitor is improved. Therefore, the rise of the ESR (equivalent series resistance) of the electrolytic capacitor after the heat resistance test can be suppressed. In addition, the reduction of the electrostatic capacitance of the electrolytic capacitor after the heat resistance test can also be suppressed.
[0022] It should be noted that the self-doping conductive polymer refers to a conductive polymer having an anionic group directly or indirectly bonded to the skeleton of the conductive polymer by a covalent bond. The anionic group possessed by the conductive polymer itself functions as a dopant of the conductive polymer, so it is called a self-doping type. The anionic group includes, for example, an acidic group (acid type) or its conjugated anionic group (salt type).
[0023] Hereinafter, the electrolytic capacitor and the method for manufacturing the same according to the above aspect of the present invention will be described in more detail with reference to the drawings as needed.
[0024] [Electrolytic capacitors]
[0025] (Anode)
[0026] The anode body may include a valve metal, an alloy including a valve metal, a compound including a valve metal, and the like. These materials may be used alone or in combination of two or more. As the valve metal, for example, aluminum, tantalum, niobium, and titanium are preferably used. The anode body usually has a porous portion on the surface layer. Such an anode body is obtained, for example, by roughening the surface of a substrate (a foil-shaped or plate-shaped substrate, etc.) including a valve metal by etching or the like. In addition, the anode body may also be a formed body of particles including a valve metal or a sintered body thereof. Since the sintered body has a porous structure, the entire anode body can become a porous portion.
[0027] (Dielectric layer)
[0028] The dielectric layer is formed by anodizing the valve action metal on the surface of the anode body by chemical conversion treatment or the like. The dielectric layer may be formed in a manner that covers at least a portion of the anode body. The dielectric layer is usually formed on the surface of the anode body. Since the dielectric layer is formed on the surface of the porous portion of the anode body, it is formed along the inner wall surface of the pores and depressions (pits) on the surface of the anode body.
[0029] The dielectric layer includes an oxide of a valve metal. For example, when tantalum is used as the valve metal, the dielectric layer includes Ta2O5, and when aluminum is used as the valve metal, the dielectric layer includes Al2O3. It should be noted that the dielectric layer is not limited to this, as long as it is a layer that functions as a dielectric.
[0030] (Solid electrolyte layer)
[0031] The solid electrolyte layer is formed in a manner covering the dielectric layer. The solid electrolyte layer does not need to cover the entire dielectric layer (the entire surface), as long as it is formed in a manner covering at least a portion of the dielectric layer. The solid electrolyte layer includes: a first layer including a first conductive polymer and a second layer formed on the first layer and including a self-doped second conductive polymer. In the case where there is an area on the dielectric layer where the first layer is not formed, the second layer can be formed on the dielectric layer in this area.
[0032] (First floor)
[0033] As the first conductive polymer, for example, a non-self-doping conductive polymer can be cited. When the first layer includes a non-self-doping conductive polymer, voids are easily generated in the first layer, but even in such a case, by forming a second layer of a self-doping second conductive polymer on the first layer, the second conductive polymer enters the first layer, thereby improving the heat resistance of the solid electrolyte layer.
[0034] Examples of non-self-doping conductive polymers include conductive polymers that do not have anionic groups (specifically, sulfonic acid groups, carboxyl groups, phosphoric acid groups, phosphonic acid groups, and salts thereof) directly or indirectly bonded to the conductive polymer skeleton via covalent bonds.
[0035] As a non-self-doping conductive polymer, polypyrrole, polythiophene, polyaniline, etc. are preferred. They can be used alone, or two or more kinds can be used in combination, or they can be copolymers of two or more monomers. It should be noted that in this specification, polypyrrole, polythiophene, polyaniline, etc. refer to polymers with polypyrrole, polythiophene, polyaniline, etc. as basic skeletons, respectively. Therefore, polypyrrole, polythiophene, polyaniline, etc. may also include respective derivatives (substituents further having substituents other than anionic groups, etc.). For example, polythiophene includes poly (3,4-ethylenedioxythiophene) (PEDOT), etc. Among them, polypyrroles (polypyrroles and their derivatives) sometimes produce gaps in the first layer. Even in the case of including such polypyrroles in the first layer, since a second layer including a second conductive polymer is formed on the first layer, the second conductive polymer can also enter the first layer, and the high heat resistance of the solid electrolyte layer can be ensured.
