A kind of sheet sodium ion battery negative electrode material and preparation method thereof
The preparation of the sheet Ni/MnCO3 negative electrode material by spinel-type NiMnO3 solves the problem of poor volume expansion and cycle stability in sodium ion batteries, achieves higher specific surface area and cycle stability, and improves the electrochemistry of sodium ion batteries performance.
Patent Information
- Application Number
- CN202211515218.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-11-30
AI Technical Summary
The existing sodium ion battery negative electrode materials are prone to volume expansion during the process of sodium ions embedded and disengagement, resulting in damage to the electrode structure, poor circulation stability, and low specific capacity, which affects battery performance.
The Ni/MnCO3 negative electrode material with a sheet structure is prepared by low-temperature pre-firing and heating reaction. It uses CO2 in the air to form a sheet assembly to reduce the stress concentration caused by sodium ions embedded and detachment. Improve the adsorption capacity of electrolyte.
This method significantly alleviates the problem of volume expansion, improves the structural stability of the material and sodium ion transmission efficiency, significantly improves the circulation and rate performance of sodium ion batteries, and extends the service life of the battery.
Smart Images

Figure CN116102088B_ABST
Abstract
Description
Technical Field
[0001] The present invention mainly relates to the technical field of sodium ion batteries, and in particular to a sheet sodium ion battery negative electrode material and a preparation method thereof. Background Art
[0002] The progress of science and technology has further expanded people's demand for electricity, such as electric vehicles, 3C products, and home appliances, which has put tremendous pressure on electricity production. At present, domestic electricity production still mainly relies on fossil energy such as coal, oil, and natural gas, but these energy sources are not only non-renewable, but also cause great damage to the ecological environment due to excessive use. It is imperative to develop and apply new energy such as wind energy, solar energy, and tidal energy on a large scale, and use new technologies to convert new energy into "electricity" that people can use.
[0003] At present, the most widely used energy storage system should be the electrochemical energy storage system because of its low cost, high safety and convenience. The limited lithium resources and their uneven distribution have restricted the development of lithium batteries. The continuous expansion of the energy storage market capacity has exacerbated the high cost of lithium batteries, further hindering the commercialization process. Sodium resources are not only abundant in global reserves, evenly distributed, and have lower mining costs, but also the energy storage principle and production process of sodium ion batteries mediated by sodium ions are highly similar to lithium batteries. They have unique advantages in low temperature performance, fast charging and discharging, and environmental adaptability. Therefore, sodium ion batteries are considered to have the potential to become a new type of energy storage system that has the potential to be industrialized and commercialized in the future, and become a supplement or substitute for lithium batteries.
[0004] Chinese patent CN 113675398 A discloses the use of two-step hydrothermal reaction to prepare NiMnO3 / MnCo2S4 composite negative electrode material, introducing isophthalic acid to obtain NiMnO3 with high specific surface area and high porosity; then compounding it with nano-scale MnCo2S4 to ensure its high dispersion. However, when used as a lithium battery negative electrode, this material exhibits defects such as low specific capacity and unstable cycle.
[0005] Patent CN103337604 A discloses hollow spherical NiMn2O4 lithium-ion battery negative electrode material and preparation method. Based on the "Kirkendall effect", it can be directly obtained by a high-temperature solid-phase reaction method. The material is a hollow sphere with a particle size of about 1-3um. The porous spherical shell is conducive to the penetration of the electrolyte and shortens the diffusion path of lithium ions. As a negative electrode material for lithium-ion batteries, it has excellent electrochemical cycle stability and rate performance. However, when used as a lithium battery negative electrode, this material can only circulate for 248 weeks at a small current, and exhibits a low specific capacity and stability as well as poor rate performance.
[0006] As the hub of sodium-ion batteries, negative electrode materials are responsible for the storage and release of sodium ions, which directly affects the performance of the battery. Negative electrode materials for sodium-ion batteries mainly include carbon materials, alloys, and metal compounds. Among them, conversion-type metallizations and materials have been widely studied because of their easy preparation, high theoretical specific capacity, and safety. However, their application in sodium-ion batteries also shows some problems: 1. The continuous insertion and extraction of large-radius sodium ions can easily lead to large volume expansion, causing damage to the electrode structure and showing poor cycle stability; 2. Some compounds show low specific capacity, etc. Therefore, the preparation of new electrode materials with special structures and shapes is effective in maintaining the stability of the material and electrode structure, improving the battery energy density, and extending the service life. Summary of the invention
[0007] The purpose of the present invention is to provide a sheet sodium ion battery negative electrode material and a preparation method thereof, so as to solve the technical problem in the prior art that the continuous deintercalation of large-radius sodium ions easily leads to large volume expansion, causes electrode structure damage, and exhibits poor cycle stability.
