A sandwich structure composite material and preparation method thereof
By adopting sandwich structural composite materials, including polyester filaments, staple fiber fabrics and neoprene adhesive layers, through the refining, refining and sulfur drumming processes, the poor resilience and odor problems of existing ceiling materials have been solved, achieving high The ceiling materials with performance, environmental protection and plasticity meet the diverse needs of automotive ceilings.
Patent Information
- Application Number
- CN202211282039.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-19
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-10-19
AI Technical Summary
The existing automotive ceiling materials have poor resilience and insufficient weather resistance, complex production process and odor problems, and a single shape and poor plasticity, making it difficult to meet high performance and environmental protection requirements.
Sandwich structural composite materials, including polyester filament woven fabric, staple fiber woven fabric and neoprene adhesive layer, are prepared through intensive refining, sulphur drumming processes to form high resilience, folding and environmentally friendly Ceiling material.
It achieves high resilience, weather resistance, plasticity and environmental protection of the ceiling, eliminates odor problems, provides customized design and diverse shapes, and has sound insulation, heat insulation, waterproof and anti-aging properties.
Smart Images

Figure BDA0003898576750000011 
Figure BDA0003898576750000021 
Figure BDA0003898576750000041
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of automobile roof materials, and particularly relates to a sandwich structure composite material and a preparation method thereof. Background Art
[0002] With the continuous improvement of the quality of life, the function of the car is not only a means of transportation, but consumers gradually regard the car as a safe, trendy and fully functional "second home". As a home, the car is required to be safe, beautiful, comfortable, and have certain functions and environmental protection performance. The car roof occupies a large area in the car, and it should meet the requirements of high performance and green environmental protection. The ceiling on the market today is a fabric + sponge pressed on the main material of the top of the car through a hot pressing process. This material is usually a composite material. The ceiling fabric of this material has poor resilience and is not weather-resistant. In addition, during production and processing, glue is used during hot pressing, which produces odor. Such a ceiling composite has complex process, expensive materials, single shape, and poor plasticity.
[0003] Therefore, it is necessary to develop a new type of sandwich structure composite material. Summary of the invention
[0004] The purpose of the present invention is to provide a sandwich structure composite material and a preparation method thereof to solve the above problems.
[0005] A technical solution of the present invention is:
[0006] A sandwich structure composite material comprises: a first fabric layer, a chloroprene rubber adhesive layer and a second fabric layer, wherein the first fabric layer is made of polyester filament woven fabric, the second fabric layer is made of short fiber woven fabric, and the material formula of the chloroprene rubber adhesive layer is:
[0007]
[0008]
[0009] Another technical solution of the present invention is:
[0010] A method for preparing a sandwich structure composite material, the method comprising the following steps:
[0011] (1) cleaning the internal mixer, setting the temperature and speed of the internal mixer, opening the top plug of the internal mixer, adding raw rubber for primary internal mixing, then adding filler, closing the top plug for secondary internal mixing, and draining the rubber to obtain a mixed rubber;
[0012] (2) cleaning the open mill, setting the roller temperature and roller speed of the two rollers of the open mill, adjusting the roller distance of the two rollers for the first time, starting the open mill, placing the rubber mix between the two rollers, so that the rubber mix is rolled on the open mill and a rubber accumulation is generated between the two rollers, adding small materials evenly in an "S" shape, tapping the rubber mix with a rubber tapping knife to pre-disperse the small materials evenly, removing the rubber mix, pausing the open mill, adjusting the roller distance of the two rollers of the open mill for the second time, placing the rubber mix, starting the open mill, thinning, and obtaining a secondary rubber mix;
[0013] (3) adjusting the roller distance between the two rollers of the open mill for the third time, setting the initial temperature, starting the open mill, re-heating the secondary rubber mix, placing the secondary rubber mix on the open mill for calendering so that the secondary rubber mix can be completely wrapped on one side of the roller, taking a piece of the calendered secondary rubber mix from the roller as a rubber compound, measuring the thickness of the rubber compound with a vernier caliper, and obtaining a chloroprene rubber adhesive;
[0014] (4) stretching and straightening the first fabric and the second fabric respectively, and bonding the first fabric, the second fabric and the chloroprene rubber adhesive together by a calendering roller to obtain a semi-finished product;
[0015] (5) vulcanizing the semi-finished product through a sulphur drum process to obtain a finished product.
[0016] Furthermore, in step (1), the temperature of the internal mixer is 60° C. and the rotation speed is 60 rpm / min.