[0036] The weight average molecular weight of the first conductive polymer is not particularly limited, and is, for example, 1,000 or more and 1,000,000 or less.
[0037] In addition, in this specification, the weight average molecular weight is a weight average molecular weight based on polystyrene measured by gel permeation chromatography (GPC).
[0038] The first layer may contain a self-doping type second conductive polymer. The second conductive polymer may be contained in the first layer when the first layer is formed, or may be contained in the first layer by allowing the second conductive polymer to enter the first layer when the second layer is formed. Examples of the self-doping conductive polymer include the conductive polymers described below.
[0039] The first layer may be a single layer or may be composed of multiple layers. When the first layer is composed of multiple layers, the first conductive polymer contained in each layer may be the same or different.
[0040] The first layer may further contain a dopant. As the dopant, for example, anions and / or polyanions may be used.
[0041] Examples of anions include sulfate ions, nitrate ions, phosphate ions, borate ions, and organic sulfonate ions, without particular limitation. Examples of dopants that generate sulfonate ions include p-toluenesulfonic acid and / or naphthalenesulfonic acid. Anions may be included in the first layer in the form of salts.
[0042] Examples of the polyanion include polyvinyl sulfonic acid, polystyrene sulfonic acid, polyallyl sulfonic acid, polyacrylic acid sulfonic acid and / or polymethacrylic acid sulfonic acid, etc., without particular limitation. The polyanion may be contained in the first layer in the form of a salt. In the first layer, the anion and / or the polyanion may form a conductive polymer composite together with the first conductive polymer.
[0043] As described above, the dielectric layer is formed along the inner wall surfaces of the holes and pits of the porous portion of the anode body, so the first layer formed on the dielectric layer is also formed in the porous portion of the anode body. The distribution state of the first layer in the porous portion is not particularly limited, and the first layer can be formed on the entire porous portion, and the distribution state of the first layer on the surface and inside of the porous portion can also be different. For example, the amount of the first layer inside the porous portion can be less than that near the surface of the porous portion. In addition, the second layer can also be formed on the first layer formed in the porous portion. The second layer can also be formed (or exist) in the gaps in the porous portion. In such a case, air is not easy to pass through the porous portion, so the effect of suppressing the degradation of the solid electrolyte layer is improved, and the increase in ESR can be further suppressed. In addition, the effect of suppressing the reduction of electrostatic capacitance can be further improved.
[0044] The first layer can be formed, for example, by chemically polymerizing and / or electrolytically polymerizing the precursor of the first conductive polymer (raw material monomer, etc.). Alternatively, it can be formed by contacting a liquid composition (first liquid composition) containing at least the first conductive polymer with the dielectric layer. In particular, electrolytic polymerization is easy to proceed on the surface side of the first layer (the surface side of the porous portion), so the first layer is easy to form densely, but it is difficult to proceed inside, so it is easy to produce voids. Air easily intrudes into the capacitor element through the voids, which easily leads to the degradation of the solid electrolyte layer. However, even in the case where the first layer is such an electrolytic polymerization film that is easy to produce voids, by forming the second layer, the permeation of air can be reduced, and the degradation of the solid electrolyte layer can be suppressed. Therefore, in particular, in the case where the first layer is formed by electrolytic polymerization, the effect brought about by forming the second layer (more specifically, allowing the second conductive polymer to enter the first layer) is significantly exerted. It should be noted that if the second layer is formed on the electrolytic polymerization film as the first layer, as described above, the amount of the first layer inside the porous portion becomes less than that near the surface of the porous portion. In addition, the second layer is also formed on the first layer formed in the porous portion, and is formed in a state where the second layer intrudes or fills the voids in the porous portion (or the first layer).