[0008] The present invention discloses a method for preparing a sheet-type sodium ion battery negative electrode material, comprising the following steps: S1. preparing spinel-type NiMnO3;
[0009] S2. Pre-sintering spinel-type NiMnO3 at low temperature and then heating it to react to obtain Ni / MnCO3.
[0010] Furthermore, the spinel-type NiMnO3 preparation strategy is a solvent thermal pathway.
[0011] Furthermore, when the spinel type NiMnO3 is prepared, the Ni source is one or more of nickel acetate, nickel chloride, nickel nitrate, nickel sulfate or nickel acetylacetonate.
[0012] Furthermore, when the spinel type NiMnO3 is prepared, the Mn source is one or more of manganese acetate, manganese chloride, manganese nitrate, manganese sulfate or manganese acetylacetonate.
[0013] Furthermore, the material ratio between the Ni source and the Mn source during the preparation of the spinel type NiMnO3 is 1:1.
[0014] Furthermore, the spinel-type NiMnO3 is prepared, and the active agent of the solution used is cyclohexamethylenetetramethylenetetramethylene.
[0015] Furthermore, the spinel-type NiMnO3 is prepared using a solvent selected from the group consisting of methanol, ethanol, benzyl alcohol, ethylene glycol, polyethylene glycol, and triethylene glycol.
[0016] Furthermore, the spinel type NiMnO3 is prepared at a reaction temperature of 100-300 degrees.
[0017] Furthermore, the spinel type NiMnO3 is prepared with a reaction time of 10-48h.
[0018] Furthermore, the pre-sintering temperature of the spinel type NiMnO3 is 100-500 degrees.
[0019] Furthermore, the pre-sintering time of the spinel type NiMnO3 is 0-5h.
[0020] Furthermore, the pre-sintering heating rate of the spinel-type NiMnO3 is 5 degrees per minute.
[0021] Furthermore, the temperature of the heating reaction of the spinel type NiMnO3 is 200-500 degrees.
[0022] Furthermore, the heating reaction time of the spinel type NiMnO3 is 1-5h.
[0023] Furthermore, the heating temperature of the spinel type NiMnO3 is 200-500 degrees.
[0024] The second purpose of the present invention is to protect a sheet-like sodium ion battery negative electrode material prepared using the above method.
[0025] A sheet-like sodium ion battery negative electrode material has a sheet-like Ni / MnCO3 structure.
[0026] The third purpose of the present invention is to protect an assembled button battery, which is a button battery assembled using the material obtained by the above preparation method or the above material.
[0027] Furthermore, in the battery, Ni / MnCO3:conductive carbon black:CMC (sodium carboxymethyl cellulose):SBR (styrene-butadiene rubber)=7:2:0.5:0.5.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1. The preparation method of the negative electrode material of the sodium ion battery of the present invention uses spinel NiMnO3 as a precursor, sintering in air to absorb CO2 in the air, and deriving the sheet-assembled negative electrode material Ni / MnCO3, the morphology structure of which can greatly alleviate the volume expansion caused by the stress concentration caused by the insertion and removal of sodium ions, and maintain the stability of the material structure;
[0030] 2. The large specific surface area of the negative electrode material of the sodium ion battery can also improve the material's adsorption capacity for the electrolyte and enhance the sodium ion transmission efficiency; the interaction between Ni / Mn metal ions can also promote the sodium ion battery to exhibit excellent cycle and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is the XRD pattern of the precursor;
[0032] Figure 2 is the FESEM image of the precursor;
[0033] Figure 3 is the XRD pattern of the target product Ni / MnCO3;
[0034] Figure 4 and Figure 5 This is the XPS graph of the target product Ni / MnCO3;
[0035] Figure 6 and Figure 7 is the FESEM image of the target product Ni / MnCO3;
[0036] Figure 8 , 9 , 10 and 11 are EDS images of the target product Ni / MnCO3;
[0037] Fig.12 It is the Capacity-Voltage diagram of the target product Ni / MnCO3;
[0038] Fig.13 It is the CYCLE diagram of the target product Ni / MnCO3;
[0039] Fig.14 It is the RATE diagram of the target product Ni / MnCO3. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.