[0017] Furthermore, in step (1), the raw rubber is LANXESS B210, the filler is protective wax Antilux111, magnesium oxide, stearic acid, antioxidant OCTAM, phenol-formaldehyde resin MK95, white carbon black, carbon black N774, aromatic oil and DOS, and the filling ratio of the mixed rubber in the internal mixer is 0.69.
[0018] Furthermore, in step (1), the time of the first mixing is 3 minutes, the total time of the two mixings is 8 minutes and 30 seconds, and the temperature of the debinding is greater than 90°C and less than 110°C.
[0019] Furthermore, in step (2), the small materials are ETU-80, TMTD-80, zinc oxide and RA-65.
[0020] Furthermore, in step (2), the roller temperature of the two rollers of the mixing mill is 30°C, the roller speed is 17 rpm / min, the first adjustment of the roller spacing of the two rollers is 1 mm; the second adjustment of the roller spacing of the two rollers of the mixing mill is 0.5 mm; the rubber tapping is specifically: tapping the rubber at 3 / 4 of the left and right sides of the mixed rubber 3 times each; the thinning is specifically: thinning 5 times in the form of rolling and triangle packing.
[0021] Furthermore, in step (3), the roller distance between the two rollers of the mixing mill is adjusted for the third time to 3 mm, and the initial temperature is 60°C.
[0022] Furthermore, in step (3), the specific process parameters of the calendering are: using a 4-roll calender, a low roller speed of 5-10 m / min, a calendering temperature less than 60° C., and the thickness of the rubber material is 0.9 mm-1 mm.
[0023] Furthermore, in step (5), the specific parameters of the sulfur blowing process are: temperature 110° C., pressure 0.2 MPa, and speed 10 m / min.
[0024] The advantages of the present invention are:
[0025] 1. The ceiling made of the sandwich structure composite material of the present invention has good resilience, weather resistance and folding resistance;
[0026] 2. The ceiling made of the sandwich structure composite material of the present invention has no odor and meets environmental protection requirements;
[0027] 3. The chloroprene rubber adhesive of the present invention will not damage the fabric during bonding; and can provide the ceiling with a customizable design;
[0028] 4. The sandwich structure composite material of the present invention has good plasticity, is suitable for various shapes, has texture, has hardness, can be soundproof, heat-insulating, waterproof, and aging-resistant. DETAILED DESCRIPTION
[0029] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the technical solutions of the present invention are further described below in conjunction with embodiments. However, the present invention is not limited to the embodiments listed, and should also include any other known changes within the scope of the rights claimed by the present invention.
[0030] First, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0031] Embodiment 1
[0032] This embodiment forms a sandwich structure composite material according to the following structure:
[0033] The present invention is a sandwich structure using fabric-composite material-fabric, which can replace the roof composite of the car. The middle layer is a chloroprene rubber adhesive layer, and the upper and lower layers are fabrics. One layer of fabric is exposed to the outside. This layer of fabric is a polyester filament woven fabric, which has the characteristics of sun resistance, heat resistance, and cut resistance. It adopts the original liquid coloring technology and has strong color fastness. The other layer of fabric is inside the car, and it is a short-fiber woven fabric, which has the characteristics of softness and good hand feel. Please refer to Table 1, which is a formula table (weight parts) of the chloroprene rubber adhesive layer:
[0034]
[0035]
[0036] Table 1
[0037] The chloroprene rubber adhesive layer adopts the raw material formula in Table 1 to make the ceiling plastic, textured, hard, soundproof, heat-insulating, waterproof, aging-resistant, and most importantly, resilient and fold-resistant. In addition, the rubber adhesive layer using this formula has extremely low odor and is environmentally friendly. Compared with the existing ceiling composite, the cost advantage is obvious.