[0045] (Second floor)
[0046] As the anionic group possessed by the second conductive polymer, there can be mentioned a sulfonic acid group, a carboxyl group, a phosphoric acid group, a phosphonic acid group, or their salts (salts with inorganic bases, salts with organic bases, etc.). The second conductive polymer may have one anionic group, or may have two or more anionic groups. As the anionic group, a sulfonic acid group or its salt is preferred, or it may be a combination of a sulfonic acid group or its salt and an anionic group other than a sulfonic acid group or its salt. The amount of anionic groups contained in the second conductive polymer is preferably 1 to 3 per molecule corresponding to the main skeleton of the second conductive polymer, and more preferably 1 or 2 (especially 1).
[0047] As the second conductive polymer, preferably polypyrrole with anionic groups, polythiophene with anionic groups, polyaniline with anionic groups, etc. They can be used alone or in combination of two or more, and the second conductive polymer can be a copolymer of two or more monomers. It should be noted that polypyrrole, polythiophene, polyaniline, etc. may also include respective derivatives (in addition to anionic groups, substituents of substituents other than anionic groups, etc.). From the viewpoint of further improving the effect of suppressing the rise of ESR and the reduction of electrostatic capacitance even after exposure to a high temperature environment, among them, for example, self-doped PEDOT (PEDOT and its derivatives, etc.) is preferred.
[0048] From the viewpoint of easily penetrating into the first layer, the weight average molecular weight of the second conductive polymer is preferably 100000 or less, and more preferably 30000 or less. The weight average molecular weight of the second conductive polymer is, for example, 1000 or more.
[0049] The viscosity of the second liquid composition containing the second conductive polymer is not particularly limited as long as it is 500 mPa·s or less at 25° C. and 60 rpm, but is preferably 300 mPa·s or less, and more preferably 100 mPa·s or less, when evaluated using a B-type viscometer.
[0050] The second layer may contain a conductive polymer other than the second conductive polymer (e.g., a non-self-doped conductive polymer, etc.), and preferably the second conductive polymer content is high. The ratio of the second conductive polymer to the entire conductive polymer contained in the second layer is, for example, 90% by mass or more, or 100% by mass.
[0051] The second conductive polymer has an anionic group, and the second layer may contain a dopant as needed. As the dopant, for example, anions and / or polyanions are used. In the second layer, the anions and / or polyanions can form a conductive polymer composite together with the conductive polymer. As the anions and polyanions, they can be selected from the anions and polyanions described for the first layer, respectively.
[0052] The content of the dopant in the second layer is, for example, 0 to 50 parts by mass, or preferably 0 to 10 parts by mass or 0.1 to 10 parts by mass, relative to 100 parts by mass of the second conductive polymer.
[0053] The second layer may be a single layer or may be composed of multiple layers. When the second layer is composed of multiple layers, the second conductive polymer contained in each layer may be the same or different.
[0054] The second layer may further contain a base as necessary. The base may be selected from the bases exemplified for the first layer.
[0055] The solid electrolyte layer may further contain other components within a range not impairing the effects of the present invention.
[0056] Figure 1 It is a cross-sectional view schematically showing the structure of an electrolytic capacitor according to one embodiment of the present invention. Figure 2 It indicates schematically Figure 1 The electrolytic capacitor 1 includes a capacitor element 2, a resin sealing material (external body) 3 that seals the capacitor element 2, and an anode terminal 4 and a cathode terminal 5, each of which is exposed at least in part outside the resin sealing material 3. The anode terminal 4 and the cathode terminal 5 can be made of metal (copper or copper alloy, etc.), for example. The resin sealing material 3 has a roughly rectangular parallelepiped shape, and the electrolytic capacitor 1 also has a roughly rectangular parallelepiped shape. As a raw material for the resin sealing material 3, for example, epoxy resin can be used.