[0041] Example 1
[0042] A method for preparing a negative electrode material for a lamellar sodium ion battery specifically comprises the following steps: firstly, dissolving 1mmol of nickel acetate, 1mmol of manganese acetate and 5mmol of cyclohexamethylenetetramethylene in 10ml of deionized water and 25ml of triethylene glycol, stirring for 30 minutes, adding the materials into a reactor after they are fully dissolved, performing hydrothermal reaction at 180 degrees for 24 hours, and then filtering and centrifuging with deionized water and anhydrous alcohol to obtain a slightly yellow solid powder.
[0043] like Figure 1 As shown, the XRD pattern of the precursor matches well with the standard card PDF#75-2089, proving that NiMnO3 was successfully prepared. Figure 2 The field emission pattern of the precursor NiMnO3 at a small magnification is shown, showing a spherical structure formed by self-assembly of the sheets.
[0044] The above powder was placed in a muffle furnace, heated to 200 degrees, and kept warm for 2 hours to obtain the target product.
[0045] Figure 3 This is the XRD test diagram of the current product. The results show that the target substance is a mixture of Ni / MnCO3 (PDF#10-0272) and MnCO3 (PDF#07-0268). The crystal diffraction peak matches the standard card perfectly, and there is no characteristic peak of impurities, which proves the high purity of the material.
[0046] In order to further explore the valence state of the substance, we conducted elemental valence analysis of Ni and Mn. Figure 4 and Figure 5 XPS data of Mn and Ni are shown. Figure 4 The test results show that 652.77eV corresponds to Mn 2P 1 / 2; 640.78eV corresponds to Mn2P 3 / 2, and the difference between the two peaks is 11.99eV; Figure 5 The test results show that 855.27eV corresponds to Ni 2P 3 / 2; 873.22eV corresponds to Ni 2P 1 / 2, and the difference between the two peaks is 17.95eV.
[0047] The morphology and structure of the target product were then further tested. Figure 6 and Figure 7 This shows that after the product is heated in a muffle furnace and reacts with carbon dioxide in the air, its morphology does not change and it still maintains a spherical structure assembled from sheets. Figure 8 , 9 , 10, and 11 respectively show the total distribution of the target product constituent elements, the distribution of Ni, Mn, and O, proving that each contained element is distributed inside and on the surface of the material, which is beneficial to the reaction of the material during continuous charging and discharging.
[0048] The target substance obtained above, conductive carbon black and binder were weighed in a ratio of 7:2:0.5:0.5, 200 mg were added to agate and ground for 10 minutes at room temperature. After that, secondary water was added and grinding continued for at least 20 minutes to form a negative electrode slurry. The negative electrode slurry was coated on the aluminum plate by a four-sided scraper.
[0049] On the foil, the coating thickness is 75um and the electrode mass is approximately 1.5mg.
[0050] Place the current collector coated with the material in a 120-degree vacuum drying oven and dry for 12 hours.
[0051] Next, in a glove box under an argon atmosphere, using a sodium sheet as a counter electrode and a reference electrode, the positive electrode shell, the negative electrode shell, the glass fiber separator, the sodium sheet, and the electrolyte were assembled together into a CR2032 button battery. The electrolyte was a diethylene glycol dimethyl ether solvent in which 1 M NaPF6 was dissolved.
[0052] The assembled sodium ion battery was subjected to constant current charge and discharge test in the blue electric test system. -1 , 0.2Ag -1 , 0.5Ag -1 , 1.0Ag -1 , 2.0Ag -1 , 5.0Ag -1 The rate performance and cycle performance were tested in the voltage range of 0.01-3.0V.
[0053] Fig.12 The button cell assembled from the electrode prepared with the target product as the active material has a high conductivity at 0.1Ag. -1 The cycle diagram of the first cycle of the battery measured below,
[0054] Fig.13 The battery showed a 2.0Ag -1 The long cycle data graph was measured at a current density of 1.5 %. The results showed that after 700 cycles, it can still show nearly 330 mAh g -1 The capacity is high and the cycle stability is good. The Coulomb efficiency curve also shows that the ratio of discharge capacity to charge capacity is close to 100%, and the capacity retention rate is very high.
[0055] Fig.14 The rate performance of the battery was measured at different current densities. -1 At current densities of 1.3, 1.7, 2.1, 3.3, 4.5, 5.9, 6.3, 7.9, 8.8, and 9.5 mAh g, respectively. -1 When the current density returns to the initial current density of 0.1A -1When the battery is charged, not only does the battery capacity not decay, but even shows a higher specific capacity. This is mainly due to the gradual activation of the material, more active sites and better structural stability.