[0038] Embodiment 2
[0039] This embodiment prepares the sandwich structure composite material according to the following steps:
[0040] a. First clean the internal mixer with car wash gel, then wipe the entire internal mixer room with a paper towel dipped in alcohol;
[0041] b. Then set the mixer temperature to 60°C and the speed to 60rpm / min;
[0042] c. Open the top plug and add raw rubber (LANXESS B210). After 3 minutes of mixing, add the prepared fillers (protective wax Antilux111, magnesium oxide, stearic acid, antioxidant OCTAM, phenol-formaldehyde resin MK95, white carbon black, carbon black N774, aromatic oil and DOS), and close the top plug;
[0043] d. After another 2 minutes of internal mixing, clean the top bolt, sweep the top bolt and the small materials around it into the internal mixer, and then close the top bolt; after the total internal mixing time reaches 8 minutes and 30 seconds, stop the internal mixing, open the internal mixing chamber for glue discharge (note: the glue discharge temperature must be higher than 90°C and not higher than 110°C. The entire internal mixing process is 8 minutes and 30 seconds. If the glue discharge temperature is too high, the mixed rubber will stick to the internal mixing chamber and cannot be taken out of the internal mixer, affecting the subsequent open mixing process) to obtain the mixed rubber;
[0044] e. First clean the mill with car wash glue, then wipe the two rollers of the mill with a paper towel dipped in alcohol;
[0045] f. Then set the mill roll temperature to 30 ° C, adjust the roll gap to 1 mm, and set the roll speed to 17 rpm / min;
[0046] g. Start the open mill and put the mixed rubber after internal mixing between the two rollers so that the rubber material wraps around the rollers on the open mill and the rubber accumulation needs to be generated between the two rollers;
[0047] h. Add small materials (ETU-80, TMTD-80, zinc oxide, RA-65) evenly in an "S" shape. After adding the small materials, add the small materials left under the roller into the rubber compound;
[0048] i. Use a rubber cutting knife to cut the rubber on the left and right 3 / 4 for 3 times each to make the filler pre-dispersed evenly, remove the rubber and stop the mixing mill;
[0049] j. Adjust the roller distance of the mixing mill to 0.5mm, put the rubber on, start the mixing mill, and make 5 passes in the form of rolling and triangle packing;
[0050] k. Finally, adjust the roll distance of the mixing mill to 1.5mm to exhaust the lower sheet (remember the calendering direction) to obtain the secondary mixed rubber;
[0051] l. First adjust the roller distance of the mixing mill to 3mm, set the initial temperature to 60℃, start the mixing mill to heat the above-mentioned rubber mix again;
[0052] m. Place the mixed rubber on an open mill for calendering (calendering parameters: 4-roll calender, low roller speed 5-10m / min, calendering temperature cannot exceed 60 degrees Celsius, ensure that the rubber spline can be smoothly peeled off from the calendering roller after opening, and the thickness of the rubber is 0.9mm-1mm), so that the mixed rubber can be completely wrapped on one side of the roller, take a piece of calendered rubber from the roller, measure the thickness of the rubber with a vernier caliper, and check whether the thickness of the rubber meets the requirements (the thickness of the rubber is 0.9mm-1mm), and adjust the roller distance of the open mill in time to finally obtain the chloroprene rubber adhesive;
[0053] n. Tighten and straighten two rolls of fabric (high temperature resistant and will not shrink at 160°C) respectively, and bond the two fabrics and the chloroprene rubber adhesive together through a calendering roller. It is necessary to ensure that the chloroprene rubber adhesive can be evenly bonded between the two fabrics, so that the surface of the semi-finished product is flat without protrusions or depressions;
[0054] o. Finally, the semi-finished product is vulcanized by the vulcanization process (rubber vulcanization can easily flatten the fabric pattern, and the vulcanization process can retain the original pattern and texture of the fabric, so that the ceiling can be customized according to customer needs without being limited by process drawbacks.) to obtain the finished product. Specific parameters: temperature 110, pressure 0.2MPa, speed 10m / min.
[0055] The specific formula and dosage of the above process are shown in Table 2
[0056]
[0057] Table 2
[0058] In the above process, the following points should also be noted:
[0059] 1. During the bonding process of the two fabrics and the neoprene adhesive, the roller speed is slow, the cloth must have tension, and the calender cannot have a roller speed ratio. The temperature of the calender roller cannot be high, otherwise the mixed rubber will not be well bonded from the calender roller to the adhesive fabric.
[0060] 2. A lot of viscosity-enhancing components are added to the formula, such as phenol-formaldehyde resin MK95, white carbon black, and RA-65. This allows for good adhesion under low pressure without destroying the original pattern of the fiber. This is an inter-formaldehyde white viscosity-enhancing system.
[0061] 3. Adding tackifying resin will cause the roller to stick, which is not conducive to processing. However, LANXESS B210 has good processing performance and can be easily removed from the open mill or internal mixer even with the addition of tackifying resin.
[0062] 4. Filling ratio refers to the ratio of the total volume of these formula materials to the volume of the internal mixer.