[0057] Capacitor element 2 includes an anode body 6, a dielectric layer 7 covering the anode body 6, and a cathode portion 8 covering the dielectric layer 7. Cathode portion 8 includes a solid electrolyte layer 9 covering the dielectric layer 7 and a cathode lead layer 10 covering the solid electrolyte layer 9. Cathode lead layer 10 includes, for example, a carbon layer 11 and a silver paste layer 12.
[0058] The anode body 6 has a porous portion 6a and includes a region facing the cathode portion 8 and a region not facing the cathode portion 8. In the region of the anode body 6 not facing the cathode portion 8, an insulating separation layer 13 is formed in a portion adjacent to the cathode portion 8 in a band-like manner to cover the surface of the anode body 6, thereby limiting the contact between the cathode portion 8 and the anode body 6. In the region of the anode body 6 not facing the cathode portion 8, another portion is electrically connected to the anode terminal 4 by welding. The cathode terminal 5 is electrically connected to the cathode portion 8 via an adhesive layer 14 formed of a conductive adhesive.
[0059] The main surfaces 4S and 5S of the anode terminal 4 and the cathode terminal 5 are exposed from the same surface of the resin sealing material 3. The exposed surfaces are used for solder connection with a substrate (not shown) on which the electrolytic capacitor 1 is to be mounted.
[0060] The carbon layer 11 only needs to be conductive, and can be made of, for example, a conductive carbon material (graphite, etc.). The silver paste layer 12 can be made of, for example, a composition containing silver powder and a binder resin (epoxy resin, etc.). It should be noted that the composition of the cathode lead layer 10 is not limited to this, and any composition having a current collection function can be used.
[0061] The solid electrolyte layer 9 is formed so as to cover the dielectric layer 7. The dielectric layer 7 is formed along the surface of the anode body 6 (including the surface of the inner wall surface of the hole). The surface of the dielectric layer 7 is formed with a concavo-convex shape corresponding to the shape of the surface of the anode body 6. The solid electrolyte layer 9 is preferably formed so as to fill the concavo-convex of the dielectric layer 7.
[0062] The solid electrolyte layer 9 includes a first layer 9a formed on the dielectric layer 7 and a second layer 9b formed on the first layer. The first layer 9a includes a first conductive polymer, and the second layer 9b includes a self-doped second conductive polymer. The first layer 9a is formed in the porous portion 6a of the anode body 6 (or is in a filled state), and has voids P in the layer. When the second layer 9b is formed, the second conductive polymer enters the first layer 9a. Therefore, the second conductive polymer enters the voids P in the first layer 9a, and the second layer 9b is formed in the voids P. It should be noted that the voids P are schematically shown in the figure, but in the porous portion (or the first layer 9a), at least a portion of the voids P is continuous.
[0063] The electrolytic capacitor of the above aspect is not limited to the electrolytic capacitor of the above structure, and can be applied to electrolytic capacitors of various structures. Specifically, the present invention can also be applied to a wound electrolytic capacitor, an electrolytic capacitor using a sintered body of metal powder as an anode body, and the like.
[0064] [Method for manufacturing electrolytic capacitor]
[0065] The manufacturing method of the electrolytic capacitor of the above aspect includes: a step of preparing an anode body having a dielectric layer formed thereon (first step), and a step of forming a solid electrolyte layer on the dielectric layer (second step). In addition, the manufacturing method of the electrolytic capacitor may include a step of preparing an anode body before the first step. The manufacturing method may further include a step of forming a cathode lead layer and / or a step of sealing the capacitor element.
[0066] Hereinafter, each step will be described in more detail.
[0067] (Step of Preparing Anode Body)
[0068] In this step, the anode body is formed by a known method depending on the type of the anode body.
[0069] The anode body can be prepared, for example, by roughening the surface of a foil-shaped or plate-shaped substrate containing a valve metal. By roughening, a porous portion is formed on the surface layer of the anode body. Roughening can be performed as long as it can form unevenness on the surface of the substrate, for example, by etching the surface of the substrate (for example, electrolytic etching).