[0056] Comparative Example 1
[0057] As a comparative example of the present invention, the implementation method is the same as that of Example 1, except that nickel acetate is replaced by nickel chloride, and manganese acetate is replaced by manganese chloride, and other conditions are the same.
[0058] Implementation results: Since the anions in nickel chloride and manganese chloride are strongly acidic anions, they cannot be decomposed by heat during the reaction, and the reaction system does not contain an oxygen source, so it cannot be obtained.
[0059] Comparative Example 2
[0060] As a comparative example of the present invention, the implementation method is the same as that of Example 1, except that nickel acetate is replaced by nickel acetylacetonate, and manganese acetate is replaced by manganese acetylacetonate, and other conditions are the same.
[0061] Implementation results: The same precursor was obtained, and the same target product was obtained after post-treatment reaction.
[0062] Electrochemical performance test: at 0.1Ag -1 At the current density, the specific capacity is stable at 470mAhg -1 The specific capacity is about 5.0Ag -1 At the current density, the specific capacity is stable at 320mAhg -1 At the same time, at 2.0Ag -1 After 500 cycles of charge and discharge at the same current density, the specific capacity remains at 300 mAh g -1 about.
[0063] Comparative Example 3
[0064] As a comparison of the present invention, its implementation method is the same as Example 1, and the only change is that the raw material addition ratio of the nickel source and the manganese source is replaced with 1:1.5, and other conditions are the same.
[0065] Implementation results: Because the ratio of the elements is no longer maintained at 1:1, the manganese content is higher, and thus a mixture of NiMn2O4 and NiMnO3 is generated during the reaction.
[0066] Comparative Example 4
[0067] As a comparative example of the present invention, the implementation method is the same as that of Example 1, with the only change being that the temperature of NiMnO3 during heating reaction in the muffle furnace is changed to 500 degrees, the insulation time is increased to 5 hours, and the other conditions remain unchanged.
[0068] Implementation results: As the temperature increases, the reaction time is longer, so the Ni / MnCO3 generated by the reaction at a lower temperature is thermally decomposed to obtain nickel oxide and manganese oxide.
[0069] The above are the implementation methods listed in this embodiment, but this embodiment is not limited to the above optional implementation methods. Those skilled in the art can arbitrarily combine the above methods to obtain other various implementation methods. Anyone can derive other various forms of implementation methods under the inspiration of this embodiment. The above specific implementation methods should not be understood as limiting the scope of protection of this embodiment. The scope of protection of this embodiment shall be based on the definition in the claims, and the description can be used to interpret the claims.
Claims
1. A method for preparing a sheet sodium ion battery negative electrode material, characterized in that: The following steps are included: S1. Preparation of spinel type NiMnO3; S2. Pre-sintering the spinel type NiMnO3 at low temperature and then heating the reaction to obtain Ni / MnCO3; The spinel type NiMnO3 preparation strategy is a solvothermal route; When the spinel type NiMnO3 is prepared, the Ni source is one or more of nickel acetate, nickel chloride, nickel nitrate, nickel sulfate or nickel acetylacetonate; When the spinel type NiMnO3 is prepared, the Mn source is one or more of manganese acetate, manganese chloride, manganese nitrate, manganese sulfate or manganese acetylacetonate; The spinel type NiMnO3 is prepared with a material ratio of 1:1 between the Ni source and the Mn source; The temperature of the heating reaction of the spinel type NiMnO3 is 200-500 degrees.
2. A sheet-like sodium ion battery negative electrode material, characterized in that: The negative electrode material is prepared using the method for preparing a sheet-like sodium ion battery negative electrode material as described in claim 1.
3. An assembled button battery, characterized in that: The negative electrode material is assembled using the sheet-like sodium ion battery negative electrode material prepared by the preparation method described in claim 1 or the sheet-like sodium ion battery negative electrode material described in claim 2.
Citation Information
Patent Citations
Hollow spherical NiMn2O4 lithium ion battery cathode material and preparation method thereof
CN103337604A
Lithium ion battery negative electrode material and preparation method thereof
CN113675398A
NiMnO3 porous nanosphere material, and preparation method and applications thereof
CN109179519A
A NiMnO3 electrode material with high specific surface area, preparation method and application thereof
CN109273274A
Sodium ion battery negative electrode material as well as preparation method and application thereof
CN112607792A