[0063] 5. If compression vulcanization is used, although the bonding is very good, there is no pattern. If the drum sulfur is used, the pattern will not be destroyed, but the bonding strength is difficult to ensure. Therefore, on the basis of the drum sulfur process, the formula of the present invention is used, so the drum sulfur pressure is small, the bonding strength is high, and the pattern is intact and undamaged (the bonding strength is greater than 60, and the pattern on the fiber is not destroyed after calendering, and the pattern is complete);
[0064] The performance indicators and test results of the sandwich structure composite material obtained by the above formula and process are as follows Table 3:
[0065]
[0066]
[0067]
[0068] Table 3
[0069] Compared with other ceiling fabrics, the sandwich structure composite material of the present invention has obvious advantages in breaking strength, tearing strength, peeling strength, waterproofness and stain resistance, as shown in Table 4 below:
[0070]
[0071] Table 4
[0072] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
Claims
1. A sandwich structure composite material, characterized in that: include: The first fabric layer, the chloroprene rubber adhesive layer and the second fabric layer, the first fabric layer is made of polyester filament woven fabric, the second fabric layer is made of short fiber woven fabric, and the material formula of the chloroprene rubber adhesive layer is: 。 2. A method for preparing the sandwich structure composite material according to claim 1, characterized in that: The method comprises the following steps: (1) cleaning an internal mixer, setting the temperature and speed of the internal mixer, opening the top plug of the internal mixer, adding raw rubber for a first internal mixing, then adding filler, closing the top plug for a second internal mixing, and draining the rubber to obtain a mixed rubber, wherein the raw rubber is LANXESS B210, and the filler is protective wax Antilux111, magnesium oxide, stearic acid, antioxidant OCTAM, phenol-formaldehyde resin MK95, white carbon black, carbon black N774, aromatic oil and DOS; (2) cleaning the open mill, setting the roller temperature and roller speed of the two rollers of the open mill, and adjusting the roller distance of the two rollers for the first time, starting the open mill, placing the rubber mix between the two rollers, so that the rubber mix is rolled on the open mill and a rubber accumulation is generated between the two rollers, adding small materials evenly in an "S" shape, tapping the rubber mix with a rubber tapping knife to pre-disperse the small materials evenly, removing the rubber mix, pausing the open mill, adjusting the roller distance of the two rollers of the open mill for the second time, placing the rubber mix, starting the open mill, and thinning to obtain a secondary rubber mix, wherein the small materials are ETU-80, TMTD-80, zinc oxide and RA-65; (3) adjusting the roller distance of the two rollers of the open mill for the third time, setting the initial temperature, starting the open mill, re-heating the secondary rubber mix, placing the secondary rubber mix on the open mill for calendering so that the secondary rubber mix can be completely wrapped around one roller, taking a piece of the calendered secondary rubber mix from the roller as a rubber compound, and measuring the thickness of the rubber compound with a vernier caliper to obtain a chloroprene rubber adhesive; (4) The first fabric and the second fabric are stretched and straightened respectively, and the first fabric, the second fabric and the chloroprene rubber adhesive are bonded together by a calendering roller to obtain a semi-finished product; (5) The semi-finished product is vulcanized by a sulphur drum process to obtain a finished product.
3. The method for preparing a sandwich structure composite material according to claim 2, wherein: In step (1), the temperature of the internal mixer is 60° C. and the rotation speed is 60 rpm / min.
4. The method for preparing a sandwich structure composite material according to claim 2, wherein: In step (1), the filling ratio of the rubber mix in the internal mixer is 0.
69.
5. The method for preparing a sandwich structure composite material according to claim 2, wherein: In step (1), the time of the first mixing is 3 minutes, the total time of the two mixings is 8 minutes and 30 seconds, and the temperature of the debinding is greater than 90°C and less than 110°C.
6. The method for preparing a sandwich structure composite material according to claim 2, wherein: In step (2), the roller temperature of the two rollers of the open mill is 30°C, the roller speed is 17 rpm / min, the first adjustment of the roller spacing of the two rollers is 1 mm; the second adjustment of the roller spacing of the two rollers of the open mill is 0.5 mm; the tapping is specifically: tapping the rubber at 3 / 4 on the left and right sides of the mixed rubber 3 times each; the thinning is specifically: thinning 5 times in the form of rolling and triangle packing.
7. The method for preparing a sandwich structure composite material according to claim 2, wherein: In step (3), the roller spacing between the two rollers of the mixing mill is adjusted to 3 mm for the third time, and the initial temperature is 60°C.
8. The method for preparing a sandwich structure composite material according to claim 2, wherein: In step (3), the specific process parameters of the calendering are: using a 4-roll calender, a low roller speed of 5-10 m / min, a calendering temperature less than 60° C., and the thickness of the rubber material is 0.9 mm-1 mm.
9. The method for preparing a sandwich structure composite material according to claim 2, wherein: In step (5), the specific parameters of the sulfur blowing process are: temperature 110° C., pressure 0.2 MPa, and speed 10 m / min.