[0070] In addition, a valve-acting metal powder is prepared, and a molded body is formed into a desired shape (e.g., a block) while one end of a rod-shaped anode terminal in the longitudinal direction is embedded in the powder. The molded body is sintered to form an anode body with a porous structure in which one end of the anode terminal is embedded.
[0071] (First process)
[0072] In the first step, a dielectric layer is formed on the anode body. The dielectric layer is formed by anodizing the anode body. Anodization can be performed by a known method, such as chemical conversion treatment. The chemical conversion treatment can be performed, for example, as follows: the anode body is immersed in a chemical conversion solution, the chemical conversion solution is infiltrated into the surface of the anode body, and a voltage is applied between the anode body and a cathode immersed in the chemical conversion solution, using the anode body as an anode. As the chemical conversion solution, for example, a phosphoric acid aqueous solution is preferably used.
[0073] (Second process)
[0074] In the second step, the solid electrolyte layer is formed so as to cover at least a portion of the dielectric layer. The second step includes, for example, a step of forming the first layer on the dielectric layer and a step of forming the second layer on the first layer.
[0075] (Step of forming the first layer)
[0076] The first layer can be formed by contacting the first liquid composition containing the first conductive polymer with the dielectric layer, but is preferably formed by chemically polymerizing and / or electrolytically polymerizing the precursor of the first conductive polymer. In particular, when the precursor is polymerized by electrolytic polymerization to form the first layer containing the first conductive polymer, sometimes gaps are formed in the first layer, so it is easy to obtain a significant effect brought about by the second conductive polymer entering the first layer. In the case of electrolytic polymerization, a conductive pre-coating layer can be formed before electrolytic polymerization. The first layer can be formed directly on the dielectric layer or through the pre-coating layer.
[0077] As the first liquid composition containing the first conductive polymer, for example, a dispersion liquid (or solution) of the first conductive polymer or a dispersion liquid (or solution) of a conductive polymer complex of the first conductive polymer and a dopant can be used.
[0078] In the case of chemical polymerization, for example, the first layer is formed using a first liquid composition containing a precursor of a first conductive polymer, a dispersion medium (or solvent), an oxidant, and, if necessary, a dopant. The first liquid composition may be attached to the dielectric layer and then heated.
[0079] In the case of electrolytic polymerization, for example, a first layer is formed using a first liquid composition comprising a precursor of a first conductive polymer, a dispersion medium (or solvent) and a dopant as required. The first layer is formed, for example, by immersing an anode body having a dielectric layer and a pre-coat layer in the first liquid composition, using the pre-coat layer as an electrode, and supplying electricity from the supply electrode. The pre-coat layer is formed, for example, of a conductive material (conductive polymer, inorganic conductive material, etc.). There is no particular limitation on the conductive material constituting the pre-coat layer, and for example, a known conductive material can be used.
[0080] As the first conductive polymer and the dopant, the substances exemplified above can be used respectively. As the precursor of the first conductive polymer, the monomer constituting the first conductive polymer and / or an oligomer formed by connecting several monomers can be exemplified. As the dispersion medium (or solvent), for example, water, an organic solvent, or a mixture thereof can be cited. As the organic solvent, for example, a monohydric alcohol (methanol, ethanol, propanol, etc.), a polyhydric alcohol (ethylene glycol, glycerol, etc.) or an aprotic polar solvent (N, N-dimethylformamide, dimethyl sulfoxide, acetonitrile, acetone, benzonitrile, etc.) can be cited. The first liquid composition can also contain a base and / or other components.
[0081] (Step of forming the second layer)
[0082] The second layer is formed on the first layer, for example, by attaching a second liquid composition containing a self-doping type second conductive polymer to the first layer. The second layer can be formed, for example, by immersing an anode body having the first layer formed on a dielectric layer in the second liquid composition, or by coating or dropping the second liquid composition on an anode body having the first layer formed on a dielectric layer and then drying it.
[0083] The second liquid composition comprises a second conductive polymer, a dispersion medium (or solvent) and a dopant as required. As the second conductive polymer and the dopant, the substances exemplified above can be used. As the dispersion medium (or solvent), the substances exemplified with respect to the first liquid composition can be used. The second liquid composition may further comprise an alkali and / or other components.
[0084] As the second liquid composition, for example, a dispersion (or solution) of a second conductive polymer, a dispersion (or solution) of a conductive polymer complex of a second conductive polymer and a dopant can be used. The second liquid composition can be obtained, for example, by oxidative polymerization of a precursor of the second conductive polymer in a dispersion medium (or solvent). As the precursor, examples include monomers constituting the second conductive polymer, and / or oligomers formed by connecting several monomers. The second liquid composition containing the conductive polymer complex can be obtained by oxidative polymerization of a precursor of the second conductive polymer in a dispersion medium (or solvent) in the presence of a dopant.
[0085] The average particle size of the particles of the second conductive polymer (or conductive polymer complex) dispersed in the second liquid composition is, for example, 800 nm or less. From the viewpoint of making it easy for the second conductive polymer to enter the first layer, the average particle size is preferably 300 nm or less, more preferably 100 nm or less. The lower limit of the average particle size is not particularly limited, for example, 5 nm or more.
[0086] In the present specification, the average particle size of the conductive polymer (or conductive polymer composite) can be determined from, for example, a particle size distribution by a dynamic light scattering method.
[0087] (Step of forming cathode lead layer)
[0088] In this step, a cathode lead layer is formed by sequentially stacking a carbon layer and a silver paste layer on the solid electrolyte layer formed in the second step. By forming the cathode lead layer, a capacitor element can be obtained.
[0089] It should be noted that a conductive adhesive layer is disposed on the surface of the cathode lead layer, and one end of the cathode terminal is electrically connected to the capacitor element via the adhesive layer. As the cathode terminal, an electrode terminal used in an electrolytic capacitor can be used without particular limitation, for example, a terminal called a lead frame can be used.
[0090] (Process of sealing capacitor element with resin sealing material)
[0091] The formed capacitor element is sealed by a resin material together with a part of each of the anode terminal 4 and the cathode terminal 5, for example. By this sealing, a resin sealing material 3 is formed. As the resin material, a thermosetting resin (epoxy resin, etc.) or a resin composition is preferred. It should be noted that the resin sealing material 3 contains a cured product of a thermosetting resin or a resin composition.
[0092] [Example]
[0093] Hereinafter, the present invention will be specifically described based on Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0094] 《Example 1》
[0095] Follow the instructions below to make Figure 1 The electrolytic capacitor 1 shown was used to evaluate its characteristics.
[0096] (1) Step of preparing anode body
[0097] An aluminum foil (thickness: 100 μm) was prepared as a substrate, and the surface of the aluminum foil was subjected to etching treatment to obtain an anode body 6 .
[0098] (2) Step of forming dielectric layer 7
[0099] Anode body 6 was immersed in a 0.3 mass % phosphoric acid solution (liquid temperature 70° C.) and a DC voltage of 70 V was applied for 20 minutes to form dielectric layer 7 containing aluminum oxide (Al2O3) on the surface of anode body 6. Then, an insulating anti-corrosion tape (separation layer 13) was attached to a predetermined portion of anode body 6.
[0100] (3) Step of forming the first layer
[0101] An aqueous dispersion (first liquid composition) containing pyrrole and a dopant (naphthalenesulfonic acid) was prepared. The concentration of pyrrole in the first liquid composition was 2% by mass, and the concentration of the dopant was 10% by mass.
[0102] The anode body 6 having the dielectric layer 7 formed thereon is immersed in a liquid composition containing a conductive material to form a pre-coat layer. The anode body 6 having the dielectric layer 7 and the pre-coat layer formed thereon is immersed in a first liquid composition, and the pre-coat layer is used as an electrode to electrolytically polymerize pyrrole, thereby forming a first layer containing polypyrrole as a first conductive polymer.
[0103] (4) Step of forming the second layer
[0104] An aqueous dispersion (second liquid composition) containing a second conductive polymer was prepared. The concentration of the second conductive polymer in the second liquid composition was 4% by mass, and the average particle size of the second conductive polymer was 100 nm. As the second conductive polymer, PEDOT having a sulfonic acid group directly bonded to the PEDOT skeleton was used.
[0105] After the anode body 6 formed with the first layer 9a is immersed in the second liquid composition, a drying process is performed at 120°C for 10 to 30 minutes to form the second layer 9b. At this time, the second liquid composition penetrates into the first layer 9a, so that the second conductive polymer is also filled in the gaps P formed in the first layer 9a, so that the second layer containing the second conductive polymer is formed in the gaps P of the first layer.
[0106] In this way, solid electrolyte layer 9 composed of first layer 9a and second layer 9b is formed.
[0107] (5) Step of forming cathode lead layer
[0108] The carbon layer 11 is formed by applying a dispersion in which graphite particles are dispersed in water onto the surface of the solid electrolyte layer 9 and then drying the dispersion.
[0109] Next, a silver paste containing silver particles and a binder resin (epoxy resin) is applied to the surface of the carbon layer 11, and then the binder resin is cured by heating to form the silver paste layer 12. In this way, the cathode extraction layer 10 composed of the carbon layer 11 and the silver paste layer 12 is formed. Thus, the capacitor element 2 is obtained.
[0110] (6) Assembly of electrolytic capacitors
[0111] Anode terminal 4 , cathode terminal 5 , and adhesive layer 14 are further arranged on capacitor element 2 , and sealed with resin sealing material 3 , thereby producing an electrolytic capacitor.
[0112] Comparative Example 1
[0113] An electrolytic capacitor was produced in the same manner as in Example 1 except that the second layer was not formed.
[0114] Comparative Example 2
[0115] As the second liquid composition for forming the second layer, an aqueous dispersion of PEDOT doped with polystyrene sulfonic acid (PSS) as a non-self-doping conductive polymer was used. The concentration of the conductive polymer in the second liquid composition was 4% by mass, and the average particle size of the conductive polymer was 400 nm. Otherwise, the same operation as in Example 1 was performed to prepare an electrolytic capacitor.
[0116] [evaluate]
[0117] The electrolytic capacitors of the examples and comparative examples produced above were evaluated for capacitance and ESR in accordance with the following procedures.
[0118] In an environment of 20°C, a 4-terminal LCR meter is used to measure the initial electrostatic capacitance value C0 (μF) of the electrolytic capacitor and the initial ESR value X0 (mΩ) at a frequency of 100kHz. Next, the rated voltage is applied to the electrolytic capacitor for 125 hours at a temperature of 145°C (heat resistance test). Then, the electrostatic capacitance value C1 (μF) and the ESR value (X1) (mΩ) are measured respectively using the same method as above. Then, the value obtained by subtracting the initial electrostatic capacitance value C0 from the electrostatic capacitance value C1 is divided by the initial electrostatic capacitance value C0 and multiplied by 100 to calculate the rate of change of the electrostatic capacitance. In addition, the value obtained by subtracting the initial ESR value X0 from the ESR value X1 is divided by the initial ESR value X0 and multiplied by 100 to calculate the rate of change of the ESR. The ratio (relative value) of the rate of change in Example 1 and Comparative Example 2 when the rate of change in Comparative Example 1 is set to 100 is calculated as an indicator for evaluating the electrostatic capacitance and ESR.
[0119] The results are shown in Table 1. Example 1 is A1, and Comparative Examples 1 and 2 are R1 and R2.
[0120] [Table 1]
[0121] ESR change rate Capacitance change rate A1 76.2 92.3 R1 100 100 R2 114.2 107.5
[0122] In Example 1, the change rates of electrostatic capacitance and ESR are smaller than those of Comparative Examples 1 and 2. It is believed that this is because, in Example 1, by filling the gaps in the first layer with a self-doped second conductive polymer, the contact between air and the solid electrolyte layer is suppressed, and the degradation of the conductive polymer is suppressed, thereby improving the heat resistance of the electrolytic capacitor. In particular, in Comparative Example 2 using a non-self-doped conductive polymer, the change rates of ESR and electrostatic capacitance are increased. It is believed that this is because, in the liquid composition of Comparative Example 2, the particle size of the conductive polymer is large and the permeability into the first layer is low.
[0123] Industrial Applicability
[0124] The electrolytic capacitor of one aspect of the present invention can suppress the degradation of the conductive polymer contained in the solid electrolyte layer even when exposed to a high temperature atmosphere, and can suppress the increase of ESR. In addition, it is also possible to suppress the reduction of electrostatic capacitance. Therefore, it can be used for various applications requiring high heat resistance of the electrolytic capacitor.
[0125] Description of Reference Numerals
[0126] 1: Electrolytic capacitor, 2: Capacitor element, 3: Resin sealing material, 4: Anode terminal, 4S: Main surface of anode terminal, 5: Cathode terminal, 5S: Main surface of cathode terminal, 6: Anode body, 7: Dielectric layer, 8: Cathode part, 9: Solid electrolyte layer, 9a: First layer, 9b: Second layer, 10: Cathode lead layer, 11: Carbon layer, 12: Silver paste layer, 13: Separation layer, 14: Adhesive layer
Claims
1. An electrolytic capacitor comprising an anode body, a dielectric layer formed on the anode body, and a solid electrolyte layer formed on the dielectric layer, The solid electrolyte layer includes a first layer and a second layer, the first layer includes a non-self-doping first conductive polymer, and the second layer is formed on the first layer and includes a self-doping second conductive polymer. The first layer has a void in which the first conductive polymer does not exist, and the second conductive polymer exists in the void.
2. The electrolytic capacitor according to claim 1, wherein: The second layer does not include the first conductive polymer.
3. The electrolytic capacitor according to claim 1, wherein: The second layer includes the first conductive polymer, An amount of the second conductive polymer contained in a unit volume of the second layer is greater than an amount of the first conductive polymer contained in a unit volume of the second layer.
4. The electrolytic capacitor according to any one of claims 1 to 3, wherein The weight average molecular weight of the second conductive polymer is 30,000 or less.
5. The electrolytic capacitor according to any one of claims 1 to 3, wherein The second conductive polymer is a self-doping type poly (3, 4-ethylenedioxythiophene) type.
6. The electrolytic capacitor according to claim 5, wherein: The first conductive polymer is polypyrrole.
7. A method for manufacturing an electrolytic capacitor, comprising: A step of preparing an anode body having a dielectric layer formed thereon; as well as forming a solid electrolyte layer on the dielectric layer, The step of forming a solid electrolyte layer comprises: In a first step, a precursor of a non-self-doping first conductive polymer is polymerized to form a first layer including the first conductive polymer; as well as In the second step, a liquid composition containing a self-doping type second conductive polymer is attached to the first layer, thereby forming a second layer containing the second conductive polymer on the first layer. In the first step, voids in which the first conductive polymer does not exist are generated in the first layer. In the second step, the second conductive polymer is allowed to infiltrate the gap.
8. The method for manufacturing an electrolytic capacitor according to claim 7, wherein: The second conductive polymer particles are dispersed in the liquid composition. The average particle size of the particles is 100 nm or less.
9. The method for manufacturing an electrolytic capacitor according to claim 7 or 8, wherein: The second conductive polymer is a self-doping poly (3, 4-ethylenedioxythiophene) type.
10. The method for manufacturing an electrolytic capacitor according to claim 9, wherein: The first conductive polymer is polypyrrole.
Citation Information
Patent Citations
Elastic surface wave device
JP2013081099A
Method of manufacturing solid electrolytic capacitor and solid electrolytic capacitor
CN102169758A
Solid electrolytic capacitor
JP2008053512A